Low yield ratio hot-rolled high-strength bimetallic band saw blade backing steel and its manufacturing method

By controlling the chemical composition and smelting and rolling process, a high-strength bimetallic band saw blade backing steel plate with a low yield strength ratio is produced, which solves the problems of insufficient performance and high cost of existing materials under special working conditions, and realizes high-performance and low-cost saw blade backing material to meet the needs of the high-end market.

CN117107154BActive Publication Date: 2024-10-22ANGANG STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311057427.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-22
Publication Date
2024-10-22
Estimated Expiration
2043-08-22

AI Technical Summary

Technical Problem

Existing bimetallic band saw blade backing materials have insufficient performance under special working conditions, high costs, and are difficult to meet the needs of the high-end market, and rely on imports.

Method used

A hot-rolled high-strength bimetallic band saw blade backing steel with a low yield strength ratio was developed. The chemical composition includes C, Si, Mn, Cr, Mo, Ni, Cu, Al, P, and S, with the V element content controlled to be 0. Through specific smelting and rolling processes, a steel plate with a yield strength of 770-800 MPa, a yield strength ratio of 0.48-0.55, an elongation greater than 10%, and a hardness greater than 420 HV was produced.

Benefits of technology

This invention achieves a saw blade backing material with high strength, high hardness, and good plasticity and toughness, reducing production costs, replacing imported materials, meeting the needs of the high-end market, and bringing significant economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117107154B_ABST
    Figure CN117107154B_ABST
Patent Text Reader

Abstract

The present invention relates to a low yield ratio hot-rolled high-strength bimetallic band saw blade backing material steel and a manufacturing method thereof, wherein the chemical components of the steel are as follows by weight percentage: C 0.28%-0.35%, Si 0.3%-0.35%, Mn 0.8%-1.2%, Cr 3.2%-4.0%, Mo 1.4%-1.8%, Ni 0.4%-0.7%, Cu 0.015%-0.025%, Al 0.04%-0.05%, S≤0.005%, P≤0.005%, and the balance is Fe and unavoidable impurities. The present invention relates to a hot-rolled bimetallic band saw backing material steel plate with a tensile strength of more than 1500MPa and without V element. The hot-rolled bimetallic band saw backing steel plate produced by the present invention has a yield strength of less than 800MPa, a yield strength ratio of less than 55%, an elongation of more than 10%, and a hardness of more than 420HV, that is, it has high strength and hardness, good plasticity and toughness, and reduces costs. Due to its better performance and lower cost, the present invention can completely replace imported bimetallic saw blade backing steel, greatly meet the domestic market demand for it, and its successful development will bring huge economic benefits.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of production of steel for saw blade backing materials, and in particular to a low yield strength specific hot-rolled high-strength bimetallic band saw blade backing material steel. Background Art

[0002] With the rapid development of my country's manufacturing and mechanical processing industries, the variety and quantity of raw materials, especially sawing materials, have increased dramatically. The industry is increasingly demanding large-scale, fast and high-precision sawing. This requires sawing tools to be efficient, stable, highly wear-resistant, long-life and low-cost.

[0003] There are two common sawing methods: circular saw and band saw. Band saw uses saw blades and band saw machines, which are suitable for continuous sawing of almost all types of metals, such as structural steel, weathering steel, alloy steel, bearing steel, stainless steel, heat-resistant steel, aluminum alloy, mold steel, etc. Band saw machines and band saw blades were born in the 1930s and were invented by the American Durr Company. Its function is to use a ring saw blade on the main and driven wheels of the band saw machine to cut metal. Initially, carbon tool steel with the same material as the tooth tip and saw back was used for cutting. The production efficiency was low, the tooth tip was prone to tooth jumping or insufficient wear resistance, and the metal materials that could be cut were very limited. After years of research, Durr successfully used alloy tool steel for cutting in the 1960s. This was an important step forward in the development of band saw blades and provided preliminary preparations for the birth of bimetallic band saw blades. Subsequently, Durr developed the world's earliest bimetallic band saw blade in 1964. The birth of bimetallic saw blades has created a new era in the cutting tool industry. It is made by welding high-speed steel and alloy steel, and is manufactured through a series of machining, heat treatment and other processes, successfully solving the problems of insufficient wear resistance of tooth tips and low sawing efficiency. It has the advantages of energy saving, high efficiency, sharpness and wide application, making it have obvious advantages over traditional circular saws and bow saws in terms of energy saving, environmental protection and cutting efficiency, which has quickly replaced the traditional band saw blade cutting method.

[0004] With the recovery of the global economy and the vigorous development of infrastructure in developing countries, the demand for bimetallic band saw blade cutting tools in the basic manufacturing industry will become increasingly greater. Since the beginning of the 21st century, the market demand for sawing industry in my country has developed rapidly, and the market demand for bimetallic band saw blades has grown at an annual rate of 20%. The future market development space for bimetallic saw blades will also be broader.

[0005] Bimetallic saw blades are made of a composite of backing material and tooth material, where the backing material is made of high-strength, high-toughness and high-fatigue-resistance steel. The backing material is made of a material with a lower yield strength ratio, which can be processed more easily and reduce costs. In order to ensure the high hardness, high wear resistance and high red hardness of the tooth material, the backing can only be applied to the heat treatment process parameters of the tooth. Therefore, the research and development of the backing material has always been an important topic in the evolution and development of bimetallic saw blades. With the development of the manufacturing industry, more and more difficult-to-saw materials are applied to production, and the backing material of bimetallic band saw blades has also undergone a series of changes. From the initial spring steel to high-strength and high-to-ultra-high-strength steel, as well as the special steel for bimetallic band saw blades developed by some researchers at home and abroad in recent years.

[0006] 65Mn steel is the most commonly used spring steel as back material, with a C content in the range of 0.62-0.7% and a Mn content in the range of 0.9-1.2%. After appropriate heat treatment (860℃ quenching + 450℃ tempering), the organization of 65Mn steel is tempered troostite, with a hardness of 521HV, a tensile strength of 1574MPa, an elongation of 12%, and a cross-sectional shrinkage of 33%, with good strength and plasticity matching. However, due to the high content of Mn elements, the thermal conductivity of the steel drops sharply, the linear expansion coefficient increases, and it is very easy to form large internal stress during rapid heating or cooling, the cracking tendency after welding increases, and the welding performance is poor. After a period of time, it was replaced by D6A and RM78 high-strength steel.

[0007] The composition of D6A and RM78 high-strength steel is quite different from that of 65Mn spring steel. The specific composition is shown in Table 1. It not only reduces the content of Mn element, but also adds micro-alloying elements, which significantly improves the strength and oxidation resistance of steel. The use of high-strength steel as the back material is of great significance to the sawing industry. It not only increases the service life of the saw blade, but also can be used in harsh working conditions, promoting the development of the manufacturing industry. The saw blade with high-strength steel as the back material is relatively cheap and can adapt to most working conditions, occupying the low-end market.

[0008] In recent years, with the development of high-tech such as aerospace, a large number of high-hardness and high-temperature resistant materials have been applied, which requires bimetallic band saw blades to have better cutting performance. The previous band saw blades cannot or cannot fully meet the use requirements, which requires better backing materials. Ultra-high strength steel RM80 and B318 are used in the backing materials of bimetallic band saw blades. RM80 is an American brand, and B318 is a Voestalpine brand. The two have similar compositions, as shown in Table 1.

[0009] Although the use of ultra-high strength steel as the backing material of bimetallic band saw blades can meet almost all working conditions, it is not competent under some special service environments or requirements. In order to meet special working conditions, some foreign companies are developing special steel for bimetallic band saw blade backing materials. For example, the special steel for the back of the band saw blade developed by Japan's Nissin Steel for Amada does not contain Ni elements, which can prevent the generation of defects such as banded structure and white spots. Another example is RM85 developed by Carpenter Corporation in the United States, which is a special steel for the back of high-Ni band saw blades. The tensile strength reaches 2000MPa, and the elongation is consistent with the existing materials, but its quenching temperature is low, which is not suitable for the high quenching process of tooth materials and is limited. For example, Germany's Bruce Company has also developed special materials BE100, etc., but due to the blockade of information, its specific composition is unknown.

[0010] Although China has been developing bimetallic band saw blade materials for nearly 40 years, high-end products still need to be imported in large quantities. This makes it very necessary to improve my country's independent production and manufacturing of bimetallic band saw blade steel.

[0011] Table 1 Chemical composition of common bimetallic band saw blade back materials (mass fraction / %)

[0012]

[0013]

[0014] Publication No. CN 114351060 A discloses "hot-rolled steel strip and its preparation method and application in bimetallic band saw backing material", Rp0.2≥800MPa, tensile strength≥1200MPa, elongation≥6%. The tensile strength is not high. The main alloy components are: C, Si, Mn, Al, P, S, Cr, Mo, Ni, V, Nb, Cu. The V content is 0.2-0.5%wt, which is relatively high in cost.

[0015] The publication number of CN 104451421 B is "a high-strength and toughness bimetallic band saw blade backing steel and its preparation method". The bimetallic band saw blade backing steel has a tensile strength of more than 1500MPa. To achieve this performance, it is necessary to spheroidize anneal after hot rolling and then cold rolling, which is costly. The main alloy components are: C, Si, Mn, Cr, Ni, Mo, V, Nb, Al. The element contains V 0.3-0.4%wt, which is costly.

[0016] The publication number of CN 109468527 B, "A cold-rolled strip steel for bimetallic saw blade backing material and its manufacturing method", is a product that undergoes soft annealing, pickling, full hydrogen hood annealing, and single-stand reversible cold rolling after hot rolling, which is relatively expensive. The main alloying elements are C, Si, Mn, P, S, Cr, V, Ni, Mo, and Al. Among them, V is 0.3-0.4%wt, which is relatively expensive.

[0017] The publication number of CN 109136746 B is "a kind of steel for bimetallic band saw backing material and its preparation method", with a width of 327mm to 410mm, and the hot-rolled raw material alloy composition is: C, Si, Mn, Cr, Ni, Mo, V, Al, P, S. The V content is 0.3-0.4%wt. The cost is relatively high and all are 410mm narrow strips. The process is cumbersome and the cost is relatively high, with hot rolling followed by annealing, cold rolling, annealing, and cold rolling. Summary of the invention

[0018] The present invention provides a low yield ratio hot-rolled high-strength bimetallic band saw blade backing material steel and a manufacturing method thereof, which produces a hot-rolled bimetallic band saw backing material steel plate with a tensile strength of more than 1500MPa and no V element. The hot-rolled bimetallic band saw backing material steel plate produced by the present invention has a yield strength of less than 800MPa, a yield ratio of less than 55%, an elongation of more than 10%, and a hardness of more than 420HV, that is, it has high strength and hardness, good plasticity and toughness, and reduces costs. Due to its better performance and lower cost, the present invention can completely replace imported bimetallic saw blade backing material steel, greatly solving the domestic market demand for it, and its successful development will bring huge economic benefits.

[0019] In order to achieve the above object, the present invention adopts the following technical solutions:

[0020] A low yield strength ratio hot-rolled high-strength bimetallic band saw blade backing material steel, the chemical composition of the steel is as follows by weight percentage: C 0.28%-0.35%, Si 0.3%-0.35%, Mn 0.8%-1.2%, Cr 3.2%-4.0%, Mo 1.4%-1.8%, Ni 0.4%-0.7%, Cu 0.015%-0.025%, Al 0.04%-0.05%, S≤0.005%, P≤0.005%, and the balance is Fe and unavoidable impurities.

[0021] The steel plate has a yield strength of 770-800 MPa, a tensile strength of 1500-1566 MPa, a yield strength ratio of 0.48-0.55, an elongation greater than 10%, and a hardness of 420-451 HV.

[0022] The steel plate has a thickness of 1.0 to 12 mm and a width of 600 to 1550 mm. The steel plate structure is pearlite + bainite + martensite + residual austenite, and the thickness of the double-sided decarburized layer of the steel plate accounts for 1.8% to 2.0%.

[0023] The following is a detailed description of the mechanism of action of each alloy component of the structural steel of the present invention, wherein the percentage symbol % represents weight percentage:

[0024] C: 0.28% ≤ C ≤ 0.35%; Carbon is the basic element of steel. The most basic strengthening element to ensure that the steel strip has high strength, high hardness, high wear resistance, and good plasticity and toughness.

[0025] Si: 0.3%≤Si≤0.35%; Silicon is one of the common elements in steel, which helps the plasticity and toughness of steel and has a deoxidizing effect.

[0026] Mn: 0.8% ≤ Mn ≤ 1.2%; Manganese is one of the common elements in steel, which improves hardenability and has a solid solution strengthening effect. If the content is too high, the toughness of the steel will decrease.

[0027] Cr: 3.2% ≤ Cr ≤ 4.0%; Chromium improves the strength, hardness, high-temperature mechanical properties and hardenability of steel, improves the corrosion resistance and oxidation resistance of steel, and reduces plasticity and toughness.

[0028] Mo: 1.4% ≤ Mo ≤ 1.8%; Molybdenum is a strong carbide-forming element that can improve the hardenability, toughness and corrosion resistance of steel, and can also improve the tempering stability of steel.

[0029] Ni: 0.4%≤Ni≤0.7%; Nickel is a non-carbide forming element, which can be dissolved in steel to improve the toughness and hardenability of steel, inhibit the dissolution of carbides, hinder the growth of original austenite grains, and improve the thermal stability of steel.

[0030] Cu: 0.015% ≤ Cu ≤ 0.025%; Copper can improve the strength and toughness of steel and improve its weather resistance; but it will cause copper brittleness, and more than 0.5% will significantly reduce plasticity.

[0031] S: S≤0.005% or less; sulfur is a harmful element in steel, and the sulfide inclusions produced seriously affect the mechanical properties of steel. In the present invention, its content is reduced as much as possible and controlled to be below 0.005%.

[0032] P: P≤0.005%; although phosphorus can play a role in solid solution strengthening and significantly improve the corrosion resistance, it is easy to segregate at the grain boundary when the content is too high, thereby reducing the welding performance, plasticity and toughness of the steel plate. In the steel of the present invention, phosphorus is controlled below 0.017%.

[0033] Al: 0.04% ≤ Al ≤ 0.05%; Aluminum: Aluminum in steel mainly has the functions of deoxidation and nitrogen fixation; it refines grains, improves the toughness of steel at low temperatures, and can also reduce the brittle transition temperature of steel.

[0034] A method for manufacturing low yield ratio hot-rolled high-strength bimetallic band saw blade backing steel, comprising the following method:

[0035] The steel plate of the present invention is prepared by molten iron through converter smelting, LF refining, RH or VD refining to obtain molten steel, which is then continuously cast into a slab.

[0036] 1) LF: Add lime and alumina balls to make slag, and take appropriate amount of fluorite to adjust the fluidity of slag. Use calcium powder, fine carbon powder and aluminum powder for diffusion deoxidation to maintain the reduced slag. The minimum vacuum degree of RH is 80-100Pa, and the holding time is 15-20min to control the hydrogen content. Complete alloying and control all components to meet the requirements. Al is controlled at 0.04%-0.05%, and silicon calcium wire is added to control the morphology of inclusions. Silica argon is blown for more than 30-40 minutes. At the same time, it is strictly forbidden to expose the molten steel to avoid oxidation of the molten steel.

[0037] 2) Ingot treatment process: control the superheat, superheat 20 ~ 30 ℃, pull speed 0.8 ~ 1.4m / min, crystallizer water flow 80L / min ~ 160L / min, secondary cooling water volume 0.20 ~ 0.25L / kg, electromagnetic stirring current 350 ~ 450A, frequency 2.2 ~ 2.9Hz, automatic liquid level control, use special crystallizer protection slag. The tundish is argon-blown throughout the process, the baking time is ≥ 4 hours, the continuous casting ingot is placed in the insulation pit, with red steel substrate, and the insulation time is 30 ~ 40h; the steel slab is heated to 1150 ~ 1250 ℃ and then hot-rolled;

[0038] 3) Rolling process: Rough rolling is carried out after dephosphorization with high-pressure water, the rough rolling temperature is 1100-1200℃, and finish rolling is carried out after dephosphorization again, the finishing temperature is 850-980℃; the strip thickness fluctuates by 0.06-0.10mm, the convexity is 60-100μm, the tensile strength difference of the same coil is 10-50MPa, and the hardness difference of the same coil is 10-30HV.

[0039] 4) Cooling process: After final rolling, laminar cooling is performed to 730-790°C for coiling, and then slow cooling is performed at 650-700°C for 72-76 hours.

[0040] Compared with the prior art, the present invention has the following beneficial effects:

[0041] The present invention does not contain V, has low yield strength, low yield strength ratio, and is easy to process. The hot-rolled bimetallic band saw backing steel plate produced by the present invention has a yield strength of 770-800MPa, a yield strength ratio of 0.48-0.55, an elongation greater than 10%, a hardness greater than 420HV, and a double-sided decarburization layer depth of less than 2%, that is, it has high strength and hardness, good plasticity and toughness, and reduces costs. Due to its better performance and lower cost, the present invention can completely replace imported bimetallic saw blade backing steel, greatly solving the domestic market demand for it, and its successful development will bring huge economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 1 is a metallographic diagram showing that the structure of the steel plate according to Embodiment 1 of the present invention is pearlite+bainite+martensite+retained austenite. DETAILED DESCRIPTION

[0043] The specific implementation mode of the present invention will be further described below in conjunction with embodiments:

[0044] The chemical composition of the steel grades of the embodiment is shown in Table 2; the production process of the embodiment is shown in Table 3; and the performance of the product of the embodiment is shown in Table 4.

[0045] Table 2 Chemical composition, %

[0046] serial number C Si Mn Cr Ni Mo Cu S P Al 1 0.31 0.32 1.01 3.69 0.55 1.67 0.019 ≤0.005 ≤0.005 0.046 2 0.35 0.31 0.99 3.58 0.52 1.59 0.017 ≤0.005 ≤0.005 0.045 3 0.34 0.35 1.12 3.71 0.57 1.63 0.021 ≤0.005 ≤0.005 0.049 4 0.35 0.33 1.10 3.57 0.53 1.49 0.020 ≤0.005 ≤0.005 0.044 5 0.31 0.34 1.02 3.55 0.51 1.77 0.018 ≤0.005 ≤0.005 0.050 6 0.33 0.31 1.06 3.70 0.56 1.77 0.018 ≤0.005 ≤0.005 0.047 7 0.32 0.35 1.10 3.59 0.55 1.62 0.021 ≤0.005 ≤0.005 0.044 8 0.33 0.33 1.12 3.66 0.53 1.66 0.021 ≤0.005 ≤0.005 0.042

[0047] Table 3 Production process

[0048]

[0049] Table 4 Steel plate properties

[0050]

Claims

1. A low yield ratio hot-rolled high-strength bimetallic band saw blade backing steel, characterized in that: The chemical composition of the steel is calculated by weight percentage: C 0.28%~0.35%, Si 0.3%~0.35%, Mn 0.8%~1.2%, Cr 3.2%~4.0%, Mo 1.4%~1.8%, Ni 0.4%~0.57%, Cu 0.015%~0.025%, Al 0.04%~0.05%, S≤0.005%, P≤0.005%, the balance is Fe and unavoidable impurities; The yield strength of the steel plate is 770-800 MPa, the tensile strength is 1500-1566 MPa, the yield strength ratio is 0.48-0.55, the elongation is greater than 10%, and the hardness is 420-451 HV; The manufacturing method of low yield ratio hot-rolled high-strength bimetallic band saw blade backing steel, the steel plate is obtained by molten iron through converter smelting, LF refining, RH or VD refining, and continuous casting into slabs, specifically including the following methods: 1) RH minimum vacuum degree is 80-100Pa, holding time is 15-20min, Al is controlled at 0.04%-0.05%, and argon is blown statically for 30-40 minutes; 2) Ingot treatment process: control the superheat, the superheat is 20-30℃, the pulling speed is 0.8-1.4m / min, the tundish is blown with argon throughout the process, the baking time is ≥4 hours, the continuous casting ingot is placed in the insulation pit, and the insulation time is 30-40h; the steel slab is heated at 1150-1154℃ and then hot rolled; 3) Rolling process: Rough rolling temperature is 1100-1200℃, finishing rolling temperature is 951-980℃; 4) Cooling process: After final rolling, laminar cooling is performed to 730-790℃ for coiling, and then slow cooling is performed at 650℃-700℃ for 72-76 hours after coiling.

2. The low yield ratio hot-rolled high-strength bimetallic band saw blade backing steel according to claim 1, characterized in that: The structure of the steel plate is pearlite + bainite + martensite + retained austenite, and the thickness of the decarburized layer on both sides of the steel plate accounts for 1.8% to 2.0%.

3. The low yield ratio hot-rolled high-strength bimetallic band saw blade backing steel according to claim 1, characterized in that: The steel plate thickness is 1.0~12mm and the width is 600~1550mm.

4. A method for manufacturing a low yield ratio hot-rolled high-strength bimetallic band saw blade backing material steel as claimed in any one of claims 1 to 3, wherein the steel plate is obtained by molten iron through converter smelting, LF refining, RH or VD refining, and the molten steel is continuously cast into a slab, characterized in that: The specific methods include the following: 1) RH minimum vacuum degree is 80-100Pa, holding time is 15-20min, Al is controlled at 0.04%-0.05%, and argon is blown statically for 30-40 minutes; 2) Ingot treatment process: control the superheat, the superheat is 20-30℃, the pulling speed is 0.8-1.4m / min, the tundish is blown with argon throughout the process, the baking time is ≥4 hours, the continuous casting ingot is placed in the insulation pit, and the insulation time is 30-40h; the steel slab is heated at 1150-1154℃ and then hot rolled; 3) Rolling process: Rough rolling temperature is 1100-1200℃, finishing rolling temperature is 951-980℃; 4) Cooling process: After final rolling, laminar cooling is performed to 730-790℃ for coiling, and then slow cooling is performed at 650℃-700℃ for 72-76 hours after coiling.

5. The method for manufacturing a low yield ratio hot-rolled high-strength bimetallic band saw blade backing steel according to claim 4, characterized in that: LF adds lime and alumina balls to make slag, and uses fluorite to adjust the fluidity of the slag; calcium powder, carbon powder and aluminum powder are used for diffusion deoxidation to maintain the reduced slag.

6. The method for manufacturing a low yield ratio hot-rolled high-strength bimetallic band saw blade backing steel according to claim 4, characterized in that: RH adds silicon-calcium wire to control the morphology of inclusions.

7. The method for manufacturing a low yield ratio hot-rolled high-strength bimetallic band saw blade backing steel according to claim 4, characterized in that: In step 2), the water flow rate of the continuous casting crystallizer is 80-160 L / min, the secondary cooling water volume is 0.20-0.25 L / kg, the electromagnetic stirring current is 350-450 A, and the frequency is 2.2-2.9 Hz.