Photothermal characterization device and method for curing viscosity of solid rocket nozzle adhesive based on broadband dual laser excitation

Through wide-band dual laser excitation technology, the photothermal signal of solid engine nozzle adhesive is measured, and the response model is established, which solves the problem that the curing time cannot be quantitatively evaluated in the existing technology, and realizes the degree of curing of solid engine nozzle adhesive. Accurate quantitative evaluation.

CN117030775BActive Publication Date: 2024-11-15HARBIN INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310829599.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-07
Publication Date
2024-11-15
Estimated Expiration
2043-07-07

AI Technical Summary

Technical Problem

The prior art cannot effectively and quantitatively determine the curing time of solid engine nozzle adhesive, and lacks quantitative indicators, resulting in the inability to accurately evaluate the curing degree during the bonding process.

Method used

The adhesive is measured through computer-controlled high-power and low-power semiconductor lasers, HCT thermal detectors and other components such as computer-controlled components. The photothermal signal is established, and the response model of dual laser excitation-induced thermal radiation signal is achieved to achieve quantitative evaluation of the degree of curing.

Benefits of technology

It can effectively identify the optimal curing time of solid engine nozzle adhesive. The adhesive thickness covers 20μm~200μm. The characteristic phase difference between the optimal cured and uncured adhesive is greater than 30 degrees, and the inverse of thermal conductivity and thermal diffusion coefficient The performance accuracy is better than 10-4W/m℃ and 10-3m2/s, providing quantitative evaluation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117030775B_ABST
    Figure CN117030775B_ABST
Patent Text Reader

Abstract

A solid engine nozzle adhesive curing viscosity photothermal characterization device based on broadband dual laser excitation and a characterization method thereof. A computer (1) is sequentially connected to a first function generator (4) and a high-power semiconductor laser power supply (6), the high-power semiconductor laser power supply (6) is respectively connected to a high-power semiconductor laser (9) and a TEC refrigerator power supply (11), a TEC semiconductor refrigerator (10) is arranged on the TEC refrigerator power supply (11), the high-power semiconductor laser (9) is sequentially connected to a first collimator (20), a first engineering diffuser (21) and a second polarizer (22); the computer (1) is also connected to a phase-locked detection amplifier (39), the phase-locked detection amplifier (39) is sequentially connected to a preamplifier (15), an HCT thermal detector (17), a first polarizer (18) and a bandpass filter (19). The present invention solves the problem that the curing time of the solid engine nozzle adhesive cannot be quantified during practical application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of photothermal science, detection and signal processing technology, and specifically relates to a photothermal characterization device for solid engine nozzle adhesive curing viscosity based on broadband dual laser excitation and a characterization method thereof. Background Art

[0002] Solid engine nozzle bonding includes the bonding of resin-based carbon fiber composite material lining and metal shell. The bonding effect is mainly determined by the surface state of the adherend, the performance of the adhesive and the characteristics of the interface layer. Since epoxy resin is active on many materials, the curing reaction is a nucleophilic addition reaction. It does not require high pressure during curing, and the bonding molding process is simple. The formula selection based on this is also relatively easy. According to the curing temperature used, the corresponding curing agent is selected, while taking into account the applicable period and the performance of the adhesive after curing. In the actual application process, the E-51 epoxy resin and 2-ethyl-4-methylimidazole formula system adhesive is a medium-temperature curing epoxy resin structural adhesive. After long-term use of batch production models, it has been shown that it can meet the bonding between the metal shell and the fiberglass lining of the long tail nozzle of the tactical missile solid rocket engine. The adhesive performance indicators, molding process, quality stability, reliability, etc. fully meet the product use requirements. Based on the apparent kinetic equation, the complete curing time of the E-51 epoxy resin and 2-ethyl-4-methylimidazole formula system adhesive at a specified temperature can be roughly calculated. Setting the ambient temperature to 80°C, the full curing time is 4.44 hours. Taking into account the effects of heat conduction and radiation between the material and the environment, the full curing time is generally 6 to 8 hours at 80°C. In order to ensure effective bonding between the solid engine composite material lining and the metal shell, it is generally necessary to bond at a certain time before the material is fully cured, and there is currently no empirical or theoretical formula for calculation reference at this time. After sufficient investigation, the current production workshop still mainly relies on the actual engineering experience of the bonding workers to determine this time, and uses fingers to touch the adhesive during the curing process. When the adhesive shows a "wire drawing without adhesion" effect, it is the optimal bonding time.

[0003] In the prior art, a terahertz time-domain spectrometer is used to collect the terahertz time-domain signal of the organic adhesive bonding sample after the room temperature curing time T1 time, and obtain a terahertz data set. The variance value and the flight time of each point in the variance imaging diagram and the flight time imaging diagram are mathematically statistically analyzed to form a bar graph; the bar graph is fitted with a Gaussian curve, and the characteristic value μ of the Gaussian curve after fitting is statistically analyzed; the above steps are repeated until the characteristic value of the Gaussian curve after room temperature curing is completed; the characteristic values ​​of the Gaussian curve of the organic adhesive bonding sample at room temperature curing in each period are statistically analyzed to obtain a curve graph. The invention uses terahertz time-domain spectroscopy to obtain characteristic changes in the curing process, which can evaluate the curing of the adhesive to a certain extent, but lacks quantitative indicators and therefore cannot be quantitatively determined. Another prior art does not mention a method for detecting or quantifying the degree of curing. The prior art also discloses that magnesium-aluminum alloy is used as the bonded material, and a nonlinear ultrasonic test system is used to excite and receive longitudinal ultrasonic signals, and the received ultrasonic signals are Fourier transformed to obtain the fundamental frequency amplitude and the frequency harmonic amplitude of the ultrasonic signal passing through the bonding structure, and the corresponding nonlinear coefficient is obtained, and finally the relationship between the nonlinear coefficient and the curing time of the adhesive is established. In this paper, the curing degree of the material is evaluated using a custom nonlinear coefficient, and the result is not interpretable. At the same time, this method is a contact measurement and is not suitable for scenes requiring non-contact detection. When the prior art takes 6061 aluminum alloy / modified acrylic adhesive / 6061 aluminum alloy bonding specimens as the research object, the colinear shear wave and longitudinal wave mixing detection technology are used to experimentally study the change of the resonance wave amplitude with the curing time of the bonding interface. The results show that there is an intrinsic relationship between the resonance wave amplitude and the number of randomly distributed cracks in the bonding layer and the curing time of the bonding specimen. However, this method is still a real-time monitoring method, and lacks an effective quantitative indicator for measuring the curing degree of the material. Summary of the invention

[0004] The present invention provides a solid engine nozzle adhesive curing viscosity photothermal characterization device based on broadband dual laser excitation and a characterization method thereof, so as to solve the problem that the curing time of the solid engine nozzle adhesive cannot be quantified in practical application. The detection method and system are applicable to the field of accurate quantitative evaluation of the curing viscosity and optimal curing time of the solid engine nozzle adhesive.

[0005] The present invention is achieved through the following technical solutions:

[0006] A solid engine nozzle adhesive curing viscosity photothermal characterization device based on broadband dual laser excitation, the characterization device comprises a computer 1, a first function generator 4, a high-power semiconductor laser power supply 6, a high-power semiconductor laser 9, a TEC semiconductor refrigerator 10, a TEC refrigerator power supply 11, a first mounting support 13, a large off-axis parabolic mirror 14, a preamplifier 15, an HCT thermal detector 17, a first polarizer 18, a bandpass filter 19, a first collimator 20, a first engineering diffuser 21, a second polarizer 22, a second collimator 23, a second engineering diffuser 24, a third polarizer 25, a focusing plate 26, a small off-axis parabolic mirror 27, a to-be-tested object 28, a constant temperature box 29, a two-dimensional micro-displacement mobile stage 30, a second mounting support 32, a two-axis driver 33, a low-power semiconductor laser 35, a second function generator 37, a phase-locked detection amplifier 39, and a drive control line 41;

[0007] The computer 1 is connected to a first function generator 4 and a high-power semiconductor laser power supply 6 in sequence, the high-power semiconductor laser power supply 6 is connected to a high-power semiconductor laser 9 and a TEC refrigerator power supply 11 respectively, a TEC semiconductor refrigerator 10 is arranged on the TEC refrigerator power supply 11, and the high-power semiconductor laser 9 is connected to a first collimator 20, a first engineering diffuser 21 and a second polarizer 22 in sequence;

[0008] The computer 1 is also connected to a phase-locked detection amplifier 39, which is connected in sequence to a preamplifier 15, an HCT thermal detector 17, a first polarizer 18, and a band-pass filter 19; the band-pass filter 19 is used in conjunction with a large off-axis parabolic mirror 14, and the large off-axis parabolic mirror 14 is disposed on a first mounting support 13;

[0009] The phase-locked detection amplifier 39 is also connected to the second function generator 37, which is connected in sequence to the low-power semiconductor laser 35, the second collimator 23, the second engineering diffuser 24, the third polarizer 25 and the focusing plate 26, and the second engineering diffuser 24, the third polarizer 25 and the focusing plate 26 are embedded in the designated installation position of the small off-axis parabolic mirror 27, and the small off-axis parabolic mirror 27 is arranged on the second mounting support 32;

[0010] The computer 1 is also connected to a two-axis driver 33 , and the two-axis driver 33 is connected to a two-dimensional micro-displacement moving stage 30 . A constant temperature box 29 is arranged on the two-dimensional micro-displacement moving stage 30 , and a test piece 28 is placed in the constant temperature box 29 .

[0011] Further, the computer 1 is provided with two output signal terminals and one input / output signal terminal. The computer 1 is connected to the phase-locked detection amplifier 39 through the input / output signal terminal Ethernet cable 40. The computer 1 is connected to the input signal terminal of the first function generator 4 through the first output signal terminal first B-type USB data cable 3; the computer 1 is connected to the two-axis driver 33 through the second output signal terminal drive control line 41; the output signal terminal of the phase-locked detection amplifier 39 is connected to the second function generator 37 through the second BNC data cable 38; the input signal terminal of the phase-locked detection amplifier 39 is connected to the preamplifier 15 through the high-performance RF coaxial cable 2; the second function generator 37 is connected to the low-power semiconductor laser 35 through the second B-type USB data cable 36, and the laser emitted by the low-power semiconductor laser 35 is transmitted to the second collimator 23 through the second laser optical fiber 34;

[0012] The second engineering diffuser 24, the third polarizer 25 and the focusing plate 26 are embedded in the designated installation position of the small off-axis parabolic mirror 27; the test piece 28 is placed in the constant temperature box 29, and the constant temperature box 29 is placed on the two-dimensional micro-displacement moving stage 30, so as to realize the position scanning detection of the test piece 28; the small off-axis parabolic mirror 27 is installed on the second mounting support 32, and the large off-axis parabolic mirror 14 is installed on the first mounting support 13; the HCT thermal detector 17 is connected to the input signal end of the preamplifier 15 through the coaxial cable 16 to realize the amplification of the photothermal signal; the bandpass filter 19 and the first polarizer 18 are fixed in front of the HCT thermal detector 17 through threaded connection, and the bandpass The filter 19 realizes effective filtering of near-infrared excitation light; the output signal end of the first function generator 4 is connected to the high-power semiconductor laser power supply 6 through the first BNC data line 5; the high-power semiconductor laser power supply 6 is connected to the high-power semiconductor laser 9 and the TEC refrigerator power supply 11 through the semiconductor laser power supply line 7 and the TEC refrigerator power supply line 8, respectively, and the TEC semiconductor refrigerator 10 is located between the high-power semiconductor laser 9 and the TEC refrigerator power supply 11; the high-power semiconductor laser 9 transmits the laser to the first collimator 20 through the first laser optical fiber 12, and the first engineering diffuser 21 and the second polarizer 22 are respectively installed in front of the first collimator 20.

[0013] A photothermal characterization method for curing viscosity of a solid engine nozzle adhesive based on broadband dual laser excitation, the characterization method comprising the following steps:

[0014] Step 1: Identify the test piece 28 and place it in the constant temperature box 29, turn on the constant temperature box 29, and set the temperature to 80° C.

[0015] Step 2: Turn on the solid engine nozzle adhesive curing viscosity photothermal characterization device based on broadband dual laser excitation;

[0016] Step 3: Adjust the position of the two-dimensional micro-displacement moving stage 30 so that the test piece 28 is at the focal position of the small off-axis parabolic mirror 27, and adjust the first mounting support 13 so that the element detected by the HCT thermal detector 17 is at the focal position of the large off-axis parabolic mirror 14;

[0017] Step 4: The computer 1 issues a command to make the low-power semiconductor laser 35 generate a laser with a modulation frequency of 0 Hz through the phase-locked detection amplifier 39 and the second function generator 37. At this time, check whether the laser spot size is normal;

[0018] At the same time, the computer 1 issues an instruction to make the high-power semiconductor laser power supply 6 generate a laser with a modulation frequency of 0 Hz through the first function generator 4. At this time, it is checked whether the laser emitted by the first collimator 20 completely covers the test piece 28;

[0019] Step 5: Observe whether the signal obtained by the phase-locked detection amplifier 39 from the HCT heat detector 17 is within the range. If it is not within the range, the preamplifier 15 needs to be adjusted to amplify or reduce the gain;

[0020] Step 6: When the temperature of the test piece 28 reaches the set temperature, start timing, and carry out a broadband dual laser excitation adhesive curing viscosity photothermal characterization test at 0 hours 0h, wherein the modulation frequency band range of the low-power semiconductor laser 35 is set to, and the frequency of the high-power semiconductor laser power supply 6 is 0Hz, and the power is 45W;

[0021] Step 7: Then, a broadband dual laser excitation adhesive curing viscosity photothermal characterization test is performed every 1 hour, and then the worker's hand touch method is combined to determine whether it is the best bonding time, and the photothermal response characteristic data is recorded, and a total of 0-5 hours is recorded;

[0022] Step 8: After the 5-hour test data is completed, it is necessary to establish a dual laser excitation induced thermal radiation signal response model based on the characteristics of the test piece to achieve a quantitative evaluation of the curing degree;

[0023] Step 9: After the test is finished, the broadband scanning results and fitting results obtained in the test are saved, and at the same time, the computer 1 controls the high-power semiconductor laser power supply 6 and the low-power semiconductor laser 35 to make their light intensity become 0, and at the same time controls the two-axis driver 33 to make the two-dimensional micro-displacement moving stage 30 return to zero, and turns off the heating function of the constant temperature box 29;

[0024] Step 10: After the test is completed, after an interval of 5 minutes, turn off the first function generator 4, the high-power semiconductor laser power supply 6, the two-axis driver 33, the preamplifier 15, the HCT thermal detector 17, the second function generator 37, and the phase-locked detection amplifier 39 in sequence. After the constant temperature box 29 returns to room temperature, put the test piece 28 into the designated storage container.

[0025] Furthermore, the characteristic of the test piece in step eight is used to establish a dual laser excitation induced thermal radiation signal response model, specifically,

[0026]

[0027]

[0028]

[0029] Where K1 is the response gain of the HCT thermal detector, k is the thermal conductivity of the test piece, h is the convection heat transfer coefficient on the surface of the test piece, and α IR (λ) is the infrared absorption coefficient of the test piece; L1 is the thickness of the test piece; σ is the Stefan-Boltzmann constant; β is the light absorption attenuation coefficient of the test piece.

[0030] Furthermore, the relationship between the thermal radiation signal and the surface temperature signal of the test piece is as follows:

[0031]

[0032] Where K is the system proportional factor; P(λ) is the spectral response frequency band of the HCT thermal detector; ε is the emissivity of the test piece; T0 is the room temperature; λ1 and λ2 are the spectral response ranges of the HCT thermal detector respectively.

[0033] Furthermore, since the signal S(ω) is a complex quantity, the amplitude-frequency and phase-frequency dynamic responses of the photothermal radiation of the test piece under the action of the modulated laser can be directly obtained, namely:

[0034]

[0035]

[0036] Multi-parameter fitting is to find the optimal parameters so that the amplitude and phase information calculated by the mathematical model at the optimal parameters and the amplitude and phase information obtained from the experiment are brought into the objective function G to minimize G.

[0037] Furthermore, the objective function of the multi-parameter fitting is:

[0038]

[0039] Where Z1, Z2 are proportional factors; g is the coefficient to be fitted; n is the number of acquisition points; f i is the modulation frequency; Ampl T , Phase T To calculate the amplitude and phase; Ampl E , Phase E Amplitude and phase characteristic data obtained for the experiment.

[0040] The beneficial effects of the present invention are:

[0041] The present invention can effectively identify the optimal curing time of solid engine nozzle adhesives. The adhesive thickness covers 20μm to 200μm, the characteristic phase difference between the best cured and uncured adhesives is greater than 30 degrees, and the frequency of the dual laser excitation light thermal radiation response signal covers 0.01Hz to 102KHz. At the same time, the curing time of the adhesive can be quantitatively evaluated based on the thermal conductivity and thermal diffusion coefficient inversion resin. The inversion accuracy of thermal conductivity and thermal diffusion coefficient is better than 10 -4 W / m℃ and 10 -3 m 2 / s.

[0042] The present invention can also be applied to various technical fields such as the photothermal performance evaluation of polymers and the real-time monitoring and quantitative evaluation of the curing degree of aerospace adhesives.

[0043] Compared with detection methods such as ultrasound and terahertz time-domain spectroscopy, the present invention can fully utilize the advantages of non-contact photothermal radiation, tunable laser, and high heat injection efficiency. At the same time, it utilizes the advantages of dual-path detection operation in filtering high-frequency harmonic signals such as noise, and effectively extracts characteristic information including the degree of adhesive curing. It can effectively identify the optimal curing time of the solid engine nozzle adhesive, detect the adhesive thickness covering 20μm to 200μm, and the characteristic phase difference between the best cured and uncured adhesive is greater than 30 degrees. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 It is a structural schematic diagram of the present invention.

[0045] Figure 2 It is a schematic diagram of a test piece of the present invention.

[0046] Figure 3 The figures are the broadband thermal radiation response results of the solid motor nozzle adhesive samples of the present invention at different curing times, including (a) the amplitude-frequency response result and (b) the phase-frequency response result.

[0047] Figure 4 These are the characteristic results of the solid motor nozzle adhesive samples of the present invention at specific frequencies at different curing times, including (a) amplitude and (b) phase.

[0048] Figure 5 It is the fitting result of the present invention.

[0049] Figure 6 The inversion results of the thermal conductivity and thermal diffusion coefficient of the solid motor nozzle adhesive of the present invention include (a) the thermal conductivity fitting result and (b) the thermal diffusion coefficient fitting result.

[0050] 1-computer, 2-high-performance RF coaxial cable, 3-first B-type USB data cable, 4-first function generator, 5-first BNC data cable, 6-high-power semiconductor laser power supply, 7-semiconductor laser power supply line, 8-TEC refrigerator power supply line, 9-high-power semiconductor laser, 10-TEC semiconductor refrigerator, 11-TEC refrigerator power supply, 12-first laser fiber, 13-first mounting bracket, 14-large off-axis parabolic mirror, 15-preamplifier, 16-coaxial cable, 17-HCT thermal detector, 18-first polarizer, 19-bandpass filter, 20-first collimator Mirror, 21-first engineering diffuser, 22-second polarizer, 23-second collimator, 24-second engineering diffuser, 25-third polarizer, 26-focusing plate, 27-small off-axis parabolic mirror, 28-test piece, 29-constant temperature box, 30-two-dimensional micro-displacement mobile stage, 31-motion control line, 32-second mounting support, 33-two-axis driver, 34-second laser fiber, 35-low-power semiconductor laser, 36-second B-type USB data cable, 37-second function generator, 38-second BNC data cable, 39-phase-locked detection amplifier, 40-Ethernet cable, 41-drive control cable DETAILED DESCRIPTION

[0051] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0052] A solid engine nozzle adhesive curing viscosity photothermal characterization device based on broadband dual laser excitation, the characterization device comprises a computer 1, a first function generator 4, a high-power semiconductor laser power supply 6, a high-power semiconductor laser 9, a TEC semiconductor refrigerator 10, a TEC refrigerator power supply 11, a first mounting support 13, a large off-axis parabolic mirror 14, a preamplifier 15, an HCT thermal detector 17, a first polarizer 18, a bandpass filter 19, a first collimator 20, a first engineering diffuser 21, a second polarizer 22, a second collimator 23, a second engineering diffuser 24, a third polarizer 25, a focusing plate 26, a small off-axis parabolic mirror 27, a to-be-tested object 28, a constant temperature box 29, a two-dimensional micro-displacement mobile stage 30, a second mounting support 32, a two-axis driver 33, a low-power semiconductor laser 35, a second function generator 37, a phase-locked detection amplifier 39, and a drive control line 41;

[0053] The computer 1 is connected to a first function generator 4 and a high-power semiconductor laser power supply 6 in sequence, the high-power semiconductor laser power supply 6 is connected to a high-power semiconductor laser 9 and a TEC refrigerator power supply 11 respectively, a TEC semiconductor refrigerator 10 is arranged on the TEC refrigerator power supply 11, and the high-power semiconductor laser 9 is connected to a first collimator 20, a first engineering diffuser 21 and a second polarizer 22 in sequence;

[0054] The computer 1 is also connected to a phase-locked detection amplifier 39, which is connected in sequence to a preamplifier 15, an HCT thermal detector 17, a first polarizer 18, and a band-pass filter 19; the band-pass filter 19 is used in conjunction with a large off-axis parabolic mirror 14, and the large off-axis parabolic mirror 14 is disposed on a first mounting support 13;

[0055] The phase-locked detection amplifier 39 is also connected to the second function generator 37, which is connected in sequence to the low-power semiconductor laser 35, the second collimator 23, the second engineering diffuser 24, the third polarizer 25 and the focusing plate 26, and the second engineering diffuser 24, the third polarizer 25 and the focusing plate 26 are embedded in the designated installation position of the small off-axis parabolic mirror 27, and the small off-axis parabolic mirror 27 is arranged on the second mounting support 32;

[0056] The computer 1 is also connected to a two-axis driver 33 , and the two-axis driver 33 is connected to a two-dimensional micro-displacement moving stage 30 . A constant temperature box 29 is arranged on the two-dimensional micro-displacement moving stage 30 , and a test piece 28 is placed in the constant temperature box 29 .

[0057] Further, the computer 1 is provided with two output signal terminals and one input / output signal terminal. The computer 1 is connected to the phase-locked detection amplifier 39 through the input / output signal terminal Ethernet cable 40. The computer 1 is connected to the input signal terminal of the first function generator 4 through the first output signal terminal first B-type USB data cable 3; the computer 1 is connected to the two-axis driver 33 through the second output signal terminal drive control line 41; the output signal terminal of the phase-locked detection amplifier 39 is connected to the second function generator 37 through the second BNC data cable 38; the input signal terminal of the phase-locked detection amplifier 39 is connected to the preamplifier 15 through the high-performance RF coaxial cable 2; the second function generator 37 is connected to the low-power semiconductor laser 35 through the second B-type USB data cable 36, and the laser emitted by the low-power semiconductor laser 35 is transmitted to the second collimator 23 through the second laser optical fiber 34;

[0058] The second engineering diffuser 24, the third polarizer 25 and the focusing plate 26 are embedded in the designated installation position of the small off-axis parabolic mirror 27; the test piece 28 is placed in the constant temperature box 29, and the constant temperature box 29 is placed on the two-dimensional micro-displacement moving stage 30, so as to realize the position scanning detection of the test piece 28; the small off-axis parabolic mirror 27 is installed on the second mounting support 32, and the large off-axis parabolic mirror 14 is installed on the first mounting support 13; the HCT thermal detector 17 is connected to the input signal end of the preamplifier 15 through the coaxial cable 16 to realize the amplification of the photothermal signal; the bandpass filter 19 and the first polarizer 18 are fixed in front of the HCT thermal detector 17 through threaded connection, and the bandpass The filter 19 realizes effective filtering of near-infrared excitation light; the output signal end of the first function generator 4 is connected to the high-power semiconductor laser power supply 6 through the first BNC data line 5; the high-power semiconductor laser power supply 6 is connected to the high-power semiconductor laser 9 and the TEC refrigerator power supply 11 through the semiconductor laser power supply line 7 and the TEC refrigerator power supply line 8, respectively, and the TEC semiconductor refrigerator 10 is located between the high-power semiconductor laser 9 and the TEC refrigerator power supply 11; the high-power semiconductor laser 9 transmits the laser to the first collimator 20 through the first laser optical fiber 12, and the first engineering diffuser 21 and the second polarizer 22 are respectively installed in front of the first collimator 20.

[0059] according to Figure 1The solid engine nozzle adhesive curing viscosity photothermal characterization device based on broadband dual laser excitation is implemented. In this embodiment, the modulated light used in the test is a low-power semiconductor laser 35 with a wavelength of 808nm (laser power 32mW, spot diameter 600μm), and the DC light is a high-power semiconductor laser 9 with a wavelength of 808nm (laser power 45W, coverage area 100mm×100mm); HCT thermal detector 17 (detection band 2μm~12μm, detection area 100μm×100μm); the relevant detection applicable frequency band is 0.01Hz~102KHz, and the test scanning frequency range is 100Hz~100KHz. The test piece 28 is an adhesive formulated by E-51 epoxy resin and 2-ethyl-4-methylimidazole, with a thickness of 150μm.

[0060] A photothermal characterization method for curing viscosity of a solid engine nozzle adhesive based on broadband dual laser excitation, the characterization method comprising the following steps:

[0061] Step 1: Identify the test piece 28 and place it in the constant temperature box 29, turn on the constant temperature box 29, and set the temperature to 80° C.

[0062] Step 2: Turn on the solid engine nozzle adhesive curing viscosity photothermal characterization device based on broadband dual laser excitation; this process includes turning on the first function generator 4, the high-power semiconductor laser power supply 6, the preamplifier 15, the HCT thermal detector 17, the phase-locked detection amplifier 39, the second function generator 37, the two-axis driver 33 and other equipment;

[0063] Step 3: Adjust the position of the two-dimensional micro-displacement moving stage 30 so that the test piece 28 is at the focal position of the small off-axis parabolic mirror 27, and adjust the first mounting support 13 so that the element detected by the HCT thermal detector 17 is at the focal position of the large off-axis parabolic mirror 14;

[0064] Step 4: The computer 1 issues a command to make the low-power semiconductor laser 35 generate a laser with a modulation frequency of 0 Hz through the phase-locked detection amplifier 39 and the second function generator 37. At this time, check whether the laser spot size is normal;

[0065] At the same time, the computer 1 issues an instruction to make the high-power semiconductor laser power supply 6 generate a laser with a modulation frequency of 0 Hz through the first function generator 4. At this time, it is checked whether the laser emitted by the first collimator 20 completely covers the test piece 28;

[0066] Step 5: Observe whether the signal obtained by the phase-locked detection amplifier 39 from the HCT heat detector 17 is within the range. If it is not within the range, the preamplifier 15 needs to be adjusted to amplify or reduce the gain;

[0067] Step 6: When the temperature of the test piece 28 reaches the set temperature, start timing, and carry out a broadband dual laser excitation adhesive curing viscosity photothermal characterization test at 0 hours 0h, wherein the modulation frequency band range of the low-power semiconductor laser 35 is set to, and the frequency of the high-power semiconductor laser power supply 6 is 0Hz, and the power is 45W;

[0068] Step 7: Then, a broadband dual laser excitation adhesive curing viscosity photothermal characterization test is performed every 1 hour, and then the worker's hand touch method is combined to determine whether it is the best bonding time, and the photothermal response characteristic data is recorded, and a total of 0-5 hours is recorded;

[0069] Step 8: After the 5-hour test data is completed, it is necessary to establish a dual laser excitation induced thermal radiation signal response model based on the characteristics of the test piece to achieve a quantitative evaluation of the curing degree;

[0070] Step 9: After the test is finished, the broadband scanning results and fitting results obtained in the test are saved, and at the same time, the computer 1 controls the high-power semiconductor laser power supply 6 and the low-power semiconductor laser 35 to make their light intensity become 0, and at the same time controls the two-axis driver 33 to make the two-dimensional micro-displacement moving stage 30 return to zero, and turns off the heating function of the constant temperature box 29;

[0071] Step 10: After the test, after an interval of 5 minutes, turn off the first function generator, high-power semiconductor laser power supply, two-axis driver, preamplifier, HCT thermal detector, second function generator, and phase-locked detection amplifier in turn; after the constant temperature box returns to room temperature, put the test piece into the designated storage container.

[0072] Furthermore, the characteristic of the test piece in step eight is used to establish a dual laser excitation induced thermal radiation signal response model, specifically,

[0073]

[0074]

[0075]

[0076] Where K1 is the response gain of the HCT thermal detector, k is the thermal conductivity of the test piece, h is the convection heat transfer coefficient on the surface of the test piece, and α IR (λ) is the infrared absorption coefficient of the test piece; L1 is the thickness of the test piece; σ is the Stefan-Boltzmann constant; β is the light absorption attenuation coefficient of the test piece.

[0077] Furthermore, the relationship between the thermal radiation signal and the surface temperature signal of the test piece is as follows:

[0078]

[0079] Where K is the system proportional factor; P(λ) is the spectral response frequency band of the HCT thermal detector; ε is the emissivity of the test piece; T0 is the room temperature; λ1 and λ2 are the spectral response ranges of the HCT thermal detector respectively.

[0080] Furthermore, since the signal S(ω) is a complex quantity, the amplitude-frequency and phase-frequency dynamic responses of the photothermal radiation of the test piece under the action of the modulated laser can be directly obtained, namely:

[0081]

[0082]

[0083] Multi-parameter fitting is to find the optimal parameters so that the amplitude and phase information calculated by the mathematical model at the optimal parameters and the amplitude and phase information obtained from the experiment are brought into the objective function G to minimize G.

[0084] Furthermore, the objective function of the multi-parameter fitting is:

[0085]

[0086] Where Z1, Z2 are proportional factors; g is the coefficient to be fitted (including thermal conductivity and thermal diffusion coefficient); n is the number of acquisition points; f i is the modulation frequency; Ampl T , Phase T To calculate the amplitude and phase; Ampl E , Phase E The amplitude and phase characteristic data obtained from the experiment. Figure 3 The results of the broadband thermal radiation response test of solid motor nozzle adhesive samples with different curing times are given. The characteristic results of the solid motor nozzle adhesive samples with different curing times at specific frequencies are plotted. Figure 4 .Depend on Figure 4 It can be clearly seen that the optimal curing time is around 3 hours. The mathematical model is used to solve the range problem of the obtained test data. Figure 5 The results are the fitting results of the experimental values. Based on the fitting results, the specific values ​​of thermal conductivity and thermal diffusivity can be obtained (such as Figure 6 This value can be used as a standard for quantitative evaluation of curing time.

Claims

1. A solid engine nozzle adhesive curing viscosity photothermal characterization device based on broadband dual laser excitation, characterized in that: The characterization device comprises a computer (1), a first function generator (4), a high-power semiconductor laser power supply (6), a high-power semiconductor laser (9), a TEC semiconductor refrigerator (10), a TEC refrigerator power supply (11), a first mounting support (13), a large off-axis parabolic mirror (14), a preamplifier (15), an HCT thermal detector (17), a first polarizer (18), a bandpass filter (19), a first collimator (20), a first engineering diffuser (21), a second polarizer (22), a second collimator (23), a second engineering diffuser (24), a third polarizer (25), a focusing plate (26), a small off-axis parabolic mirror (27), a test piece (28), a constant temperature box (29), a two-dimensional micro-displacement moving stage (30), a second mounting support (32), a two-axis driver (33), a low-power semiconductor laser (35), a second function generator (37), and a phase-locked detection amplifier (39); The computer (1) is sequentially connected to a first function generator (4) and a high-power semiconductor laser power supply (6); the high-power semiconductor laser power supply (6) is respectively connected to a high-power semiconductor laser (9) and a TEC refrigerator power supply (11); a TEC semiconductor refrigerator (10) is arranged on the TEC refrigerator power supply (11); and the high-power semiconductor laser (9) is sequentially connected to a first collimator (20), a first engineering diffuser (21) and a second polarizer (22); The computer (1) is also connected to a phase-locked detection amplifier (39), which is sequentially connected to a preamplifier (15), an HCT thermal detector (17), a first polarizer (18) and a bandpass filter (19); the bandpass filter (19) is used in conjunction with a large off-axis parabolic mirror (14), and the large off-axis parabolic mirror (14) is arranged on a first mounting support (13); The phase-locked detection amplifier (39) is also connected to a second function generator (37), and the second function generator (37) is sequentially connected to a low-power semiconductor laser (35), a second collimator (23), a second engineering diffuser (24), a third polarizer (25) and a focusing plate (26), and the second engineering diffuser (24), the third polarizer (25) and the focusing plate (26) are embedded in a designated installation position of a small off-axis parabolic mirror (27), and the small off-axis parabolic mirror (27) is arranged on a second installation support (32); The computer (1) is also connected to a two-axis driver (33), and the two-axis driver (33) is connected to a two-dimensional micro-displacement mobile stage (30). A constant temperature box (29) is arranged on the two-dimensional micro-displacement mobile stage (30), and a test piece (28) is placed in the constant temperature box (29). The position of the two-dimensional micro-displacement mobile stage (30) is adjusted so that the test piece (28) is at the focal position of the small off-axis parabolic mirror (27).

2. According to claim 1, a solid engine nozzle adhesive curing viscosity photothermal characterization device based on broadband dual laser excitation is characterized in that: The computer (1) is provided with two output signal terminals and one input / output signal terminal. The computer (1) is connected to a phase-locked detection amplifier (39) via an Ethernet cable (40) at the input / output signal terminal. The computer (1) is connected to an input signal terminal of a first function generator (4) via a first output signal terminal first B-type USB data cable (3); the computer (1) is connected to a two-axis driver (33) via a second output signal terminal drive control cable (41); the output signal terminal of the phase-locked detection amplifier (39) is connected to a second function generator (37) via a second BNC data cable (38); the input signal terminal of the phase-locked detection amplifier (39) is connected to a preamplifier (15) via a high-performance radio frequency coaxial cable (2); the second function generator (37) is connected to a low-power semiconductor laser (35) via a second B-type USB data cable (36), and the laser light emitted by the low-power semiconductor laser (35) is transmitted to a second collimator (23) via a second laser optical fiber (34); The second engineering diffuser (24), the third polarizer (25) and the focusing plate (26) are embedded in the designated installation position of the small off-axis parabolic mirror (27); the test piece (28) is placed in a constant temperature box (29), and the constant temperature box (29) is placed on a two-dimensional micro-displacement moving stage (30) to achieve position scanning detection of the test piece (28); the small off-axis parabolic mirror (27) is installed on a second mounting support (32), and the large off-axis parabolic mirror (14) is installed on a first mounting support (13); the HCT thermal detector (17) is connected to the input signal end of the preamplifier (15) through a coaxial cable (16) to achieve amplification of the photothermal signal; the bandpass filter (19) and the first polarizer (18) are fixed in front of the HCT thermal detector (17) through a threaded connection, and the bandpass filter (19) and the first polarizer (18) are fixed in front of the HCT thermal detector (17) through a threaded connection. The filter (19) is used to effectively filter out near-infrared excitation light; the output signal end of the first function generator (4) is connected to a high-power semiconductor laser power supply (6) through a first BNC data line (5); the high-power semiconductor laser power supply (6) is connected to a high-power semiconductor laser (9) and a TEC refrigerator power supply (11) through a semiconductor laser power supply line (7) and a TEC refrigerator power supply line (8), respectively, and the TEC semiconductor refrigerator (10) is located between the high-power semiconductor laser (9) and the TEC refrigerator power supply (11); the high-power semiconductor laser (9) transmits laser light to a first collimator (20) through a first laser optical fiber (12), and a first engineering diffuser (21) and a second polarizer (22) are respectively installed in front of the first collimator (20).

3. The characterization method of the solid engine nozzle adhesive curing viscosity photothermal characterization device based on broadband dual laser excitation according to claim 1 or 2, characterized in that: The characterization method comprises the following steps, Step 1: Identify the test piece (28), place the test piece in a constant temperature box (29), turn on the constant temperature box (29), and set the temperature to 80° C.; Step 2: Turn on the solid engine nozzle adhesive curing viscosity photothermal characterization device based on broadband dual laser excitation; Step 3: adjusting the position of the two-dimensional micro-displacement moving stage (30) so that the test piece (28) is at the focal position of the small off-axis parabolic mirror (27), and adjusting the first mounting support (13) so that the element detected by the HCT thermal detector (17) is at the focal position of the large off-axis parabolic mirror (14); Step 4: The computer (1) issues a command to enable the low-power semiconductor laser (35) to generate laser light with a modulation frequency of 0 Hz through the phase-locked detection amplifier (39) and the second function generator (37). At this time, check whether the laser spot size is normal; At the same time, the computer (1) issues an instruction to make the high-power semiconductor laser power supply (6) generate laser light with a modulation frequency of 0 Hz through the first function generator (4), and at this time, checks whether the laser light emitted by the first collimator (20) completely covers the test piece (28); Step 5: Observe whether the signal obtained by the phase-locked detection amplifier (39) from the HCT heat detector (17) is within the range. If it is not within the range, the preamplifier (15) needs to be adjusted to amplify or reduce the gain; Step 6: When the temperature of the test piece (28) reaches the set temperature, start timing, and carry out a broadband dual laser excitation adhesive curing viscosity photothermal characterization test at 0h, wherein the modulation frequency band range of the low-power semiconductor laser (35) is set to, and the frequency of the high-power semiconductor laser power supply (6) is 0Hz, and the power is 45W; Step 7: Then, a broadband dual laser excitation adhesive curing viscosity photothermal characterization test is performed every 1 hour, and then the worker's hand touch method is combined to determine whether it is the best bonding time, and the photothermal response characteristic data is recorded, and a total of 0-5 hours is recorded; Step 8: After the 5-hour test data is completed, it is necessary to establish a dual laser excitation induced thermal radiation signal response model based on the characteristics of the test piece (28) to achieve a quantitative evaluation of the curing degree; Step 9: After the test is finished, the broadband scanning result and the fitting result obtained in the test are saved, and at the same time, the computer (1) controls the high-power semiconductor laser power supply (6) and the low-power semiconductor laser (35) to make their light intensity become 0, and at the same time controls the two-axis driver (33) to make the two-dimensional micro-displacement moving stage (30) return to zero, and turns off the heating function of the constant temperature box (29); Step 10: After the test is completed, after an interval of 5 minutes, the first function generator (4), the high-power semiconductor laser power supply (6), the two-axis driver (33), the preamplifier (15), the HCT thermal detector (17), the second function generator (37) and the phase-locked detection amplifier (39) are turned off in sequence; after the constant temperature box (29) returns to room temperature, the test piece (28) is placed in a designated storage container; The characteristic establishment model of the thermal radiation signal response induced by dual laser excitation in step eight of the test piece is specifically as follows: Where K1 is the response gain of the HCT thermal detector, k is the thermal conductivity of the test piece, h is the convection heat transfer coefficient on the surface of the test piece, and α IR is the infrared absorption coefficient of the test piece; L1 is the thickness of the test piece; σ is the Stefan-Boltzmann constant; β is the light absorption attenuation coefficient of the test piece.

4. According to claim 3, a method for photothermal characterization of solid engine nozzle adhesive curing viscosity based on broadband dual laser excitation, characterized in that: The relationship between the thermal radiation signal and the surface temperature signal of the test piece is as follows: Where K is the system proportional factor; P(λ) is the spectral response frequency band of the HCT thermal detector; ε is the emissivity of the test piece; T0 is the room temperature; λ1 and λ2 are the spectral response ranges of the HCT thermal detector.

5. According to claim 4, a method for photothermal characterization of solid engine nozzle adhesive curing viscosity based on broadband dual laser excitation, characterized in that: Since the signal S(ω) is a complex quantity, the amplitude-frequency and phase-frequency dynamic responses of the photothermal radiation of the test piece under the action of the modulated laser can be directly obtained, namely: Multi-parameter fitting is to find the optimal parameters so that the amplitude and phase information calculated by the mathematical model at the optimal parameters and the amplitude and phase information obtained by the experiment are brought into the objective function G to minimize G.

6. According to claim 5, a method for photothermal characterization of solid engine nozzle adhesive curing viscosity based on broadband dual laser excitation, characterized in that: The objective function of the multi-parameter fitting is: Where Z1, Z2 are proportional factors; g i is the coefficient to be fitted; n is the number of acquisition points; f i is the modulation frequency; Ampl T , Phase T To calculate the amplitude and phase; Ampl E , Phase E Amplitude and phase characteristic data obtained for the experiment.