A lithium battery electrolyte additive, an electrolyte containing the additive, and a lithium battery.

By using additives such as CHB and modified diatomaceous earth in lithium battery electrolytes, the balance between overcharge prevention and electrochemical performance in lithium battery electrolytes has been resolved, thereby improving the safety and electrochemical stability of lithium batteries.

CN117096445BActive Publication Date: 2026-11-17LIUZHOU FANSAIKE NEW ENERGY TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202311308525.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-10
Publication Date
2026-11-17
Estimated Expiration
2043-10-10

AI Technical Summary

Technical Problem

Existing lithium battery electrolyte additives struggle to balance overcharge protection and electrochemical performance, leading to safety hazards and electrochemical degradation during overcharging.

Method used

A lithium battery electrolyte additive based on CHB, combined with modified diatomaceous earth, acetylene black, graphene powder and paraffin, is formed through a specific mixing and processing process to create an additive with excellent overcharge protection and minimal degradation of electrochemical performance. This includes the preparation of modified diatomaceous earth and optimization of the additive ratio.

Benefits of technology

It improves the overcharge safety performance of lithium batteries, reduces the risk of thermal runaway during overcharging, and maintains the stability of the battery's electrochemical performance and cycle performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004487028680000041
    Figure BDA0004487028680000041
  • Figure BDA0004487028680000051
    Figure BDA0004487028680000051
  • Figure BDA0004487028680000171
    Figure BDA0004487028680000171
Patent Text Reader

Abstract

This invention provides a lithium battery electrolyte additive, an electrolyte containing the additive, and a lithium battery, relating to the field of lithium battery technology. The lithium battery electrolyte additive, by weight, comprises: 100 parts CHB, 15-20 parts modified diatomaceous earth, 2-3 parts acetylene black, 13-15 parts graphene powder, and 6-8 parts paraffin wax. CHB is selected for optimization to develop a battery electrolyte overcharge prevention additive with good overcharge protection and minimal degradation of electrochemical performance. The addition amount of the lithium battery electrolyte additive is 5-7 wt% to effectively prevent overcharging. When overcharging occurs, CHB monomers undergo dehydrogenation electropolymerization to form polycyclohexylbenzene and generate hydrogen gas. This increases the battery's internal resistance, preventing thermal runaway and improving the battery's overcharge safety performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium battery technology, and in particular to a lithium battery electrolyte additive, an electrolyte containing the additive, and a lithium battery. Background Technology

[0002] Lithium-ion batteries are rechargeable batteries that primarily function by the movement of lithium ions between the positive and negative electrodes. During charging and discharging, Li... + Intercalation and deintercalation between the two electrodes: During charging, Li... + Lithium ions are extracted from the positive electrode, pass through the electrolyte, and embed into the negative electrode, which is then in a lithium-rich state. The process reverses during discharge. Lithium-based batteries typically use materials containing lithium as electrodes and are representative of modern high-performance batteries. Lithium-based batteries are divided into lithium-ion batteries and lithium-ion batteries. Mobile phones and laptops use lithium-ion batteries, commonly referred to as lithium batteries. When a lithium-ion battery is charged, lithium ions are generated at the positive electrode and move through the electrolyte to the negative electrode. The carbon layer at the negative electrode has a layered structure with many micropores. The lithium ions that reach the negative electrode embed into these micropores; the more lithium ions embedded, the higher the charging capacity. Similarly, when the battery is discharged (i.e., when we use the battery), the lithium ions embedded in the carbon layer at the negative electrode are extracted and move back to the positive electrode. The more lithium ions return to the positive electrode, the higher the discharge capacity.

[0003] Currently, commonly used overcharge protection additives for battery electrolytes include BP, CHB, and TAB. Among them, BP has good overcharge protection performance, but high concentrations can easily lead to electrochemical performance degradation; CHB has good overcharge protection performance, but high concentrations may also lead to electrochemical performance degradation; TAB's overcharge protection performance is not as good as BP and CHB, but its electrochemical performance degradation is smaller. In summary, each type of overcharge protection additive for battery electrolytes has its advantages and disadvantages. This application selects CHB, which has good overcharge protection performance, for optimization, and develops a battery electrolyte overcharge protection additive with good overcharge protection performance and smaller electrochemical performance degradation. Summary of the Invention

[0004] The purpose of this invention is to address the aforementioned problems by providing a lithium battery electrolyte additive with good overcharge protection and minimal degradation of electrochemical performance, as well as an electrolyte containing the additive and a lithium battery.

[0005] This invention is achieved through the following technical solution:

[0006] This invention provides a lithium battery electrolyte additive, which, by weight, comprises: 100 parts CHB, 15-20 parts modified diatomaceous earth, 2-3 parts acetylene black, 13-15 parts graphene powder, and 6-8 parts paraffin wax.

[0007] The lithium battery electrolyte additive is prepared according to the following steps:

[0008] (1) Weigh each component that makes up the lithium battery electrolyte additive according to the proportion;

[0009] (2) Mix the acetylene black, graphene powder and paraffin obtained in step (1) evenly to obtain a mixture;

[0010] (3) Mix diatomaceous earth and modification liquid evenly according to the ratio of 1 part by weight of diatomaceous earth to 1.8 to 2.2 parts by weight of modification liquid, ultrasonically grind for 50 to 60 minutes, and spray dry to obtain modified diatomaceous earth; the modification liquid includes, by weight, 3 parts of coupling agent KH-550, 15 to 20 parts of ethylene glycol, 20 to 25 parts of ethanol, and 10 to 15 parts of water.

[0011] (4) Add CHB and modified diatomaceous earth to the mixture, mix evenly, granulate, and then grind to 1000-1200 mesh to obtain the lithium battery electrolyte additive.

[0012] Furthermore, the lithium battery electrolyte additives, by weight, include: 100 parts CHB, 17-20 parts modified diatomaceous earth, 2.5-3 parts acetylene black, 14-15 parts graphene powder, and 7-8 parts paraffin wax.

[0013] Furthermore, the lithium battery electrolyte additives, by weight, include: 100 parts CHB, 18-20 parts modified diatomaceous earth, 2.7-3 parts acetylene black, 14.5-15 parts graphene powder, and 7.5-8 parts paraffin wax.

[0014] Further, in step (3), the modified liquid comprises, by weight, 3 parts of coupling agent KH-550, 18-20 parts of ethylene glycol, 23-25 ​​parts of ethanol, and 12-15 parts of water.

[0015] Further, in step (3), the diatomaceous earth and the modification liquid are mixed evenly according to the ratio of 1 part by weight of diatomaceous earth to 2.1 to 2.2 parts by weight of modification liquid, ultrasonically ground for 55 to 60 minutes, and spray dried to obtain modified diatomaceous earth.

[0016] Further, in step (4), CHB and modified diatomaceous earth are added to the mixture, mixed evenly, granulated, and then ground to 1100-1200 mesh to obtain the lithium battery electrolyte additive.

[0017] The present invention also provides a lithium battery electrolyte, wherein the lithium battery electrolyte contains the lithium battery electrolyte additive described in any one of claims 1-6.

[0018] Furthermore, the lithium battery electrolyte also includes lithium hexafluorophosphate, ethylene carbonate, and dimethyl carbonate.

[0019] Furthermore, the amount of the lithium battery electrolyte additive added to the lithium battery electrolyte is 5-7 wt%.

[0020] The present invention also provides a lithium battery, the lithium battery comprising: a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and a lithium battery electrolyte; the lithium battery electrolyte is the lithium battery electrolyte according to any one of claims 7-9.

[0021] Cyclohexylbenzene (phenylcyclohexane) is an important chemical intermediate with a high boiling point and a freezing point close to room temperature. In the lithium battery field, cyclohexylbenzene is mainly used as an additive in lithium-ion battery electrolytes to prevent overcharging and improve the safety of lithium batteries. As an overcharge protection additive, it should have the following characteristics: good solubility and fast diffusion rate in organic electrolytes, providing protection in a high current range; good stability within the battery operating temperature range; suitable oxidation potential; no other side reactions generated during the reduction process of oxidation products; Currently, there are two explanations for the overcharge protection mechanism of cyclohexylbenzene: (1) self-discharge mechanism: when the battery is charged to a certain voltage, the additive monomer undergoes electropolymerization, generating a conductive polymer film on the positive electrode surface, causing the battery to self-discharge to a safe state; (2) blocking mechanism: when the battery voltage exceeds the electropolymerization voltage of the additive, the additive monomer undergoes polymerization reaction, generating black polycyclohexylbenzene, forming a blocking layer on the electrode surface, causing the battery internal resistance to increase rapidly, thereby slowing down or preventing further decomposition of the electrolyte, significantly reducing the generated gas and heat, preventing thermal runaway, and keeping the battery in a safe state. The introduction of cyclohexylbenzene additive has no effect on the initial discharge capacity of the battery, but excessive cyclohexylbenzene addition will affect the battery's cycle performance. Therefore, a suitable proportion of cyclohexylbenzene additive can ensure the battery's cycle performance and service life. Studies have shown that cyclohexylbenzene achieves optimal performance when its content in the electrolyte is 5%–7% (by mass). When the cyclohexylbenzene content is less than 5%, its overcharge prevention effect in lithium-ion battery electrolytes is not significant; when the content is greater than 7%, it leads to a decrease in electrolyte conductivity, a decline in battery cycle performance, and an increase in self-discharge. Currently, the main approach is to rationally control the cyclohexylbenzene content in the electrolyte to maximize its overcharge prevention effect in lithium batteries.

[0022] This invention discloses a lithium battery electrolyte additive, an electrolyte containing the additive, and a lithium battery. CHB was selected for optimization to develop a battery electrolyte overcharge prevention additive with good overcharge protection performance and minimal degradation of electrochemical performance. The amount of the lithium battery electrolyte additive added to the lithium battery electrolyte is 5-7 wt% to effectively prevent overcharging.

[0023] This invention provides a lithium battery electrolyte additive, an electrolyte containing the additive, and a lithium battery. When overcharging occurs, CHB monomers undergo dehydrogenation electropolymerization to form polycyclohexylbenzene and generate hydrogen gas. This increases the battery's internal resistance, thereby preventing thermal runaway and improving the battery's overcharge safety performance.

[0024] The reaction formula for CHB monomer is as follows:

[0025] Attached Figure Description

[0026] Figure 1 This is a production flow diagram of the lithium battery electrolyte of the present invention. Detailed Implementation

[0027] Any feature disclosed in this specification (including any appended claims and abstract) may be replaced by other equivalent or similar features, unless specifically stated otherwise. That is, unless specifically stated otherwise, each feature is merely one example of a series of equivalent or similar features.

[0028] This invention discloses a lithium battery electrolyte additive, an electrolyte containing the additive, and a lithium battery. In the following embodiments, during the stirring and additive addition step, the added lithium battery electrolyte additive, by weight, comprises: 100 parts CHB, 15-20 parts modified diatomaceous earth, 2-3 parts acetylene black, 13-15 parts graphene powder, and 6-8 parts paraffin wax. The function of the lithium battery electrolyte additive is to prevent overcharging.

[0029] This invention discloses a lithium battery electrolyte additive, an electrolyte containing the additive, and a lithium battery. When preparing a lithium battery using the electrolyte in the following examples and comparative examples, since the lithium battery includes: a positive electrode, a negative electrode, a separator placed between the positive and negative electrodes, and a lithium battery electrolyte; to simplify the process, the lithium battery electrolyte is directly injected into a pre-made battery casing with dimensions of: a thickness of 7.5 cm (±0.2), a width of 16.5 cm (±0.2), and a length of 61 cm (±0.2). After the lithium battery electrolyte injection is completed and no other problems are found, the battery performance can be tested.

[0030] This invention discloses a lithium battery electrolyte additive, an electrolyte containing the additive, and a lithium battery. The operation methods and operation times of each step in the following embodiments are shown in Table 1 below:

[0031] Table 1

[0032]

[0033] Example 1

[0034] A method for preparing a lithium battery electrolyte includes the following steps:

[0035] Incoming material inspection and production preparation:

[0036] First, the incoming materials are inspected. After the raw materials are sampled and tested and found to be qualified, the unloading personnel connect the nitrogen pipeline to the top of the tank truck, open the nitrogen pipeline valve and the nitrogen inlet valve on the top of the truck to ensure continuous pressure replenishment of the tank. Then, the flange ball valve, exhaust valve, fluid loading and unloading arm outlet valve and inlet valve are opened in sequence. The main unloading valve of the tank truck is opened. After the raw materials enter the magnetic pump, the flange ball valve is closed and the magnetic pump is turned on. After the magnetic pump stabilizes, the flange ball valve is slowly opened to carry out normal unloading.

[0037] Preparation of the reactor cleaning and addition of various solvents:

[0038] First, clean the mixing vessel; then, according to the "Production Batching Process Sheet", confirm that the solvent used meets the usage amount and that the specified mixing vessel is empty. Click the ratio selection for the corresponding mixing vessel, enter the theoretical usage amount of the solvent required by the formula according to the "Production Batching Process Sheet", click to confirm the formula, click "Automatic Feeding", click the reset button in the pop-up interface, click the flow accumulation reset button, confirm that the feed weight is all displayed as zero, and then click the "Not Started" button to start automatic feeding.

[0039] Solvent stirring:

[0040] In the central control system, click the start motor of the corresponding mixing vessel. In the pop-up interface, click the start button, then click the frequency control button for the stirring motor. In the pop-up interface, set the frequency to 40Hz to start the stirring motor. Ensure the stirring motor indicator above the mixing vessel is green. After completing the solvent mixing operation, record the stirring frequency, pressure, and stirring time on the "Production Batching Process Sheet".

[0041] Solvent control and detection:

[0042] First, fill in the corresponding batch, model, and equipment number in the header of the inspection application form. Next, in the solvent mixing section, fill in the corresponding inspection date, time, completion time, required testing items, and the name of the person applying for inspection. Finally, forward it to the Quality and Technical Department. After passing the inspection, return it to the main control unit to proceed to the next step.

[0043] Cooling the preparation vessel:

[0044] To cool down the mixing vessel, click on the corresponding mixing vessel in the central control system, then click on the chilled water supply pneumatic valve of the mixing vessel, and click the "Open" button on the pop-up page; go to the refrigeration room to turn on the refrigeration unit, and observe the temperature of the mixing vessel, which needs to be reduced to -5 to -5℃.

[0045] Stir and add solute:

[0046] Add T01 lithium salt. The batching operator confirms the status of the T01 material, places the finished T01 material drum on the electronic scale and connects the quick-connect flange, zeros the electronic scale, opens the nitrogen valve and the T01 material drum valve to pressurize the T01 material drum, closes the nitrogen valve, opens the feeding valve of the mixing tank, and starts adding T01. Fill in the T01 drum number, batch number and quantity, as well as the pressure, frequency of the mixing tank and the stirring start time on the "Production Batching Process Sheet".

[0047] Click the start motor button of the corresponding mixing tank in the central control system, click the start button on the pop-up interface, click the frequency control button of the stirring motor, set 40Hz on the pop-up interface, and complete the start-up of the stirring motor. Confirm that the stirring motor above the used mixing tank shows a green light. After completing the solvent mixing operation, record the stirring frequency, pressure and stirring time on the "Production Batching Process Sheet".

[0048] Fill in the corresponding inspection application date, time, completion time, items to be tested and inspection applicant in the T01 electrolyte addition column, then transfer to the Quality and Technology Department. After the test is qualified, return it to the main control to proceed to the next step.

[0049] Stirring and adding additives:

[0050] Additive addition is divided into the addition of two types of additives: solid and liquid. For liquid addition (combining manual and automatic feeding), the automatic additive addition is to input the corresponding additive quantity through the main control, and the additive is delivered to the corresponding mixing tank through the pipeline of the workshop additive tank. For manual additive addition, the batching operator fully opens the feeding valve of the mixing tank below the glove box, adds all the solid additives into the mixing tank through the feeding pipeline, and completes the feeding work.

[0051] Electrolyte stirring and mixing:

[0052] Click the start motor button of the corresponding mixing tank in the central control system, click the start button on the pop-up interface, click the frequency control button of the stirring motor, set 40Hz on the pop-up interface, and complete the start-up of the stirring motor. Confirm that the stirring motor above the used mixing tank shows a green light. After completing the solvent mixing operation, record the stirring frequency, pressure and stirring time on the "Production Batching Process Sheet".

[0053] Finished product filtration:

[0054] The finished product obtained from the electrolyte stirring and mixing step is filtered to remove impurities.

[0055] Finished product testing:

[0056] After the finished product is filtered, finished product testing is carried out. Fill in the corresponding inspection application date, time, completion time, items to be tested and inspection applicant in the finished electrolyte column, then transfer to the Quality and Technology Department. A qualified return after testing indicates that the finished product is completed and qualified.

[0057] Packaging barrel preparation process, product packaging process:

[0058] The automated filling line is remotely controlled via the Sunflower software. Filling operators click on the "MES" management system in the operation interface on the display screen according to the production order, and then click "Create Work Order" in the "MES" system. After preparing a series of filling tasks, filling can begin.

[0059] In the above stirring and additive steps, the added lithium battery electrolyte additives, by weight, include: 100 parts CHB, 15 parts modified diatomaceous earth, 2 parts acetylene black, 13 parts graphene powder, and 6 parts paraffin wax; the amount of the lithium battery electrolyte additives added to the lithium battery electrolyte is 5 wt%.

[0060] The lithium battery electrolyte additive is prepared according to the following steps:

[0061] (1) Weigh each component that makes up the lithium battery electrolyte additive according to the proportion;

[0062] (2) Mix the acetylene black, graphene powder and paraffin obtained in step (1) evenly to obtain a mixture;

[0063] (3) Mix the diatomaceous earth and the modification liquid evenly according to the ratio of 1 part by weight of diatomaceous earth to 1.8 parts by weight of modification liquid, ultrasonically grind for 50 minutes, and spray dry to obtain modified diatomaceous earth; the modification liquid includes, by weight, 3 parts of coupling agent KH-550, 15 parts of ethylene glycol, 20 parts of ethanol and 10 parts of water.

[0064] (4) Add CHB and modified diatomaceous earth to the mixture, mix evenly, granulate, and then grind to 1000 mesh to obtain the lithium battery electrolyte additive.

[0065] Example 2

[0066] A method for preparing a lithium battery electrolyte includes the following steps:

[0067] Incoming material inspection and production preparation:

[0068] First, the incoming materials are inspected. After the raw materials are sampled and tested and found to be qualified, the unloading personnel connect the nitrogen pipeline to the top of the tank truck, open the nitrogen pipeline valve and the nitrogen inlet valve on the top of the truck to ensure continuous pressure replenishment of the tank. Then, the flange ball valve, exhaust valve, fluid loading and unloading arm outlet valve and inlet valve are opened in sequence. The main unloading valve of the tank truck is opened. After the raw materials enter the magnetic pump, the flange ball valve is closed and the magnetic pump is turned on. After the magnetic pump stabilizes, the flange ball valve is slowly opened to carry out normal unloading.

[0069] Preparation of the reactor cleaning and addition of various solvents:

[0070] First, clean the mixing vessel; then, according to the "Production Batching Process Sheet", confirm that the solvent used meets the usage amount and that the specified mixing vessel is empty. Click the ratio selection for the corresponding mixing vessel, enter the theoretical usage amount of the solvent required by the formula according to the "Production Batching Process Sheet", click to confirm the formula, click "Automatic Feeding", click the reset button in the pop-up interface, click the flow accumulation reset button, confirm that the feed weight is all displayed as zero, and then click the "Not Started" button to start automatic feeding.

[0071] Solvent stirring:

[0072] In the central control system, click the start motor of the corresponding mixing vessel. In the pop-up interface, click the start button, then click the frequency control button for the stirring motor. In the pop-up interface, set the frequency to 40Hz to start the stirring motor. Ensure the stirring motor indicator above the mixing vessel is green. After completing the solvent mixing operation, record the stirring frequency, pressure, and stirring time on the "Production Batching Process Sheet".

[0073] Solvent control and detection:

[0074] First, fill in the corresponding batch, model, and equipment number in the header of the inspection application form. Next, in the solvent mixing section, fill in the corresponding inspection date, time, completion time, required testing items, and the name of the person applying for inspection. Finally, forward it to the Quality and Technical Department. After passing the inspection, return it to the main control unit to proceed to the next step.

[0075] Cooling the preparation vessel:

[0076] To cool down the mixing vessel, click on the corresponding mixing vessel in the central control system, then click on the chilled water supply pneumatic valve of the mixing vessel, and click the "Open" button on the pop-up page; go to the refrigeration room to turn on the refrigeration unit, and observe the temperature of the mixing vessel, which needs to be reduced to -5 to -5℃.

[0077] Stir and add solute:

[0078] Add lithium salt T01. The mixing worker confirms the state of the T01 material, places the finished T01 material barrel on the electronic scale and connects the flange quick connector, zeroes the electronic scale, opens the nitrogen valve and the T01 material barrel valve to pressurize the T01 material barrel, closes the nitrogen valve, opens the feed valve of the mixing kettle, and adds T01. Fill in the T01 barrel number, batch number and quantity, mixing kettle pressure, frequency and start stirring time on the "Production Batching Process Sheet".

[0079] In the central control system, click the start motor of the corresponding mixing vessel. In the pop-up interface, click the start button, then click the frequency control button for the stirring motor. In the pop-up interface, set the frequency to 40Hz to start the stirring motor. Ensure the stirring motor indicator above the mixing vessel is green. After completing the solvent mixing operation, record the stirring frequency, pressure, and stirring time on the "Production Batching Process Sheet".

[0080] Fill in the corresponding inspection application date, time, completion time, items to be tested and inspector in the column for adding T01 electrolyte, then transfer to the Quality and Technology Department. After passing the test, return it to the main control to proceed to the next step.

[0081] Stirring and adding additives:

[0082] Additives are divided into two types: solid additives and liquid additives; for liquid addition (combining manual and automatic feeding), automatic additive addition is performed by inputting the corresponding additive amount via the main control, and the additive is conveyed through the workshop additive tank pipeline to the corresponding preparation kettle; manual additive addition is that the preparation operator fully opens the feeding valve of the preparation kettle below the glove box, adds all solid additives into the preparation kettle through the feeding pipeline to complete the feeding work;

[0083] Electrolyte stirring and mixing:

[0084] Click the start motor of the corresponding preparation kettle in the central control system, click the start button on the pop-up interface, click the frequency control button of the stirring motor, set 40Hz on the pop-up interface to complete the start of the stirring motor. Confirm that the stirring motor above the used preparation kettle shows a green light, and record the stirring frequency, pressure and stirring time on the "Production Batching Process Sheet" after completing the solvent mixing operation.

[0085] Finished product filtration:

[0086] Filter and remove impurities from the finished product obtained by the electrolyte stirring and mixing step.

[0087] Finished product testing:

[0088] After the finished product is filtered, the finished product is tested; fill in the corresponding inspection application date, time, completion time, items to be tested and inspector in the finished electrolyte column, then transfer to the Quality and Technology Department. Passing the test indicates that the finished product is completed and qualified.

[0089] Packaging bucket preparation process, product packaging process:

[0090] The automatic filling line is connected with the main control Sunflower software for remote control. The filling operator clicks the "MES" management system on the operation interface in the display screen according to the production order, and clicks "Create Work Order" in the "MES" system. After completing a series of filling preparations, the filling can be carried out.

[0091] In the above step of stirring and adding additives, the added lithium battery electrolyte additives include, in parts by weight: 100 parts of CHB, 20 parts of modified diatomaceous earth, 3 parts of acetylene black, 15 parts of graphene powder, and 8 parts of paraffin; the addition amount of the lithium battery electrolyte additive in the lithium battery electrolyte is 7wt%;

[0092] The lithium battery electrolyte additive is prepared according to the following steps:

[0093] (1) Weigh each component that makes up the lithium battery electrolyte additive according to the proportion;

[0094] (2) Mix the acetylene black, graphene powder and paraffin obtained in step (1) evenly to obtain a mixture;

[0095] (3) Mix the diatomaceous earth and the modification liquid evenly according to the ratio of 1 part by weight of diatomaceous earth to 2.2 parts by weight of modification liquid, ultrasonically grind for 60 minutes, and spray dry to obtain modified diatomaceous earth; the modification liquid includes, by weight, 3 parts of coupling agent KH-550, 20 parts of ethylene glycol, 25 parts of ethanol, and 15 parts of water.

[0096] (4) Add CHB and modified diatomaceous earth to the mixture, mix evenly, granulate, and then grind to 1200 mesh to obtain the lithium battery electrolyte additive.

[0097] Example 3

[0098] A method for preparing a lithium battery electrolyte includes the following steps:

[0099] Incoming material inspection and production preparation:

[0100] First, the incoming materials are inspected. After the raw materials are sampled and tested and found to be qualified, the unloading personnel connect the nitrogen pipeline to the top of the tank truck, open the nitrogen pipeline valve and the nitrogen inlet valve on the top of the truck to ensure continuous pressure replenishment of the tank. Then, the flange ball valve, exhaust valve, fluid loading and unloading arm outlet valve and inlet valve are opened in sequence. The main unloading valve of the tank truck is opened. After the raw materials enter the magnetic pump, the flange ball valve is closed and the magnetic pump is turned on. After the magnetic pump stabilizes, the flange ball valve is slowly opened to carry out normal unloading.

[0101] Preparation of the reactor cleaning and addition of various solvents:

[0102] First, clean the mixing vessel; then, according to the "Production Batching Process Sheet", confirm that the solvent used meets the usage amount and that the specified mixing vessel is empty. Click the ratio selection for the corresponding mixing vessel, enter the theoretical usage amount of the solvent required by the formula according to the "Production Batching Process Sheet", click to confirm the formula, click "Automatic Feeding", click the reset button in the pop-up interface, click the flow accumulation reset button, confirm that the feed weight is all displayed as zero, and then click the "Not Started" button to start automatic feeding.

[0103] Solvent stirring:

[0104] In the central control system, click the start motor of the corresponding mixing vessel. In the pop-up interface, click the start button, then click the frequency control button for the stirring motor. In the pop-up interface, set the frequency to 40Hz to start the stirring motor. Ensure the stirring motor indicator above the mixing vessel is green. After completing the solvent mixing operation, record the stirring frequency, pressure, and stirring time on the "Production Batching Process Sheet".

[0105] Solvent control and detection:

[0106] First, fill in the corresponding batch, model, and equipment number in the header of the inspection application form. Next, in the solvent mixing section, fill in the corresponding inspection date, time, completion time, required testing items, and the name of the person applying for inspection. Finally, forward it to the Quality and Technical Department. After passing the inspection, return it to the main control unit to proceed to the next step.

[0107] Cooling the preparation vessel:

[0108] To cool down the mixing vessel, click on the corresponding mixing vessel in the central control system, then click on the chilled water supply pneumatic valve of the mixing vessel, and click the "Open" button on the pop-up page; go to the refrigeration room to turn on the refrigeration unit, and observe the temperature of the mixing vessel, which needs to be reduced to -5 to -5℃.

[0109] Stir and add solute:

[0110] Add lithium salt T01. The mixing worker confirms the state of the T01 material, places the finished T01 material barrel on the electronic scale and connects the flange quick connector, zeroes the electronic scale, opens the nitrogen valve and the T01 material barrel valve to pressurize the T01 material barrel, closes the nitrogen valve, opens the feed valve of the mixing kettle, and adds T01. Fill in the T01 barrel number, batch number and quantity, mixing kettle pressure, frequency and start stirring time on the "Production Batching Process Sheet".

[0111] In the central control system, click the start motor of the corresponding mixing vessel. In the pop-up interface, click the start button, then click the frequency control button for the stirring motor. In the pop-up interface, set the frequency to 40Hz to start the stirring motor. Ensure the stirring motor indicator above the mixing vessel is green. After completing the solvent mixing operation, record the stirring frequency, pressure, and stirring time on the "Production Batching Process Sheet".

[0112] In the "Add T01 Electrolyte" field, fill in the corresponding inspection date, time, completion time, required testing items, and the person submitting the application. Then, forward it to the Quality and Technical Department. After passing the inspection, return it to the main control unit to proceed to the next step.

[0113] Add additives by stirring:

[0114] The addition of additives is divided into the addition of two types of additives: solid and liquid; for liquid addition (combining manual and automatic feeding), the automatic addition of additives is carried out by inputting the corresponding amount of additive through the main control, and the additive is conveyed to the corresponding preparation kettle through the pipeline of the workshop additive tank; for manual addition of additives, the preparation operator fully opens the feed valve of the preparation kettle below the glove box, adds all the solid additives into the preparation kettle through the feeding pipeline, and completes the feeding work;

[0115] Electrolyte stirring and mixing:

[0116] Click the start motor of the corresponding preparation kettle in the central control system, click the start button on the pop-up interface, click the frequency control button of the stirring motor, set 40Hz on the pop-up interface, and complete the start-up of the stirring motor. Confirm that the stirring motor above the used preparation kettle shows a green light, and record the stirring frequency, pressure and stirring time on the "Production Batching Process Sheet" after the solvent mixing operation is completed.

[0117] Finished product filtration:

[0118] The finished product obtained from the electrolyte stirring and mixing step is filtered to remove impurities.

[0119] Finished product inspection:

[0120] After the finished product is filtered, the finished product is inspected; fill in the corresponding inspection application date, time, completion time, items to be inspected and inspection applicant in the column of finished electrolyte, and then transfer to the Quality and Technology Department. After passing the inspection, it indicates that the finished product is completed and qualified.

[0121] Packaging bucket preparation process, product packaging process:

[0122] The automatic filling line is connected with the main control Sunflower software for remote control. The filling operator clicks the "MES" management system on the operation interface in the display screen according to the production order, and clicks "Create Work Order" in the "MES" system. After a series of filling preparations are completed, the filling can be carried out.

[0123] In the above step of stirring and adding additives, the lithium battery electrolyte additive added includes, in parts by weight: 100 parts of CHB, 17 parts of modified diatomaceous earth, 2.5 parts of acetylene black, 14 parts of graphene powder, and 7 parts of paraffin; the addition amount of the lithium battery electrolyte additive in the lithium battery electrolyte is 6 wt%;

[0124] The lithium battery electrolyte additive is prepared according to the following steps:

[0125] (1) Weigh each component constituting the lithium battery electrolyte additive according to the ratio;

[0126] (2) Mix the acetylene black, graphene powder and paraffin weighed in step (1) uniformly to obtain a mixture;

[0127] (3) Mix the diatomaceous earth and the modification liquid evenly according to the ratio of 1 part by weight of diatomaceous earth to 2.1 parts by weight of modification liquid, ultrasonically grind for 55 minutes, and spray dry to obtain modified diatomaceous earth; the modification liquid includes, by weight, 3 parts of coupling agent KH-550, 18 parts of ethylene glycol, 23 parts of ethanol, and 12 parts of water.

[0128] (4) Add CHB and modified diatomaceous earth to the mixture, mix evenly, granulate, and then grind to 1100 mesh to obtain the lithium battery electrolyte additive.

[0129] Example 4

[0130] A method for preparing a lithium battery electrolyte includes the following steps:

[0131] Incoming material inspection and production preparation:

[0132] First, the incoming materials are inspected. After the raw materials are sampled and tested and found to be qualified, the unloading personnel connect the nitrogen pipeline to the top of the tank truck, open the nitrogen pipeline valve and the nitrogen inlet valve on the top of the truck to ensure continuous pressure replenishment of the tank. Then, the flange ball valve, exhaust valve, fluid loading and unloading arm outlet valve and inlet valve are opened in sequence. The main unloading valve of the tank truck is opened. After the raw materials enter the magnetic pump, the flange ball valve is closed and the magnetic pump is turned on. After the magnetic pump stabilizes, the flange ball valve is slowly opened to carry out normal unloading.

[0133] Preparation of the reactor cleaning and addition of various solvents:

[0134] First, clean the mixing vessel; then, according to the "Production Batching Process Sheet", confirm that the solvent used meets the usage amount and that the specified mixing vessel is empty. Click the ratio selection for the corresponding mixing vessel, enter the theoretical usage amount of the solvent required by the formula according to the "Production Batching Process Sheet", click to confirm the formula, click "Automatic Feeding", click the reset button in the pop-up interface, click the flow accumulation reset button, confirm that the feed weight is all displayed as zero, and then click the "Not Started" button to start automatic feeding.

[0135] Solvent stirring:

[0136] In the central control system, click the start motor of the corresponding mixing vessel. In the pop-up interface, click the start button, then click the frequency control button for the stirring motor. In the pop-up interface, set the frequency to 40Hz to start the stirring motor. Ensure the stirring motor indicator above the mixing vessel is green. After completing the solvent mixing operation, record the stirring frequency, pressure, and stirring time on the "Production Batching Process Sheet".

[0137] Solvent control and detection:

[0138] First, fill in the corresponding batch, model, and equipment number in the header of the inspection application form. Next, in the solvent mixing section, fill in the corresponding inspection date, time, completion time, required testing items, and the name of the person applying for inspection. Finally, forward it to the Quality and Technical Department. After passing the inspection, return it to the main control unit to proceed to the next step.

[0139] Cooling the preparation vessel:

[0140] To cool down the mixing vessel, click on the corresponding mixing vessel in the central control system, then click on the chilled water supply pneumatic valve of the mixing vessel, and click the "Open" button on the pop-up page; go to the refrigeration room to turn on the refrigeration unit, and observe the temperature of the mixing vessel, which needs to be reduced to -5 to -5℃.

[0141] Stir and add solute:

[0142] Add lithium salt T01. The mixing worker confirms the state of the T01 material, places the finished T01 material barrel on the electronic scale and connects the flange quick connector, zeroes the electronic scale, opens the nitrogen valve and the T01 material barrel valve to pressurize the T01 material barrel, closes the nitrogen valve, opens the feed valve of the mixing kettle, and adds T01. Fill in the T01 barrel number, batch number and quantity, mixing kettle pressure, frequency and start stirring time on the "Production Batching Process Sheet".

[0143] In the central control system, click the start motor of the corresponding mixing vessel. In the pop-up interface, click the start button, then click the frequency control button for the stirring motor. In the pop-up interface, set the frequency to 40Hz to start the stirring motor. Ensure the stirring motor indicator above the mixing vessel is green. After completing the solvent mixing operation, record the stirring frequency, pressure, and stirring time on the "Production Batching Process Sheet".

[0144] In the "Add T01 Electrolyte" field, fill in the corresponding inspection date, time, completion time, required testing items, and the person submitting the application. Then, forward it to the Quality and Technical Department. After passing the inspection, return it to the main control unit to proceed to the next step.

[0145] Add additives by stirring:

[0146] Additive addition is divided into two types: solid and liquid. Liquid additive addition (combination of manual and automatic feeding) involves automatic additive addition by inputting the corresponding additive quantity into the main control, and the additive is transported to the corresponding mixing vessel through the workshop additive tank pipeline. Manual additive addition involves the mixing operator fully opening the feeding valve of the mixing vessel below the glove box and adding all the solid additive into the mixing vessel through the feeding pipeline to complete the feeding work.

[0147] Electrolyte mixing:

[0148] Click the start motor of the corresponding preparation tank in the central control system, click the start button on the pop-up interface, click the frequency control button of the stirring motor, set 40Hz on the pop-up interface, and complete the start-up of the stirring motor. Confirm that the stirring motor above the used preparation tank shows a green light, and record the stirring frequency, pressure and stirring time on the "Production Batching Process Sheet" after completing the solvent mixing operation.

[0149] Finished product filtration:

[0150] The finished product obtained from the electrolyte stirring and mixing step is filtered to remove impurities.

[0151] Finished product inspection:

[0152] After the finished product is filtered, the finished product inspection is carried out; fill in the corresponding inspection application date, time, completion time, items to be inspected and inspection applicant in the finished electrolyte column, and then transfer to the quality technology department. After passing the inspection, it indicates that the finished product is completed and qualified.

[0153] Packaging barrel preparation process, product packaging process:

[0154] The automatic filling line is connected with the main control Sunflower software for remote control. The filling operator clicks the "MES" management system in the operation interface on the display screen according to the production order, and clicks "Create Work Order" in the "MES" system. After a series of filling preparations are completed, the filling can be carried out.

[0155] In the above step of adding additives under stirring, the lithium battery electrolyte additive added includes, in parts by weight: 100 parts of CHB, 18 parts of modified diatomaceous earth, 2.7 parts of acetylene black, 14.5 parts of graphene powder, and 7.5 parts of paraffin; the addition amount of the lithium battery electrolyte additive in the lithium battery electrolyte is 6wt%;

[0156] The lithium battery electrolyte additive is prepared according to the following steps:

[0157] (1) Weigh each component constituting the lithium battery electrolyte additive according to the ratio;

[0158] (2) Mix the acetylene black, graphene powder and paraffin weighed in step (1) uniformly to obtain a mixture;

[0159] (3) According to the ratio of adding 2.1 parts by weight of modifying solution to 1 part by weight of diatomaceous earth, mix diatomaceous earth and modifying solution uniformly, perform ultrasonic grinding for 55min, and then perform spray drying to obtain modified diatomaceous earth; the modifying solution includes, in parts by weight: 3 parts of coupling agent KH-550, 18 parts of ethylene glycol, 23 parts of ethanol, and 12 parts of water;

[0160] (4) Add CHB and modified diatomaceous earth to the mixture, mix evenly, granulate, and then grind to 1100 mesh to obtain the lithium battery electrolyte additive.

[0161] Comparative Example 1

[0162] A method for preparing a lithium battery electrolyte includes the following steps:

[0163] Incoming material inspection and production preparation:

[0164] First, the incoming materials are inspected. After the raw materials are sampled and tested and found to be qualified, the unloading personnel connect the nitrogen pipeline to the top of the tank truck, open the nitrogen pipeline valve and the nitrogen inlet valve on the top of the truck to ensure continuous pressure replenishment of the tank. Then, the flange ball valve, exhaust valve, fluid loading and unloading arm outlet valve and inlet valve are opened in sequence. The main unloading valve of the tank truck is opened. After the raw materials enter the magnetic pump, the flange ball valve is closed and the magnetic pump is turned on. After the magnetic pump stabilizes, the flange ball valve is slowly opened to carry out normal unloading.

[0165] Preparation of the reactor cleaning and addition of various solvents:

[0166] First, clean the mixing vessel; then, according to the "Production Batching Process Sheet", confirm that the solvent used meets the usage amount and that the specified mixing vessel is empty. Click the ratio selection for the corresponding mixing vessel, enter the theoretical usage amount of the solvent required by the formula according to the "Production Batching Process Sheet", click to confirm the formula, click "Automatic Feeding", click the reset button in the pop-up interface, click the flow accumulation reset button, confirm that the feed weight is all displayed as zero, and then click the "Not Started" button to start automatic feeding.

[0167] Solvent stirring:

[0168] In the central control system, click the start motor of the corresponding mixing vessel. In the pop-up interface, click the start button, then click the frequency control button for the stirring motor. In the pop-up interface, set the frequency to 40Hz to start the stirring motor. Ensure the stirring motor indicator above the mixing vessel is green. After completing the solvent mixing operation, record the stirring frequency, pressure, and stirring time on the "Production Batching Process Sheet".

[0169] Solvent control and detection:

[0170] First, fill in the corresponding batch, model, and equipment number in the header of the inspection application form. Next, in the solvent mixing section, fill in the corresponding inspection date, time, completion time, required testing items, and the name of the person applying for inspection. Finally, forward it to the Quality and Technical Department. After passing the inspection, return it to the main control unit to proceed to the next step.

[0171] Cooling the preparation vessel:

[0172] To cool down the mixing vessel, click on the corresponding mixing vessel in the central control system, then click on the chilled water supply pneumatic valve of the mixing vessel, and click the "Open" button on the pop-up page; go to the refrigeration room to turn on the refrigeration unit, and observe the temperature of the mixing vessel, which needs to be reduced to -5 to -5℃.

[0173] Stir and add solute:

[0174] Add lithium salt T01. The mixing worker confirms the state of the T01 material, places the finished T01 material barrel on the electronic scale and connects the flange quick connector, zeroes the electronic scale, opens the nitrogen valve and the T01 material barrel valve to pressurize the T01 material barrel, closes the nitrogen valve, opens the feed valve of the mixing kettle, and adds T01. Fill in the T01 barrel number, batch number and quantity, mixing kettle pressure, frequency and start stirring time on the "Production Batching Process Sheet".

[0175] In the central control system, click the start motor of the corresponding mixing vessel. In the pop-up interface, click the start button, then click the frequency control button for the stirring motor. In the pop-up interface, set the frequency to 40Hz to start the stirring motor. Ensure the stirring motor indicator above the mixing vessel is green. After completing the solvent mixing operation, record the stirring frequency, pressure, and stirring time on the "Production Batching Process Sheet".

[0176] In the "Add T01 Electrolyte" field, fill in the corresponding inspection date, time, completion time, required testing items, and the person submitting the application. Then, forward it to the Quality and Technical Department. After passing the inspection, return it to the main control unit to proceed to the next step.

[0177] Add additives by stirring:

[0178] Additive addition is divided into two types: solid and liquid. Liquid additive addition (combination of manual and automatic feeding) involves automatic additive addition by inputting the corresponding additive quantity into the main control, and the additive is transported to the corresponding mixing vessel through the workshop additive tank pipeline. Manual additive addition involves the mixing operator fully opening the feeding valve of the mixing vessel below the glove box and adding all the solid additive into the mixing vessel through the feeding pipeline to complete the feeding work.

[0179] Electrolyte mixing:

[0180] In the central control system, click the start motor of the corresponding mixing vessel. In the pop-up interface, click the start button, then click the frequency control button for the stirring motor. In the pop-up interface, set the frequency to 40Hz to start the stirring motor. Ensure the stirring motor indicator above the mixing vessel is green. After completing the solvent mixing operation, record the stirring frequency, pressure, and stirring time on the "Production Batching Process Sheet".

[0181] Finished product filtration:

[0182] The finished product obtained from the electrolyte stirring and mixing step is filtered to remove impurities.

[0183] Finished product inspection:

[0184] After the finished product is filtered, finished product inspection is carried out; fill in the corresponding inspection application date, time, completion time, items to be inspected and inspection applicant in the column of finished electrolyte, and then transfer to the Quality and Technology Department. After passing the inspection, it indicates that the finished product is completed and qualified.

[0185] Packaging drum preparation process, product packaging process:

[0186] The automatic filling line is connected to the main control Sunflower software for remote control. The filling operator clicks the "MES" management system on the operation interface in the display screen according to the production order, and clicks "Create Work Order" in the "MES" system. After a series of filling preparations are completed, the filling can be carried out.

[0187] In the above step of stirring and adding additives, the lithium battery electrolyte additive added includes, in parts by weight: 100 parts of CHB, 18 parts of diatomaceous earth, 2.7 parts of acetylene black, 14.5 parts of graphene powder, and 7.5 parts of paraffin; the addition amount of the lithium battery electrolyte additive in the lithium battery electrolyte is 6 wt%; each component constituting the lithium battery electrolyte additive is weighed according to the ratio and mixed uniformly to obtain the lithium battery electrolyte additive.

[0188] Comparative Example 2

[0189] A preparation method of lithium battery electrolyte, comprising the following steps:

[0190] Incoming material inspection, production preparation:

[0191] First, incoming material inspection is carried out. After the sampled raw materials are tested to be qualified, the unloading personnel connect the top of the tank truck with a nitrogen pipeline, open the nitrogen pipeline valve and the nitrogen inlet valve on the top of the tank to ensure continuous pressure supplement for the tank body; open the flange ball valve, exhaust valve, the valve at the outlet of the fluid loading and unloading arm and the inlet valve in sequence, open the main unloading valve of the tank truck, close the flange ball valve and start the magnetic pump after the raw material enters the magnetic pump, and slowly open the flange ball valve after the magnetic pump is stabilized to carry out normal unloading.

[0192] Preparation kettle cleaning, feeding of each solvent:

[0193] First, clean the preparation kettle; then confirm that the solvents to be used meet the usage amount and the designated preparation kettle is empty according to the "Production Batching Process Sheet", click the proportion selection of the corresponding preparation kettle, input the theoretical usage amount of the solvent required by the formula according to the "Production Batching Process Sheet", click to confirm the formula, click "Automatic Feeding", click the reset button on the pop-up interface, click the flow cumulative reset button, and click the not-started button to carry out automatic feeding after confirming that all the displayed feeding weights are zero.

[0194] Solvent stirring:

[0195] In the central control system, click the start motor of the corresponding mixing vessel. In the pop-up interface, click the start button, then click the frequency control button for the stirring motor. In the pop-up interface, set the frequency to 40Hz to start the stirring motor. Ensure the stirring motor indicator above the mixing vessel is green. After completing the solvent mixing operation, record the stirring frequency, pressure, and stirring time on the "Production Batching Process Sheet".

[0196] Solvent control and detection:

[0197] First, fill in the corresponding batch, model, and equipment number in the header of the inspection application form. Next, in the solvent mixing section, fill in the corresponding inspection date, time, completion time, required testing items, and the name of the person applying for inspection. Finally, forward it to the Quality and Technical Department. After passing the inspection, return it to the main control unit to proceed to the next step.

[0198] Cooling the preparation vessel:

[0199] To cool down the mixing vessel, click on the corresponding mixing vessel in the central control system, then click on the chilled water supply pneumatic valve of the mixing vessel, and click the "Open" button on the pop-up page; go to the refrigeration room to turn on the refrigeration unit, and observe the temperature of the mixing vessel, which needs to be reduced to -5 to -5℃.

[0200] Stir and add solute:

[0201] Add lithium salt T01. The mixing worker confirms the state of the T01 material, places the finished T01 material barrel on the electronic scale and connects the flange quick connector, zeroes the electronic scale, opens the nitrogen valve and the T01 material barrel valve to pressurize the T01 material barrel, closes the nitrogen valve, opens the feed valve of the mixing kettle, and adds T01. Fill in the T01 barrel number, batch number and quantity, mixing kettle pressure, frequency and start stirring time on the "Production Batching Process Sheet".

[0202] In the central control system, click the start motor of the corresponding mixing vessel. In the pop-up interface, click the start button, then click the frequency control button for the stirring motor. In the pop-up interface, set the frequency to 40Hz to start the stirring motor. Ensure the stirring motor indicator above the mixing vessel is green. After completing the solvent mixing operation, record the stirring frequency, pressure, and stirring time on the "Production Batching Process Sheet".

[0203] In the "Add T01 Electrolyte" field, fill in the corresponding inspection date, time, completion time, required testing items, and the person submitting the application. Then, forward it to the Quality and Technical Department. After passing the inspection, return it to the main control unit to proceed to the next step.

[0204] Add additives by stirring:

[0205] Additive feeding is divided into feeding of two types of additives, i.e., solid and liquid additives; for liquid feeding (combining manual and automatic feeding), the automatic additive feeding is realized by inputting the corresponding additive amount at the main control, and delivering the additive from the workshop additive tank to the corresponding preparation kettle through a pipeline; in the manual additive feeding, the preparation operator fully opens the feed valve of the preparation kettle below the glove box, adds all the solid additives into the preparation kettle through the feeding pipeline, and completes the feeding work;

[0206] Electrolyte stirring and mixing:

[0207] Click the start motor of the corresponding preparation kettle in the central control system, click the start button on the pop-up interface, click the frequency control button of the stirring motor, set 40Hz on the pop-up interface, and complete the start-up of the stirring motor. Confirm that the stirring motor above the used preparation kettle shows a green light, and after the solvent mixing operation is completed, record the stirring frequency, pressure and stirring time on the "Production Batching Process Sheet".

[0208] Finished product filtration:

[0209] The finished product obtained from the electrolyte stirring and mixing step is filtered to remove impurities.

[0210] Finished product inspection:

[0211] After the finished product is filtered, the finished product inspection is carried out; fill in the corresponding inspection application date, time, completion time, items to be inspected and inspection applicant in the finished electrolyte column, and then transfer to the quality and technical department. After passing the inspection, it indicates that the finished product is completed and qualified.

[0212] Packaging barrel preparation process and product packaging process:

[0213] The automatic filling line is connected with the main control Sunflower software for remote control, and the filling operator clicks the "MES" management system in the operation interface on the display screen according to the production order, and clicks "Create Work Order" in the "MES" system. After a series of filling preparations are completed, the filling can be carried out.

[0214] In the above step of stirring and adding additives, the added lithium battery electrolyte additive is CHB; the addition amount of the lithium battery electrolyte additive in the lithium battery electrolyte is 6 wt%.

[0215] The statistical results of the use conditions of the lithium battery electrolyte additives, lithium battery electrolytes and corresponding batteries in the above examples and comparative examples are shown in Table 2 below;

[0216] Table 2

[0217]

[0218]

[0219] This invention discloses a lithium battery electrolyte additive, an electrolyte containing the additive, and a lithium battery. CHB is selected for optimization to develop an electrolyte overcharge prevention additive with good overcharge protection and minimal degradation of electrochemical performance. The additive is added to the lithium battery electrolyte at a concentration of 5-7 wt% to effectively prevent overcharging. When overcharging occurs, CHB monomers undergo dehydrogenation electropolymerization to form polycyclohexylbenzene and generate hydrogen gas. This increases the battery's internal resistance, preventing thermal runaway and improving the battery's overcharge safety.

[0220] The foregoing description of specific exemplary embodiments of the invention is for illustrative and explanatory purposes. These descriptions are not intended to limit the invention to the precise forms disclosed, and it will be apparent that many changes and variations can be made in accordance with the foregoing teachings. The exemplary embodiments were chosen and described in order to explain the specific principles of the invention and its practical application, thereby enabling those skilled in the art to implement and utilize various different exemplary embodiments of the invention, as well as various different choices and variations. The scope of the invention is intended to be defined by the claims and their equivalents.

Claims

1. A lithium battery electrolyte additive, characterized by, The lithium battery electrolyte additives, by weight, include: 100 parts CHB, 15-20 parts modified diatomaceous earth, 2-3 parts acetylene black, 13-15 parts graphene powder, and 6-8 parts paraffin wax. The lithium battery electrolyte additive is prepared according to the following steps: (1) Weigh each component of the lithium battery electrolyte additive according to the specified ratio; (2) Mix the acetylene black, graphene powder and paraffin obtained in step (1) evenly to obtain a mixture; (3) Mix diatomaceous earth and modification liquid evenly according to the ratio of 1 part by weight of diatomaceous earth to 1.8 to 2.2 parts by weight of modification liquid, ultrasonically grind for 50 to 60 minutes, and spray dry to obtain modified diatomaceous earth; the modification liquid includes, by weight, 3 parts of coupling agent KH-550, 15 to 20 parts of ethylene glycol, 20 to 25 parts of ethanol, and 10 to 15 parts of water; (4) Add CHB and modified diatomaceous earth to the mixture, mix evenly, granulate, and then grind to 1000-1200 mesh to obtain the lithium battery electrolyte additive.

2. The lithium battery electrolyte additive according to claim 1, characterized in that, The lithium battery electrolyte additives, by weight, include: 100 parts CHB, 17-20 parts modified diatomaceous earth, 2.5-3 parts acetylene black, 14-15 parts graphene powder, and 7-8 parts paraffin wax.

3. The lithium battery electrolyte additive according to claim 1, wherein, The lithium battery electrolyte additives, by weight, include: 100 parts CHB, 18-20 parts modified diatomaceous earth, 2.7-3 parts acetylene black, 14.5-15 parts graphene powder, and 7.5-8 parts paraffin wax.

4. The lithium battery electrolyte additive according to claim 1, wherein, In step (3), the modified liquid comprises, by weight, 3 parts of coupling agent KH-550, 18-20 parts of ethylene glycol, 23-25 ​​parts of ethanol, and 12-15 parts of water.

5. The lithium battery electrolyte additive according to claim 1, wherein, In step (3), the diatomaceous earth and the modification liquid are mixed evenly according to the ratio of 1 part by weight of diatomaceous earth to 2.1 to 2.2 parts by weight of modification liquid, ultrasonically ground for 55 to 60 minutes, and spray dried to obtain modified diatomaceous earth.

6. The lithium battery electrolyte additive according to claim 1, wherein, In step (4), CHB and modified diatomaceous earth are added to the mixture, mixed evenly, granulated, and then ground to 1100-1200 mesh to obtain the lithium battery electrolyte additive.

7. A lithium battery electrolyte, characterized by, The lithium battery electrolyte contains the lithium battery electrolyte additive described in any one of claims 1-6.

8. The lithium battery electrolyte according to claim 7, characterized in that, The lithium battery electrolyte also includes lithium hexafluorophosphate, ethylene carbonate, and dimethyl carbonate.

9. A lithium battery electrolyte according to claim 7, characterized in that, The amount of the lithium battery electrolyte additive added is 5-7 wt%.

10. A lithium battery, characterized in that, The lithium battery includes: a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and a lithium battery electrolyte; the lithium battery electrolyte is the lithium battery electrolyte according to any one of claims 7-9.

Citation Information

Patent Citations

  • Surface modification method of nanosilicon dioxide

    CN103013182A

  • Oil absorbent prepared from low grade diatomite and preparation method thereof

    CN103252209A

  • Battery system containing phase change material-containing capsules in interior configuration thereof

    US20060063066A1

  • Graphene, graphene-including layer, electrode, and power storage device