A method for fabricating an LED chip

By forming grooves on the ITO conductive film using plasma gas etching technology, the problems of complex and costly wet etching operations are solved, achieving the effects of simplified operation and cost reduction.

CN117199212BActive Publication Date: 2026-11-17JIANGXI ZHAO CHI SEMICON CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311322295.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-12
Publication Date
2026-11-17
Estimated Expiration
2043-10-12

AI Technical Summary

Technical Problem

In existing technologies, the roughening of the surface ITO conductive film by wet etching is a complex, cumbersome, and costly process.

Method used

Plasma gas etching technology is used to inject ethanol reactive gas into the plasma chamber and contact it with the ITO conductive film. Through the ionization process, active groups are formed, and the ITO conductive film is etched to form grooves, which replaces the traditional wet etching method.

Benefits of technology

It simplifies the operation process, reduces production costs, and effectively improves the surface roughening effect of ITO conductive film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117199212B_ABST
    Figure CN117199212B_ABST
Patent Text Reader

Abstract

This invention provides a method for fabricating an LED chip, comprising: providing a substrate for growth; growing an epitaxial layer on the substrate; sequentially fabricating a current blocking layer, an ITO conductive film, and a mask blocking layer on the epitaxial layer to form an initial chip; the mask blocking layer is used to divide the surface of the ITO conductive film into an etching region and a masking region; placing the initial chip in a plasma chamber and injecting a reactive gas including ethanol; after an ionization and reaction process, grooves are formed in the etching region to complete surface roughening. After injecting the reactive gas into the plasma chamber, the reactive gas is ionized into active groups through an ionization process, and a chemical reaction occurs directly in the etching region, forming grooves on the ITO conductive film, thereby forming an uneven structure in the ITO conductive film and completing the roughening. This method replaces wet etching, is simple to operate, and only requires gas injection, effectively saving production costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of semiconductor technology, and in particular to a method for preparing an LED chip. Background Technology

[0002] In recent years, with the great progress made in P-type gallium nitride doping technology, gallium nitride-based LEDs, which have excellent characteristics such as fast response, long life, low power consumption, small size and high brightness, have been widely used in LCD displays, full-color displays, traffic displays and other fields.

[0003] Light extraction efficiency has always been a technical challenge that has hindered its development. Currently, the light extraction efficiency of gallium nitride-based LEDs depends on the internal quantum efficiency and the external quantum efficiency. The internal quantum efficiency has been approached to its maximum. However, the external quantum efficiency is easily reduced because the refraction difference between the surface ITO conductive film and the air is large, which can easily lead to full emission at the interface. In other words, there is still room for further improvement in the external quantum efficiency.

[0004] In recent years, some methods have been developed to improve external quantum efficiency by roughening the surface ITO conductive film using post-processing techniques. The principle is to increase the selectivity of light by adding a rough structure to the ITO conductive film, effectively altering the light path and increasing the probability of emission. However, current roughening methods mostly involve wet etching, which is complex, cumbersome, and costly. Summary of the Invention

[0005] In view of the shortcomings of the prior art, the purpose of this invention is to provide a method for preparing LED chips, which aims to solve the technical problems of the complex operation, cumbersome process and high cost of roughening the surface ITO conductive film by wet etching in the prior art.

[0006] To achieve the above objectives, the present invention provides the following technical solution: a method for preparing an LED chip, comprising the following steps:

[0007] Provide a substrate for growth, and grow an epitaxial layer on the substrate;

[0008] A current blocking layer, an ITO conductive film, and a mask blocking layer are sequentially fabricated on the epitaxial layer to form an initial chip. The mask blocking layer is used to divide the surface of the ITO conductive film into an etching area and a masking area.

[0009] The initial chip is placed in a plasma chamber, and a reaction gas including ethanol is injected into the plasma chamber. After the reaction gas undergoes an ionization process and a reaction process with the ITO conductive film, a groove is formed in the etched area of ​​the ITO conductive film to complete the surface roughening.

[0010] The initial chip with roughened surface is then processed into a finished chip.

[0011] Compared with the prior art, the beneficial effects of the present invention are as follows: After the ITO conductive film and the mask barrier layer are fabricated on the epitaxial layer, the surface of the ITO forms the etched area and the mask barrier area due to the shielding of the mask barrier layer. After the reactive gas is injected into the plasma chamber, the reactive gas is ionized into active groups through the ionization process. The active groups directly contact the etched area of ​​the ITO conductive film and undergo a chemical reaction to decompose the ITO conductive film in the etched area, thereby forming grooves on the ITO conductive film. Because the mask barrier layer protects the mask barrier area, the ITO conductive film forms an uneven structure, which is roughened. Gas etching replaces wet etching, and its operation method and process are relatively simple. It only requires gas injection, which effectively saves production costs.

[0012] Furthermore, the step of growing an epitaxial layer on the substrate specifically includes:

[0013] Metal chemical vapor deposition (MCV) is used, with high-purity hydrogen as the carrier gas, high-purity ammonia as the nitrogen source, trimethylgallium and triethylgallium as gallium sources, trimethylindium as the indium source, silane as the N-type dopant, trimethylaluminum as the aluminum source, and magnesium thiocene as the P-type dopant. An N-type semiconductor layer, a multi-quantum-well active layer, and a P-type semiconductor layer are sequentially deposited on the substrate to form an epitaxial layer.

[0014] Furthermore, the doping element of the N-type semiconductor layer is Si, the doping element of the P-type semiconductor layer is Mg, and the doping concentration of Si in the N-type semiconductor layer is 5 × 10⁻⁶. 18 cm -3 ~1×10 19 cm -3 The doping concentration of Mg in the P-type semiconductor layer is 5 × 10⁻⁶. 17 cm -3 ~1×10 20 cm -3 .

[0015] Furthermore, the step of sequentially fabricating a current blocking layer, an ITO conductive film, and a mask blocking layer on the epitaxial layer includes:

[0016] The epitaxial layer is etched to expose a portion of the N-type semiconductor layer;

[0017] A SiO2 layer is deposited on the surface of the etched epitaxial layer, and the SiO2 layer is photolithographically treated to form a current blocking layer.

[0018] An ITO conductive film is deposited on the surface of the epitaxial layer where the current blocking layer is disposed by magnetron sputtering, and then annealed.

[0019] A Ni metal layer is fabricated on the ITO conductive film, and the Ni metal layer is subjected to wet etching to form a mask barrier layer.

[0020] Furthermore, the thickness of the SiO2 layer is 280nm to 320nm, and the thickness of the Ni metal layer is 180nm to 220nm.

[0021] Furthermore, the reaction gas also includes argon.

[0022] Furthermore, the chemical reaction formula for the ionization process is:

[0023] C2H5OH→CH + 3+CH 2+ 2+OH-+2e,

[0024] 2OH-→H2O↑+O - ,

[0025] CH + 3+e→CH * 3;

[0026] The chemical reaction formula for the reaction process is:

[0027] In+3CH * 3→In(CH3)3↑,

[0028] Sn+4CH * 3→Sn(CH3)4↑,

[0029] In+3CH * 3+3O - →In(OCH3)3↓.

[0030] Furthermore, after the step of placing the initial chip in a plasma chamber and injecting a reactive gas into the plasma chamber, whereby the reactive gas undergoes an ionization and reaction process with the ITO conductive film to form grooves in the etched area of ​​the ITO conductive film to complete the surface roughening, the method further includes:

[0031] Cleaning gas is injected into the plasma chamber at preset intervals to remove deposits in the groove.

[0032] Furthermore, the cleaning gas is oxygen, the preset interval is 25S to 35S, and the injection time of the cleaning gas is 8S to 12S.

[0033] Furthermore, the step of preparing the initial chip with roughened surface into a finished chip includes:

[0034] Remove the mask barrier layer on the initial chip after surface roughening;

[0035] Electrodes are fabricated on the initial chip to obtain a staged chip;

[0036] A silicon oxide passivation layer is fabricated on the surface of the chip at the aforementioned stage to obtain the finished chip. Attached Figure Description

[0037] Figure 1 This is a flowchart of the LED chip fabrication method in the first embodiment of the present invention;

[0038] Figure 2 This is a flowchart of the LED chip fabrication method in the second embodiment of the present invention;

[0039] Figure 3 This is a flowchart of the LED chip fabrication method in the third embodiment of the present invention;

[0040] The following detailed description, in conjunction with the accompanying drawings, will further illustrate the present invention. Detailed Implementation

[0041] To facilitate understanding of the present invention, a more complete description will be given below with reference to the accompanying drawings. Several embodiments of the invention are illustrated in the drawings. However, the invention can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete.

[0042] It should be noted that when a component is said to be "fixed to" another component, it can be directly on the other component or there may be an intervening component. When a component is said to be "connected to" another component, it can be directly connected to the other component or there may be an intervening component. The terms "vertical," "horizontal," "left," "right," and similar expressions used in this document are for illustrative purposes only.

[0043] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.

[0044] Please see Figure 1 The LED chip fabrication method in the first embodiment of the present invention includes the following steps:

[0045] S10: Provide a substrate for growth, and grow an epitaxial layer on the substrate;

[0046] In this embodiment, metal chemical vapor deposition is used, with high-purity hydrogen as the carrier gas, high-purity ammonia as the nitrogen source, trimethylgallium and triethylgallium as gallium sources, trimethylindium as the indium source, silane as the N-type dopant, trimethylaluminum as the aluminum source, and magnesium thiocene as the P-type dopant. An N-type semiconductor layer, a multi-quantum-well active layer, and a P-type semiconductor layer are sequentially deposited on the substrate to form an epitaxial layer.

[0047] S20: A current blocking layer, an ITO conductive film, and a mask blocking layer are sequentially fabricated on the epitaxial layer to form an initial chip. The mask blocking layer is used to divide the surface of the ITO conductive film into an etching area and a masking area.

[0048] The current blocking layer is a structure in a semiconductor device used to prevent or limit the transfer of charge between different parts. Generally, the current blocking layer is made of a wide bandgap semiconductor material. The main function of the current blocking layer is to isolate different functional regions and prevent unwanted charge transfer and crosstalk. The ITO conductive film is an N-type oxide semiconductor—indium tin oxide (ITO). After Sn is doped into In₂O₃, the Sn element can replace the In element in the In₂O₃ lattice and exist in the form of SnO₂. Because the In element in In₂O₃ is trivalent, when SnO₂ is formed, it will contribute an electron to the conduction band, and simultaneously generate oxygen holes under certain oxygen-deficient conditions, forming a 1020cm⁻¹ band gap. -3 ~1021cm -3 carrier concentration and 1030 cm 2 / vs~30cm 2 The migration rate is / vs. The mask barrier layer is used to delineate the etching locations of the ITO conductive film, thereby forming a roughened structure.

[0049] S30: The initial chip is placed in a plasma chamber, and a reaction gas including ethanol is injected into the plasma chamber. After the reaction gas and the ITO conductive film undergo an ionization process and a reaction process, a groove is formed in the etched area of ​​the ITO conductive film to complete the surface roughening.

[0050] That is, after the reaction gas including ethanol enters the plasma chamber, it is ionized into active groups after the ionization process. The active groups contact the ITO conductive film. The mask barrier layer protects part of the surface of the ITO conductive film, preventing the active groups from contacting this part of the ITO conductive film. In the etched area where the mask barrier layer is not provided, the active groups directly contact the ITO conductive film, and after the reaction process, the grooves are generated on the ITO conductive film, so that the ITO conductive film forms an uneven structure, completing the surface roughening.

[0051] S40: The initial chip with roughened surface is processed into a finished chip;

[0052] That is, the initial chip after surface roughening is subjected to electrode preparation and other steps to obtain the finished chip.

[0053] After the ITO conductive film and the mask barrier layer are fabricated on the epitaxial layer, the surface of the ITO forms the etched area and the masking area due to the shielding effect of the mask barrier layer. After the reactive gas is injected into the plasma chamber, the reactive gas is ionized into active groups through the ionization process. The active groups directly contact the etched area of ​​the ITO conductive film and undergo a chemical reaction to decompose the ITO conductive film in the etched area, thereby forming grooves on the ITO conductive film. Because the masking area is protected by the mask barrier layer, the ITO conductive film forms an uneven structure, which is roughened. Gas etching replaces wet etching, and its operation method and process are relatively simple. It only requires gas injection, which effectively saves production costs.

[0054] Please see Figure 2 The LED chip fabrication method in the second embodiment of the present invention includes the following steps:

[0055] S110: Provide a substrate for growth, and grow an epitaxial layer on the substrate;

[0056] An epitaxial layer is formed by sequentially depositing an N-type semiconductor layer, a multi-quantum-well active layer, and a P-type semiconductor layer on the substrate. The N-type semiconductor layer is an N-GaN layer, the P-type semiconductor layer is a P-GaN layer, and the multi-quantum-well active layer comprises several alternately stacked quantum well layers and quantum barrier layers, wherein the quantum well layers are InGaN quantum well layers.

[0057] Preferably, the thickness of the N-type semiconductor layer is 1 μm to 3 μm, and the thickness of the P-type semiconductor layer is 200 nm to 300 nm. In this embodiment, the thickness of the N-type semiconductor layer is 2 μm, and the thickness of the P-type semiconductor layer is 260 nm. The doping element of the N-type semiconductor layer is Si, and the Si doping concentration in the N-type semiconductor layer is 5 × 10⁻⁶. 18 cm -3 ~1×10 19 cm -3 The doping element of the P-type semiconductor layer is Mg, and the doping concentration of Mg in the P-type semiconductor layer is 5 × 10⁻⁶. 17 cm -3 ~1×10 20 cm -3 That is, the N-type semiconductor layer is an electron-type semiconductor layer, which is an impurity-type semiconductor layer with a free electron concentration much greater than a hole concentration, and the P-type semiconductor layer is a hole-type semiconductor layer, which is a semiconductor layer in which positively charged holes conduct electricity. The molar ratio of In component in the quantum well layer is 10% to 35%.

[0058] S120: The epitaxial layer is etched to expose a portion of the N-type semiconductor layer;

[0059] The purpose of exposing a portion of the N-type semiconductor layer is to prepare for subsequent electrode fabrication. In this embodiment, the epitaxial layer is etched using ICP etching technology.

[0060] S130: A SiO2 layer is deposited on the surface of the epitaxial layer after etching, and the SiO2 layer is photolithographically treated to form a current blocking layer.

[0061] In this embodiment, the SiO2 layer is deposited using plasma-enhanced chemical vapor deposition (PECVD). Preferably, the thickness of the SiO2 layer is 280 nm to 320 nm; in this embodiment, the thickness is 300 nm. The SiO2 layer undergoes photolithography, i.e., photoresist is coated onto the surface of the SiO2 layer, and after spin coating, exposure, and development, a portion of the SiO2 layer is retained to form the current blocking layer. This current blocking layer corresponds to the position of the electrodes in subsequent fabrication processes.

[0062] S140: An ITO conductive film is deposited on the surface of the epitaxial layer where the current blocking layer is disposed by magnetron sputtering, and then annealed.

[0063] The epitaxial layer with the current blocking layer is placed in a plating bath, and the target material is bombarded by Ar gas ionization, thereby sputtering the target material onto the surface of the epitaxial layer with the current blocking layer, thus forming the ITO conductive film. Since the ITO conductive film itself contains oxygen, a large number of oxygen negative ions are generated during magnetron sputtering. Under the influence of an electric field, these oxygen negative ions bombard the surface of the deposited ITO conductive film with a certain particle energy, causing defects in the crystal structure and crystal state of the ITO conductive film. The higher the sputtering voltage, the greater the energy of the oxygen negative ions bombarding the film surface, thus increasing the probability of defects and making the defects more severe, leading to an increase in the resistivity of the ITO conductive film. In this embodiment, the sputtering voltage of the magnetron sputtering is below -200V, which not only improves the product quality of the ITO conductive film but also reduces the product's production cost.

[0064] However, the ITO conductive film formed by sputtering has poor density. To improve the density, it needs to be annealed. The annealing process can make the crystal arrangement more vaporized, the film layer more dense, and the conductivity more stable.

[0065] Specifically, the epitaxial layer on which the ITO conductive film is deposited is placed in an annealing chamber. The annealing temperature in the annealing chamber is 500°C to 600°C, and the annealing time is 12 to 18 minutes. In this embodiment, the annealing temperature in the annealing chamber is 550°C, and the annealing time is 15 minutes.

[0066] S150: A Ni metal layer is formed on the ITO conductive film, and the Ni metal layer is subjected to wet etching to form a mask barrier layer, thereby forming an initial chip. The mask barrier layer is used to divide the surface of the ITO conductive film into an etching area and a masking area.

[0067] Since the ITO conductive film needs to be etched with gas subsequently, organic photoresist is not suitable for patterning. Therefore, in this embodiment, a Ni metal layer is used. Preferably, the thickness of the Ni metal layer is 180nm to 220nm. In this embodiment, the thickness of the Ni metal layer is 200nm. After the Ni metal layer is fabricated, photoresist is spin-coated onto the surface of the Ni metal layer, and after photolithography, wet etching is performed to change the shape of the Ni metal layer, thereby forming the mask barrier layer. It can be understood that the mask barrier layer covers the ITO conductive film in an intermittent manner, thereby protecting certain areas of the ITO conductive film.

[0068] S160: The initial chip is placed in a plasma chamber, and a reaction gas including ethanol is injected into the plasma chamber. After the reaction gas undergoes an ionization process and a reaction process with the ITO conductive film, a groove is formed in the etched area of ​​the ITO conductive film to complete the surface roughening.

[0069] When the reaction gas including ethanol is injected, the ethanol flow rate is 30 sccm to 100 sccm, the radio frequency power in the plasma chamber is 50 W to 300 W, and the pressure in the plasma chamber is 40 Pa to 100 Pa. In this embodiment, the ethanol flow rate is 70 sccm, the radio frequency power in the plasma chamber is 200 W, and the pressure in the plasma chamber is 60 Pa.

[0070] Specifically, the chemical reaction formula for the ionization process is:

[0071] C2H5OH→CH + 3+CH 2+ 2+OH - +2e,

[0072] 2OH - →H₂O↑+O - ,

[0073] CH + 3+e→CH *3 ;

[0074] The chemical reaction formula for the reaction process is:

[0075] In+3CH * 3→In(CH3)3↑,

[0076] Sn+4CH * 3→Sn(CH3)4↑,

[0077] In+3CH * 3+3O - →In(OCH3)3↓.

[0078] Understandably, CH * 3 and CH + The only difference between the three is their electrical charge, and it can be seen from the chemical reaction formula of the reaction process that both In and Sn elements are vaporized. It should be noted that in this embodiment, by injecting the reactive gas into the plasma chamber, the surface roughening process can be completed after the groove is formed. In some embodiments, the patterned etching of the ITO conductive film can be achieved by adjusting the specific shape of the mask barrier layer after wet etching and increasing the injection dosage of the reactive gas.

[0079] Furthermore, directly reacting the ITO conductive film with ionized ethanol alone results in a slow reaction rate, meaning the surface roughening process is slow, which affects the overall production schedule and prolongs the operation time. Therefore, the reaction gas also includes argon. After argon enters the plasma chamber and is ionized along with the ethanol, it bombards the ITO conductive film, causing the Sn-O and In-O bonds to open rapidly, thereby accelerating the reaction process, effectively improving reaction efficiency, and optimizing the reaction process.

[0080] After the argon gas is introduced, the argon gas is ionized along with the argon gas, and the chemical reaction formula is as follows:

[0081] Ar→Ar + +e,

[0082] At the chemical level, it does not affect the etching effect on the ITO conductive film.

[0083] S170: Remove the mask barrier layer on the initial chip after surface roughening;

[0084] After surface roughening is completed, the mask barrier layer is removed to prevent it from affecting subsequent fabrication processes.

[0085] S180: Electrodes are fabricated on the initial chip to obtain a staged chip;

[0086] The initial chip is placed on the wafer tray of an electron beam evaporation machine. Understandably, the evaporation source emitter is located below the wafer tray. Cr, Al, Ti, Ni, Pt, Ni, Pt and Au layers are deposited sequentially to form the electrode, thereby obtaining the stage chip.

[0087] S190: A silicon oxide passivation layer is formed on the surface of the chip in the aforementioned stage to obtain the finished chip.

[0088] The thickness of the silicon oxide passivation layer is 70nm to 90nm. In this embodiment, the thickness of the silicon oxide passivation layer is 80nm. By setting the silicon oxide passivation layer, a protective layer can be formed on the finished chip to prevent the external environment from corroding the finished chip and thus reducing the yield of the product.

[0089] Please see Figure 3 The LED chip fabrication method in the third embodiment of the present invention includes the following steps:

[0090] S101: Provide a substrate for growth, and grow an epitaxial layer on the substrate;

[0091] S102: The epitaxial layer is etched to expose a portion of the N-type semiconductor layer;

[0092] S103: Deposit a SiO2 layer on the surface of the epitaxial layer after etching, and perform photolithography on the SiO2 layer to form a current blocking layer;

[0093] S104: An ITO conductive film is deposited on the surface of the epitaxial layer where the current blocking layer is disposed by magnetron sputtering, and then annealed.

[0094] S105: A Ni metal layer is formed on the ITO conductive film, and the Ni metal layer is subjected to wet etching to form a mask barrier layer, thereby forming an initial chip. The mask barrier layer is used to divide the surface of the ITO conductive film into an etching area and a masking area.

[0095] S106: The initial chip is placed in a plasma chamber, and a reaction gas including ethanol is injected into the plasma chamber. After the reaction gas undergoes an ionization process and a reaction process with the ITO conductive film, a groove is formed in the etched area of ​​the ITO conductive film to complete the surface roughening.

[0096] S1061: Inject cleaning gas into the plasma chamber at preset intervals to remove deposits in the groove;

[0097] During the reaction, from its chemical reaction: In + 3CH * 3+3O - As can be seen from →In(OCH3)3↓, during the reaction process, the precipitate will also be formed in the groove. The precipitate is a carbon-containing precipitate. In order to better complete the surface roughening process, the cleaning gas is injected to react with the precipitate and remove the precipitate.

[0098] Specifically, the cleaning gas is oxygen, the preset interval is 25S to 35S, and the injection time of the cleaning gas is 8S to 12S. In this embodiment, the preset interval is 30S and the injection time of the cleaning gas is 10S.

[0099] S107: Remove the mask barrier layer on the initial chip after surface roughening;

[0100] S108: Electrodes are fabricated on the initial chip to obtain a staged chip;

[0101] S109: A silicon oxide passivation layer is formed on the surface of the chip in the aforementioned stage to obtain the finished chip.

[0102] In the description of this specification, references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.

[0103] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are specific and detailed, they should not be construed as limiting the scope of the present invention. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these modifications and improvements all fall within the scope of protection of the present invention. Therefore, the scope of protection of this patent should be determined by the appended claims.

Claims

1. A method for fabricating an LED chip, characterized in that, Includes the following steps: A substrate is provided for growth, and an N-type semiconductor layer, a multiple quantum well active layer and a P-type semiconductor layer are sequentially deposited on the substrate to form an epitaxial layer; A current blocking layer, an ITO conductive film, and a mask blocking layer are sequentially fabricated on the epitaxial layer to form an initial chip. The mask blocking layer is used to divide the surface of the ITO conductive film into an etching area and a masking area. The step of sequentially fabricating a current blocking layer, an ITO conductive film, and a mask blocking layer on the epitaxial layer includes: The epitaxial layer is etched to expose a portion of the N-type semiconductor layer; A SiO2 layer is deposited on the surface of the etched epitaxial layer, and the SiO2 layer is photolithographically treated to form a current blocking layer. An ITO conductive film is deposited on the surface of the epitaxial layer where the current blocking layer is disposed by magnetron sputtering, and then annealed. A Ni metal layer is fabricated on the ITO conductive film, and the Ni metal layer is subjected to wet etching to form a mask barrier layer. The initial chip is placed in a plasma chamber, and a reaction gas including ethanol is injected into the plasma chamber. After the reaction gas undergoes an ionization process and a reaction process with the ITO conductive film, a groove is formed in the etched area of ​​the ITO conductive film to complete the surface roughening. The initial chip with roughened surface is then processed into a finished chip.

2. The method for preparing an LED chip according to claim 1, characterized in that, The specific steps for growing an epitaxial layer on the substrate are as follows: Metal chemical vapor deposition was employed, using high-purity hydrogen as the carrier gas, high-purity ammonia as the nitrogen source, trimethylgallium and triethylgallium as gallium sources, trimethylindium as the indium source, silane as the N-type dopant, trimethylaluminum as the aluminum source, and magnesia pyrocene as the P-type dopant.

3. The method for preparing an LED chip according to claim 2, characterized in that, The N-type semiconductor layer is doped with Si, the P-type semiconductor layer is doped with Mg, and the Si doping concentration in the N-type semiconductor layer is 5 × 10⁻⁶. 18 cm -3 ~1×10 19 cm -3 The doping concentration of Mg in the P-type semiconductor layer is 5 × 10⁻⁶. 17 cm -3 ~1×10 20 cm -3 .

4. The method for preparing an LED chip according to claim 1, characterized in that, The thickness of the SiO2 layer is 280nm~320nm, and the thickness of the Ni metal layer is 180nm~220nm.

5. The method for preparing an LED chip according to claim 1, characterized in that, The reaction gases also include argon.

6. The method for preparing an LED chip according to claim 1, characterized in that, The chemical reaction formula for the ionization process is: C2H5OH → CH + 3+CH 2+ 2+OH - + 2e, 2OH - → H2O↑+O - , CH + 3+e→CH 3; The chemical reaction formula for the reaction process is: In + 3CH 3→ In(CH3)3↑, Sn + 4CH 3→ Sn(CH3)4↑, In + 3CH 3+ 3O - → In(OCH3)3↓。 7. The method for preparing an LED chip according to claim 1, characterized in that, After placing the initial chip in a plasma chamber and injecting reactive gas into the plasma chamber, and after the reactive gas undergoes an ionization and reaction process with the ITO conductive film to form grooves in the etched area of ​​the ITO conductive film to complete the surface roughening step, the method further includes: Cleaning gas is injected into the plasma chamber at preset intervals to remove deposits in the groove.

8. The method for preparing an LED chip according to claim 7, characterized in that, The cleaning gas is oxygen, the preset interval is 25S~35S, and the injection time of the cleaning gas is 8S~12S.

9. The method for preparing an LED chip according to claim 1, characterized in that, The step of preparing the initial chip with roughened surface into a finished chip includes: Remove the mask barrier layer on the initial chip after surface roughening; Electrodes are fabricated on the initial chip to obtain a staged chip; A silicon oxide passivation layer is fabricated on the surface of the chip at the aforementioned stage to obtain the finished chip.

Citation Information

Patent Citations

  • Wafer level package method for semiconductor device

    CN104393153A

  • Light emitting element and light emitting element manufacturing method

    JP2016129180A