A welding deformation control process for aluminum alloy hull
Through preheating, spray gun heating, circle welding and rolling cooling processes, deformation and weld defects caused by temperature changes in aluminum alloy welding are solved, welding stability and quality are improved, and the strength and density of welded parts are enhanced. .
Patent Information
- Application Number
- CN202310971028.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-03
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-08-03
AI Technical Summary
During the welding process of aluminum alloy, temperature changes lead to deformation of welded parts and weld defects, affecting the welding quality.
Preheating treatment, spray gun-type open flame heating, circle-type and reciprocating welding, and rolling roller cooling processes are adopted to control welding temperature and deformation, form a reinforcement layer and extrude and supplement it during the cooling process.
Effectively reduce deformation during welding, improve welding stability and quality, avoid defects in weld cooling process, and enhance the strength and density of welded parts.
Smart Images

Figure CN117047334B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aluminum alloy welding, and in particular to a welding deformation control process for an aluminum alloy hull. Background Art
[0002] Aluminum alloy is the most widely used type of nonferrous metal structural material in industry. It has been widely used in aviation, aerospace, automobile, machinery manufacturing, shipbuilding and chemical industries. With the rapid development of industrial economy, the demand for aluminum alloy welded structural parts is increasing, which makes the research on the weldability of aluminum alloy in-depth. Aluminum alloy is a material used in hull manufacturing. In the process of using aluminum alloy, it is necessary to weld aluminum alloy so as to combine aluminum alloy into the required shape.
[0003] In the general aluminum alloy welding process, the temperature of the aluminum alloy will rise rapidly during the welding process, so the aluminum alloy itself will expand, which will cause the welding position of the aluminum alloy to deform, which will affect the welding. After welding, the temperature of the aluminum alloy will drop, and the inside of the weld will shrink, causing defects in the weld and causing deformation of the weld. Therefore, a deformation control process for aluminum alloy hull welding is needed. Summary of the invention
[0004] The purpose of the present invention is to solve the above-mentioned problem and to propose an aluminum alloy hull welding deformation control process, which improves the problem that the welded parts will deform during the welding process and during the cooling process of the welded parts after welding.
[0005] A process for controlling deformation of aluminum alloy hull welding, comprising the following steps:
[0006] S1. Preheating the prefabricated aluminum alloy hull welded parts by using a spray gun type open flame heating, then using asbestos to keep them warm, and then fixing the aluminum alloy hull welded parts;
[0007] S2. Select the middle of the welding seam for welding, and then weld the two ends of the welding seam. The welding temperature at this time is 110°C. Perform jump welding from the welding points at both ends to the middle of the welding seam to form welding points. The welding gap between the welding points is 100mm-200mm. The welding temperature is 120-150°C. Welding is performed from the welding gaps on both sides to the welding gap in the middle. The welding methods used are circular welding and reciprocating welding. The welding temperature is 110°C.
[0008] S3. Place the weldment between rolling rollers, which are distributed up and down, and two groups of rolling rollers are symmetrically arranged about the weld seam. The rolling rollers gradually move from both sides to the middle, and the gap between each group of rolling rollers gradually moves to the middle.
[0009] Preferably, the method of the spray gun type open flame heating is specifically:
[0010] Preheat the welded part from 30 cm away from the welded end to the welded end, and heat both sides of the welded part simultaneously. The moving speed (V) of the spray gun is inversely proportional to the thickness (H) of the plate.
[0011] Preferably, the spray gun type open flame heating device uses CH4 as fuel.
[0012] Preferably, the reciprocating welding is specifically:
[0013] The welding gap is welded from both sides of the weld to the center of the weld, which is forward movement, and moving from the center of the weld to both ends of the weld is reverse movement. During the welding process, it moves forward 50mm, then reversely moves 40mm, then moves forward 50mm, and then moves reversely, and moves in this way alternately in forward and reverse directions.
[0014] Preferably, the circular welding is specifically:
[0015] At the beginning of welding, the welding gun and the welding point are at the same horizontal position. At this time, the welding gun draws a circle with the center point of the welding point as the center for 5 seconds at a speed of 2cm / s, and then reciprocating welding is performed.
[0016] Preferably, the speed at which the rolling rollers move toward the middle is inversely proportional to the thickness of the weldment, and the force with which the rolling rollers move toward each other is directly proportional to the thickness of the weldment.
[0017] The beneficial effects of the present invention are:
[0018] 1. During the use of the present invention, both sides of the weldment are effectively heated, thereby preheating the weldment, and the temperature of the weldment can be effectively controlled by moving the spray gun. When the temperature of the weldment rises, the weldment will stretch, thereby reducing the deformation of the weldment during the welding process and increasing the stability of the weldment during the welding process;
[0019] 2. During the welding process, firstly make a circle welding at the welding point to fix the welding point of the welded part, form a reinforcement layer at the welding point of the welded part, and then use the reciprocating welding method to weld the inside of the weld. The reciprocating welding can effectively improve the welding quality and avoid the phenomenon of inadequate welding during the welding process;
[0020] 3. After welding is completed, the welded parts will be placed on the rolling rollers for cooling. During the cooling process, the welded parts will be gradually squeezed. As the welded parts cool down, the rolling rollers will be used to squeeze other positions of the welded parts to the welding positions of the welded parts, thereby supplementing the weld seam and avoiding defects in the welding positions of the welded parts during the cooling process. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a schematic diagram of the spray gun speed and the thickness of the weldment of the present invention. DETAILED DESCRIPTION
[0022] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] The alloy hull welding deformation control process comprises the following steps:
[0024] S1. Preheating the prefabricated aluminum alloy hull welded parts by using a spray gun type open flame heating, then using asbestos to keep them warm, and then fixing the aluminum alloy hull welded parts;
[0025] In this embodiment, the method of spray gun type open flame heating is specifically:
[0026] The thickness of the aluminum alloy hull welded parts processed by this device is between 2mm and 20mm. The welded parts are preheated from 30cm away from the welding end to the welding end, and both sides of the welded parts are heated simultaneously. The moving speed (V) of the spray gun is inversely proportional to the thickness (H) of the plate.
[0027] As the thickness of the weld increases, the moving speed of the spray gun type open flame heating device also needs to be slowed down. As the thickness of the weld increases, the heating time per unit area of the weld becomes longer, so that the spray gun type open flame heating can adjust the heating time of the weld according to the thickness of the weld;
[0028] The spray gun type open flame heating device uses CH4 as fuel. The distance between the spray guns is 100mm. The power of the spray gun is 15KW. Since 1kWh (degree) = 861.25kCal (kilocalories), it means that the spray gun can provide 1500kj of heat per unit area of the welded part per second, and the heat required to increase 1KG aluminum alloy by 1℃ is 0.15KJ. The density of aluminum alloy is 2.7g / cm 3, the effective unit area heated by the spray gun is a circle with a diameter of 100mm, that is, 1000πmm 2 ;
[0029] According to the formula M=PV, it can be calculated that the mass of the aluminum alloy weldment increases by 2.7g per unit area for every 0.1mm increase in thickness of the aluminum alloy, and 0.0027KJ more heat is consumed for every 1℃ increase; the efficiency of the spray gun type open flame heating device is 20%, so the actual heat provided to the weldment by the device is 300KJ / S;
[0030] That is, the relationship between the thickness and heating time (S) of the aluminum alloy welded parts within a unit area of 0.1 mm when preheated to 100°C is:
[0031] 300*S=0.0027*100*H*10
[0032] like Figure 1 As shown, it is observed that when the plate is thin, the speed required for heating the weldment changes significantly. When the thickness of the weldment reaches 0.9mm and is heated to a fixed temperature, the welding gun moves at a speed of about 1mm / S. At this time, the device is also greatly affected by temperature. Therefore, when the thickness of the weldment is between 0.2-0.4mm, the formula used by this device is:
[0033] V=20 / 3*H+60 / 15
[0034] When the thickness of the weld is greater than 0.4MM, the welding gun uses 1mm / S to heat, so as to avoid too long welding time, which will cause more temperature loss of the weld under natural heat dissipation. Preheating the weld can effectively avoid deformation of the weld during the welding process.
[0035] S2. Select the middle of the weld for welding, and then weld the two ends of the weld. The welding temperature at this time is 110°C. Slow heating is used to heat, reduce the cooling time of the weld point, and make the weld point cool and form quickly. Then, jump welding is performed from the welds at both ends to the middle of the weld to form a weld point. The welding gap between the weld points is 100mm-200mm, and the welding temperature is 120-150°C, so that several fixed points are quickly formed between the two workpieces. The use of a higher welding temperature can significantly increase the welding speed, so that the weld point melts quickly and forms several weld points quickly. Then, welding is performed from the weld gaps on both sides to the weld gap in the middle. The welding methods used are circle welding and reciprocating welding, and the welding temperature is 110°C.
[0036] In this embodiment, reciprocating welding is specifically:
[0037] The welding gap is welded from both sides of the weld to the center of the weld, which is a forward movement, and the movement from the center of the weld to both ends of the weld is a reverse movement. During the welding process, it moves forward by 50mm, then moves reversely by 40mm, then moves forward by 50mm, and then moves reversely. In this way, the forward and reverse movements are alternately performed. Reciprocating welding is used to make the connection between the welds tighter. Reciprocating welding can avoid the phenomenon that the welding position is not welded in place. During the welding process, the forward movement interval is 50-60mm, and the reverse movement distance is 40-50mm. The operator can adjust the welding of the device according to the actual situation, so that the welding effect of the device is better. Since the device adopts both sides to the middle for welding, and the thermal insulation effect in the middle of the welded part is better, it is more conducive to avoiding the deformation of the welded part during the welding process by welding from the outer side where the heat dissipation of the welded part is faster to the inner side where the thermal insulation effect is better.
[0038] In this embodiment, the circular welding is specifically as follows:
[0039] At the beginning of welding, the welding gun and the welding point are at the same horizontal position. At this time, the welding gun draws a circle with the center point of the welding point as the center for 5 seconds at a speed of 2cm / s, and then reciprocating welding is performed. The welding point can be effectively reinforced by drawing circles, thereby forming reinforcement points equidistantly on the surface of the welded part, which can effectively increase the strength of the welded part and play a role in effectively connecting the welded part, thereby increasing the strength of the welded part and avoiding the welded part from breaking during use.
[0040] S3. Place the weldment between rolling rollers, which are distributed up and down, and two groups of rolling rollers are symmetrically arranged about the weld seam. The rolling rollers gradually move from both sides to the middle, and the gap between each group of rolling rollers gradually moves to the middle.
[0041] In this embodiment, the speed at which the rolling rollers move toward the middle is inversely proportional to the thickness of the weld, and the force of the rolling rollers moving toward each other is directly proportional to the thickness of the weld. When the welding temperature is high, the weld is placed between the rolling rollers for limiting the position, and the weld is naturally cooled. The extrusion of the weld can avoid correcting the welding position, and other positions of the weld are used to supplement the welding position. While increasing the density of the weld, it avoids the phenomenon of cold shrinkage at the welding position during the cooling process.
[0042] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A process for controlling deformation of aluminum alloy hull welding, characterized in that: The following steps are involved: S1. Preheating the prefabricated aluminum alloy hull welded parts by using a spray gun type open flame heating, then using asbestos to keep them warm, and then fixing the aluminum alloy hull welded parts; S2. Select the middle of the welding seam for welding, and then weld the two ends of the welding seam. The welding temperature at this time is 110°C. Perform jump welding from the welding points at both ends to the middle of the welding seam to form welding points. The welding gap between the welding points is 100mm-200mm. The welding temperature is 120-150°C. Welding is performed from the welding gaps on both sides to the welding gap in the middle. The welding methods used are circular welding and reciprocating welding. The welding temperature is 110°C. S3. Place the weldment between rolling rollers, which are distributed up and down, and two groups of rolling rollers are symmetrically arranged about the weld seam. The rolling rollers gradually move from both sides to the middle, and the gap between each group of rolling rollers gradually moves to the middle.
2. The aluminum alloy hull welding deformation control process according to claim 1, characterized in that: The method of the spray gun type open flame heating is specifically: Preheat the welded part from 30 cm away from the welded end to the welded end, and heat both sides of the welded part simultaneously. The moving speed (V) of the spray gun is inversely proportional to the thickness (H) of the plate.
3. The aluminum alloy hull welding deformation control process according to claim 2, characterized in that: The spray gun type open flame heating uses CH4 as fuel.
4. The aluminum alloy hull welding deformation control process according to claim 1, characterized in that: The reciprocating welding is specifically as follows: The welding gap is welded from both sides of the weld to the center of the weld, which is forward movement, and moving from the center of the weld to both ends of the weld is reverse movement. During the welding process, it moves forward 50mm, then reversely moves 40mm, then moves forward 50mm, and then moves reversely, and moves in this way alternately in forward and reverse directions.
5. The aluminum alloy hull welding deformation control process according to claim 1, characterized in that: The circle welding is specifically as follows: At the beginning of welding, the welding gun and the welding point are at the same horizontal position. At this time, the welding gun draws a circle with the center point of the welding point as the center for 5 seconds at a speed of 2cm / s, and then reciprocating welding is performed.
6. The aluminum alloy hull welding deformation control process according to claim 1, characterized in that: The speed at which the rolling rollers move toward the middle is inversely proportional to the thickness of the welded part, and the force of the rolling rollers moving toward each other is directly proportional to the thickness of the welded part.