A microalloyed, high-strength and high-toughness, high-surface-quality weathering steel and a production method thereof
By adjusting the chemical composition and smelting process of weathering steel, the problems of insufficient strength, toughness and surface quality of weathering steel are solved, achieving higher strength, toughness and purity, reducing surface defects and production costs, and improving the overall performance of weathering steel. and service life.
Patent Information
- Application Number
- CN202311166295.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-08
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-09-08
AI Technical Summary
Existing weathering steel has deficiencies in strength, toughness and surface quality, especially poor strength and toughness and prone to cracks on the surface, which affects its safety in use. At the same time, the added elements such as P and Cu increase production costs.
By adjusting the chemical composition, increasing the content of C, Si, Mn, Cr, Cu, Ni, V, Al and other elements, and using specific smelting and rolling processes, we can prepare weathering steel with microalloying, high strength, toughness, and high surface quality. , control the content of P, S and other elements, and use processes such as KR desulfurization, converter smelting, LF refining, continuous casting and temperature-controlled rolling to ensure the high strength and purity of the steel.
The strength, toughness, purity and service life of weathering steel have been improved. The hot-rolled performance reaches Rm: 550-580MPa, Rel: 370-400MPa, KV2 (0℃): 70-150J, and the level of non-metallic inclusions is reduced. Surface defects are reduced, significantly improving the overall performance and service life of steel.
Smart Images

Figure GDA0004893745930000061 
Figure GDA0004893745930000071 
Figure GDA0004893745930000082
Abstract
Description
Technical Field
[0001] The present invention relates to weathering steel in the steel industry, and more particularly to a micro-alloyed, high-strength and high-toughness, high-surface-quality weathering steel and a production method thereof. Background Art
[0002] Weathering steel is atmospheric corrosion resistant steel. It is a low alloy steel between ordinary steel and stainless steel. Weathering steel is generally made of ordinary low alloy steel with a small amount of corrosion resistant elements such as copper and nickel added. It has excellent strength, toughness, plasticity, forming, welding, abrasion, high temperature and fatigue resistance. Weathering steel's atmospheric corrosion resistance is 2-8 times that of ordinary steel, and its paintability is 1.5-10 times that of ordinary steel. At the same time, weathering steel also has the characteristics of rust resistance, corrosion resistance and life extension, energy saving and consumption reduction. Weathering steel is mainly used for steel structures such as railways, vehicles, bridges, towers, photovoltaic power generation, high-speed projects, boilers, etc. that are exposed to the atmosphere for a long time. It is also used to manufacture containers, railway vehicles, oil derricks, port buildings, oil production platforms and containers containing hydrogen sulfide corrosive media in petrochemical equipment.
[0003] At present, the national standard "Weathering Structural Steel" (GB / T 4171-2008) stipulates the following for Q355GNH steel: C≤0.12%, Si: 0.20%-0.75%, Mn≤1.00%, P: 0.07%-0.15%, S≤0.020%, Cu: 0.25%-0.55%, Cr: 0.30%-1.25%, Ni≤0.65%. Hot rolled state performance: Rm: 490MPa-630MPa, ReL≥355MPa, A≥22%, KV2(0℃)≥34J; 180° bending test is qualified; non-metallic inclusions Class A≤2.5, Class B≤2.0, Class C≤2.5, Class D≤2.0, Ds≤2.0. At present, the hot-rolled mechanical properties of Ф56mm-Ф70mm Q355GNH weathering steel can reach Rm: 520-530MPa, Rel: 335-360MPa, A: 22-26%, KV2 (0℃): 40-60J; non-metallic inclusions of Class A ≤ 2.5, Class B ≤ 2.0, Class C ≤ 2.0, Class D ≤ 2.0, Ds ≤ 2.0. However, this kind of weathering steel has poor toughness and is prone to cracks on the surface, which affects its safety in use.
[0004] Existing weathering steels are prone to surface defects due to the addition of elements such as P and Cu, which increases subsequent production costs. Therefore, it is necessary to develop a new micro-alloyed, high-strength and high-toughness, high-surface quality weathering steel with independent intellectual property rights, and use micro-alloy elements to improve the performance of the steel. Summary of the invention
[0005] In view of the shortcomings of the prior art, the technical problem to be solved by the present invention is to provide a micro-alloyed, high-strength and high-toughness, high-surface quality weathering steel, and at the same time provide a production method of such steel. The final product has higher strength and toughness, purity and service life than the Q355GNH steel in the "Weathering Resistant Structural Steel" (GB / T 4171-2008) standard.
[0006] The present invention is achieved through the following technical solutions:
[0007] A microalloyed weathering steel with high strength and toughness and high surface quality, the chemical composition mass percentage of which is: C: 0.09%-0.12%, Si: 0.50%-0.60%, Mn: 1.03%-1.10%, P: 0.070%-0.150%, S≤0.003%, Cr: 0.50%-0.60%, V: 0.03%-0.06%, Cu: 0.25%-0.30%, Ni: 0.20%-0.30%, Al: 0.040%-0.060%, [O]≤0.0015%, and the balance is Fe.
[0008] A further technical solution of the present application: the chemical composition by mass percentage is: C: 0.11%, Si: 0.55%, Mn: 1.08%, P: 0.124%, S: 0.002%, Cr: 0.56%, V: 0.05%, Cu: 0.28%, Ni: 0.25%, Al: 0.050%, [O]: 0.0009%, and the balance is Fe.
[0009] The reasons for limiting the chemical composition of the microalloyed, high-toughness, high-surface-quality weathering steel of the present invention are described in detail below:
[0010] C is one of the most effective elements for improving strength. To ensure the strength of weathering steel, the C content is controlled according to the upper limit on the existing Q355GNH, and the C content is limited to between 0.09% and 0.12%.
[0011] Si has a deoxidizing effect in steel and can dissolve in ferrite and austenite to increase the strength and hardness of steel, especially the yield strength of steel. To ensure the strength of steel, the Si content of weathering steel is controlled between 0.50% and 0.60%.
[0012] Mn can improve the hardness and wear resistance of steel, improve the hardenability of steel, and improve the hot working performance of steel. Mn also has the effect of solid solution strengthening, which can expand the austenite zone, reduce the transformation temperature of austenite to ferrite, and then refine the ferrite grains, improve the toughness of steel, and compensate for the strength loss caused by low carbon. However, too high Mn content will cause segregation. Therefore, the Mn content is controlled at an upper limit of 1.03%-1.10% based on Q355GNH;
[0013] P is generally a harmful element in steel. P makes steel cold brittle, reduces the impact toughness of steel, and deteriorates the welding performance of steel, reduces plasticity, and makes the cold bending performance worse. However, in the present invention, P and Cu need to react with each other to improve the atmospheric corrosion resistance of steel. Therefore, the present invention controls the P content to a lower limit of 0.070%-0.150%;
[0014] S is an element that is easy to segregate, reducing the ductility and toughness of steel, and also has an adverse effect on welding performance and corrosion resistance. Therefore, the present invention strictly controls the S content, which must be ≤0.003%;
[0015] Cr can significantly improve the strength, hardness, wear resistance and hardenability of steel, but at the same time reduce plasticity and toughness. It can also form a passivation film on the steel surface, which has the ability to resist oxidation and corrosion. At the same time, Cr can improve the resistance to carbon dioxide corrosion. In this invention, considering the matching of strength and toughness, the Cr element is controlled between 0.50% and 0.60%;
[0016] The addition of V element can refine the grains, improve the toughness and wear resistance of steel, and thus improve the comprehensive mechanical properties and fatigue life of hot-rolled steel. However, V element is very expensive and is not suitable for large-scale addition. The V content of this steel is controlled at 0.03%-0.06%.
[0017] Cu is generally a harmful element in steel. When the Cu content exceeds 0.20% and the steel temperature exceeds 1100°C, oxidation decarburization occurs on the steel surface, which is easily enriched at the grain boundary of the decarburized layer, resulting in copper brittleness and surface cracking, which seriously affects the quality of the steel. However, the present invention needs to add Cu element to improve the weather resistance of steel, so the present invention controls the Cu content to 0.25%-0.30%.
[0018] Ni can improve the strength of steel while maintaining good plasticity and toughness. More than 0.20% nickel has corrosion resistance to acids and alkalis. Nickel improves the hardenability of steel by lowering the critical transition temperature and the diffusion rate of each element. It has rust prevention and heat resistance at high temperatures. When Ni:Cu>0.8, adding Ni can inhibit the crack tendency caused by Cu elements, but since nickel is a scarce resource, it is expensive. Therefore, 0.20%-0.30% Ni is added to this steel.
[0019] Al is a strong reducing element and is often used as a deoxidizer in steel. When the Al content is greater than 0.015%, as the Al content increases, it also plays a role in refining grains in the steel. In order to ensure the toughness of weathering steel, the present invention limits the Al content to 0.040%-0.060%.
[0020] O: It has little effect on the strength of steel at room temperature, but significantly reduces the elongation and area reduction of steel. At lower temperatures and when the O content is extremely low, the strength and plasticity of the material decrease sharply with the increase of the O content. In terms of impact performance, as the O content increases, the maximum impact value gradually decreases, but the brittle transition temperature increases rapidly, and the range of the brittle transition temperature also becomes wider. At the same time, as the O content increases, the probability of the appearance of oxide inclusions in the material increases greatly, thereby reducing the fatigue life of the material. The present invention and production process can stably control the O content within 0.0015%.
[0021] A method for producing microalloyed, high-strength and high-toughness weathering steel with high surface quality, wherein the smelting raw materials are sequentially subjected to the following steps: (1) raw material selection: selecting high-P molten iron with a P content of 0.08% to 0.12% for smelting;
[0022] (2) KR desulfurization: After removing the blast furnace slag, insert the stirring head into the molten iron to stir it, so that the molten iron forms a vortex, and add desulfurizer to the center of the vortex. Then, remove the desulfurization products by multiple slag removal to ensure that the S content of the molten iron after desulfurization is ≤0.005%;
[0023] (3) Converter smelting: smelting in a top-bottom double-blown converter of more than 90 tons, using 90% desulfurized hot metal + 10% scrap steel as raw materials for primary smelting; adding aluminum cake for pre-deoxidation at the beginning of steel tapping, adding ferrosilicon, ferromanganese, and low-carbon ferrochrome alloy for initial composition adjustment after 30% of steel tapping, and then adding lime and synthetic refined slag; using slag cones and slide plates for composite slag blocking at the end of steel tapping to ensure slag-free steel tapping and prevent molten steel from returning to P;
[0024] (4) Refining: Deep deoxidation and alloying of molten steel are carried out in LF furnaces above 90 tons. Lime and refining slag are added to each furnace to ensure that the final slag basicity R is 5.0-8.0; nickel plates, copper blocks, ferrovanadium and ferrophosphorus are added in the early stage of refining for alloy fine adjustment; stirring is carried out throughout the refining process. Strong stirring is used in the early stage of refining to enhance desulfurization and remove inclusions through steel slag reaction; weak stirring is used in the later stage of refining to prevent secondary oxidation of molten steel;
[0025] (5) Inclusion modification and soft blowing: After refining, calcium silicon wire is added immediately for soft blowing to modify the inclusions and ensure that the inclusions are fully floated and removed;
[0026] (6) Continuous casting: The billet continuous casting machine is used for casting, and carbon-free tundish covering agent and peritectic steel mold protection slag are used to implement full-process and full-protection casting to produce continuous casting billets; the M-EMS+F-EMS two-stage electromagnetic stirring device is used to fully and evenly organize the structure and improve the internal quality of the billet;
[0027] (7) Heating: A regenerative step-beam heating furnace is used for heating. The heating temperature deviation is controlled within ±10°C, and the temperature of the soaking section is 1080°C-1100°C.
[0028] (8) Rolling: 14 continuous rolling mills are used for temperature-controlled rolling, and the starting rolling temperature is controlled at 1030℃-1050℃.
[0029] (9) Finishing: Shot blasting + manual inspection and grinding are used to check and eliminate defects one by one to ensure the surface quality of the steel.
[0030] A further improvement of the present invention is that in step 2, the desulfurizer is added in 2-3 times at a weight of 500-900 kg, the mixing head is inserted 1 m below the molten iron surface, and stirring is performed at 80-90 r / min.
[0031] A further improvement of the present invention is that in step 4, 200 kg of lime and 400 kg of refined slag are added to each furnace.
[0032] A further improvement of the present invention is that in step 4, strong stirring of 500-550 NL / min is used in the early stage of refining, and weak stirring of 100-150 NL / min is used in the later stage of refining.
[0033] A further improvement of the present invention is that in step 5, the added calcium silicon wire is 70m-120m, and the soft blowing time is controlled to be 25-35 minutes.
[0034] A further improvement of the present invention is that in step 7, the heating time is controlled within a range of 120 min to 150 min.
[0035] Compared with the prior art, the present invention has the following beneficial effects:
[0036] (1) The present invention uses alloying elements such as C, Si, Mn, Cr, Cu, Ni, and P for alloying, adds 0.03%-0.06% of V and 0.040%-0.060% of Al for microalloying, and designs the Mn content to be 1.03%-1.10%. The final product has higher strength, toughness, purity, and service life than the Q355GNH steel in the "Weathering Structural Steel" (GB / T 4171-2008) standard. It has the following properties: hot rolled properties: Rm: 550-580MPa, Rel: 370-400MPa, A: 26-28%, KV2 (0℃): 70-150J; non-metallic inclusions A coarse ≤ 1.0 level, A fine ≤ 1.0 level, B coarse ≤ 0.5 level, B fine ≤ 0.5 level, C coarse ≤ 0.5 level, C fine ≤ 0.5 level, D coarse ≤ 1.0 level, D fine ≤ 1.0 level, Ds ≤ 0.5 level. Austenite grain size ≥ 7.5 level, surface defect depth is not more than 0.1mm.
[0037] (2) The steel grade of the present invention limits the S content to ≤ 0.003%, which effectively reduces stress corrosion caused by sulfides.
[0038] (3) The steel of the present invention is smelted with high P molten iron having a P content of 0.08%-0.12%, and the P is slightly removed in the converter. The P element is adjusted as much as possible by using the residual P in the steel, and the use of P iron to adjust the chemical composition is reduced, which affects the purity of the steel.
[0039] (4) According to the characteristics of the steel grade, a desulfurizer is used for KR pre-desulfurization to ensure that the S content of the molten iron after desulfurization is ≤0.005%, creating favorable conditions for refining and desulfurization. The refining process is stirred throughout, and strong stirring is performed in the early stage of refining to enhance desulfurization through slag reaction.
[0040] (5) After refining, feed 70m-120m silicon calcium wire for soft blowing immediately to denature the inclusions. The soft blowing time is 25-35 minutes to ensure that the inclusions are fully floated and removed.
[0041] (6) The continuous casting adopts the M-EMS+F-EMS three-stage electromagnetic stirring device to fully homogenize the structure and improve the internal quality.
[0042] (7) Medium temperature controlled rolling is adopted, the starting rolling temperature is controlled at 1030℃-1050℃, and 14 continuous rolling mills are used for temperature controlled rolling to avoid surface cracks. DETAILED DESCRIPTION
[0043] The present application is further described in detail below in conjunction with the table. It is necessary to point out that the following specific implementation methods are only used to further illustrate the present application and cannot be understood as limiting the scope of protection of the present application. Technical personnel in this field can make some non-essential improvements and adjustments to the present application based on the above application content.
[0044] The chemical composition comparison between the Q355GNH currently used in China and the present invention is shown in Table 1 below.
[0045] Table 1 Chemical composition comparison wt%
[0046]
[0047] The following production process is used for preparation:
[0048] (1) Raw material selection: Use high-P molten iron with a P content of 0.08%-0.12% for smelting, and use the residual P in the steel to adjust the P element.
[0049] (2) KR desulfurization: remove the blast furnace slag, adopt the KR desulfurization method, insert the stirring head into the molten iron for stirring, insert the stirring head 1m below the liquid surface of the molten iron, stir at 80-90r / min, make the molten iron form a vortex, add 500-900kg of desulfurizer into the center of the vortex 2-3 times, make the desulfurizer gradually react with the sulfur in the molten iron, make the sulfur in the molten iron enter the slag, then remove the desulfurization product by multiple slag removal, reduce the sulfur content of the molten iron, and ensure that the sulfur content of the molten iron after desulfurization is ≤0.005%;
[0050] (3) Converter smelting: smelting in a top-bottom double-blown converter of more than 90 tons, using 90% desulfurized hot metal + 10% scrap steel as raw materials for primary smelting; adding aluminum cake for pre-deoxidation at the beginning of steel tapping, adding ferrosilicon, ferromanganese, low-carbon ferrochrome and other alloys for initial composition adjustment after 30% of steel tapping, followed by adding lime and synthetic refined slag; using slag cones and slide plates for composite slag blocking at the end of steel tapping to ensure slag-free steel tapping and prevent molten steel from returning to P;
[0051] (4) Refining: Deep deoxidation and alloying of molten steel are carried out in LF furnaces of more than 90 tons. 200kg of lime and 400kg of refining slag are added to each furnace to ensure that the final slag basicity R is 5.0-8.0; nickel plates, copper blocks, ferrovanadium and ferrophosphorus are added in the early stage of refining for alloy fine adjustment; stirring is carried out throughout the refining process. In the early stage of refining, strong stirring of 500-550NL / min is used to enhance desulfurization and remove inclusions through slag reaction; weak stirring of 100-150NL / min is used in the later stage of refining to prevent secondary oxidation of molten steel;
[0052] (5) Inclusion denaturation and soft blowing: After refining, add 70m-120m of silicon calcium wire for soft blowing to denature the inclusions. The soft blowing time is 25-35 minutes to ensure that the inclusions are fully floated and removed;
[0053] (6) Continuous casting: square billet continuous casting machine is used for casting, carbon-free tundish covering agent and special crystallizer protection slag for peritectic steel are used, and automatic baking and automatic adding devices for protection slag are used to ensure uniform and timely addition, and full-process and full-protection casting is implemented to produce continuous casting square billets; M-EMS+F-EMS three-stage electromagnetic stirring device is used to fully and evenly organize the structure and improve the internal quality of the billet.
[0054] (7) Heating: A regenerative step-beam heating furnace is used for heating. A fully automatic intelligent combustion system is used for billet heating. The heating temperature deviation is controlled within ±10°C. The temperature of the soaking section is 1080°C-1100°C. The heating time is controlled within 120min-150min.
[0055] (8) Rolling: Medium temperature controlled rolling is adopted, the starting rolling temperature is controlled at 1030℃-1050℃, and 14 continuous rolling mills are used for temperature controlled rolling.
[0056] (9) Finishing: Shot blasting + manual inspection and grinding are used to check and eliminate defects one by one to ensure the surface quality of the steel.
[0057] Table 2 Composition of weathering steel of the present invention by weight%
[0058] chemical composition C Si Mn P S Cr V Cu Ni Al Example 1 0.09 0.50 1.03 0.071 0.001 0.50 0.03 0.25 0.20 0.041 Example 2 0.10 0.53 1.05 0.085 0.002 0.53 0.04 0.26 0.23 0.052 Example 3 0.11 0.55 1.08 0.124 0.002 0.56 0.05 0.28 0.25 0.050 Example 4 0.12 0.60 1.10 0.148 0.003 0.60 0.06 0.30 0.30 0.059
[0059] According to the standard of "Weathering Structural Steel" (GB / T 4171-2008), Examples 1-4 and the prior art were tested, and the results are shown in Tables 3-5.
[0060] Table 3 Comparison of gas content and grain size of the present invention with the prior art
[0061]
[0062]
[0063] Table 4 Comparison of mechanical properties of the present invention with prior art
[0064]
[0065] Table 5 Comparison of non-metallic inclusions of the present invention with prior art
[0066] Steel Type A thick A thin B thick B thin C thick C Thin D thick D Thin Ds Example 1 1.0 1.0 0 / 0 0 0 / 0 0 / 0 1.0 1.0 0 Example 2 0.5 1.0 0 / 0.5 0 0 / 0 0 / 0 1.0 1.0 0 Example 3 0.5 1.0 0 / 0 0 0 / 0 0 / 0 1.0 1.0 0 Example 4 1.0 1.0 0.5 0 0 / 0 0 / 0 1.0 1.0 0 Existing weathering steel 2.0 2.5 1.5 2.0 1.0 1.0 1.0 1.5 2.0
[0067] In the present invention, the inclusions of type A and type D have been stably controlled at level ≤1.0, the inclusions of type B have been stably controlled at level ≤0.5, and the inclusions of type C and Ds have not been detected.
Claims
1. A micro-alloyed, high-strength and high-surface quality weathering steel. Features: The chemical composition by mass percentage is: C: 0.09%-0.12%, Si: 0.50%-0.60%, Mn: 1.03%-1.10%, P: 0.070%-0.150%, S≤0.003%, Cr: 0.50%-0.60%, V: 0.03%-0.06%, Cu: 0.25%-0.30%, Ni: 0.20%-0.30%, Al: 0.040%-0.060%, [O]≤0.0015%, the balance is Fe, Production methods include: (1) Raw material selection: Use high-P molten iron with a P content of 0.08%-0.12% for smelting; (2) KR desulfurization: After removing the blast furnace slag, insert the stirring head into the molten iron to stir it, so that the molten iron forms a vortex, and add desulfurizer to the center of the vortex. Then, remove the desulfurization products by multiple slag removal to ensure that the S of the molten iron after desulfurization is ≤0.005%; (3) Converter smelting: smelting is carried out in a top-bottom double-blown converter of more than 90 tons, with 90% desulfurized hot metal + 10% scrap steel as raw materials for primary smelting; aluminum cake is added for pre-deoxidation at the initial stage of steel tapping, and ferrosilicon, ferromanganese, and low-carbon ferrochrome alloy are added for initial composition adjustment after 30% of the steel is tapped, followed by lime and synthetic refined slag; slag cones and slide plates are used for composite slag blocking at the end of steel tapping to ensure slag-free steel tapping and prevent molten steel from returning to P; (4) Refining: Deep deoxidation and alloying of molten steel are carried out in LF furnaces above 90 tons. Lime and refining slag are added to each furnace to ensure that the final slag basicity R is 5.0-8.0; nickel plates, copper blocks, ferrovanadium and ferrophosphorus are added in the early stage of refining for alloy fine adjustment; stirring is carried out throughout the refining process. Strong stirring is used in the early stage of refining to enhance desulfurization and remove inclusions through slag reaction; weak stirring is used in the later stage of refining to prevent secondary oxidation of molten steel; (5) Inclusion modification and soft blowing: After refining, calcium silicon wire is added immediately for soft blowing to modify the inclusions and ensure that the inclusions are fully floated and removed; (6) Continuous casting: The billet continuous casting machine is used for casting, and carbon-free tundish covering agent and peritectic steel mold protection slag are used to implement full-process and full-protection casting to produce continuous casting billets; the M-EMS+F-EMS two-stage electromagnetic stirring device is used to fully and evenly organize the structure and improve the internal quality of the billet; (7) Heating: Use a regenerative step-beam heating furnace for heating, the heating temperature deviation is controlled within ±10°C, and the temperature of the soaking section is 1080°C-1100°C; (8) Rolling: 14 continuous rolling mills are used for temperature-controlled rolling, and the starting rolling temperature is controlled at 1030℃-1050℃; (9) Finishing: Shot blasting + manual inspection and grinding are used to check and eliminate defects one by one to ensure the surface quality of the steel.
2. A microalloyed, high-toughness, high-surface-quality weathering steel according to claim 1, Features: The chemical composition by mass percentage is: C: 0.11%, Si: 0.55%, Mn: 1.08%, P: 0.124%, S: 0.002%, Cr: 0.56%, V: 0.05%, Cu: 0.28%, Ni: 0.25%, Al: 0.050%, [O]: 0.0009%, and the balance is Fe.
3. A microalloyed, high-toughness, high-surface-quality weathering steel according to claim 1, Features: In the step 2, the desulfurizing agent is added in 2-3 times in an amount of 500-900 kg, the stirring head is inserted 1 m below the molten iron surface, and stirring is performed at 80-90 r / min.
4. A microalloyed, high-toughness, high-surface-quality weathering steel according to claim 1, Features: In step 4, 200 kg of lime and 400 kg of refined slag are added to each furnace.
5. A microalloyed, high-toughness, high-surface-quality weathering steel according to claim 1, It is characterized in that In the step 4, strong stirring of 500-550 NL / min is used in the early stage of refining, and weak stirring of 100-150 NL / min is used in the later stage of refining.
6. A microalloyed, high-toughness, high-surface-quality weathering steel according to claim 1, Features: In step 5, the added calcium silicon wire is 70m-120m, and the soft blowing time is controlled to be 25-35 minutes.
7. A microalloyed, high-toughness, high-surface-quality weathering steel according to claim 1, Features: In step 7, the heating time is controlled within a range of 120 min to 150 min.
Citation Information
Patent Citations
Steel of weatherproof seamless steel tube and manufacturing method of seamless steel tube
CN107699790A
Microalloyed long-life and high-strength and toughness high-speed train plate spring steel and production process thereof
CN111363976A
Super-thick high-toughness weather-proof bridge steel plate and production method thereof
CN111876691A