A rh furnace alloy calcification model and a method for directly calcifying smelting by using calcium-containing alloy
By using the RH furnace alloy calcification model and direct calcification smelting method, and by adding alloys or calcium-based alloys to the steel composition, the problem of poor calcium treatment effect in the RH furnace was solved, achieving efficient and environmentally friendly calcification smelting, reducing costs and improving the quality of molten steel.
Patent Information
- Application Number
- CN202311269963.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-28
- Publication Date
- 2025-12-30
- Estimated Expiration
- 2043-09-28
AI Technical Summary
Existing methods for treating calcium in RH furnaces suffer from problems such as poor calcium treatment efficiency, long smelting cycles, significant environmental impact, and high costs.
The RH furnace alloy calcification model is adopted. The alloy is added or a portion of calcium alloy is added according to the steel composition. Direct calcification smelting is carried out through the converter-LF-RH furnace-continuous casting process. The alloying method is selected according to the difference in manganese/silicon ratio. The alloy is added by using a high-level silo and aligned with the position of the vacuum tank downcomer to achieve efficient absorption of calcium.
It reduces steelmaking costs, shortens the smelting cycle, improves the purity of molten steel and environmental benefits, and avoids the drawbacks of calcium treatment.
Smart Images

Figure BDA0004475282560000061 
Figure BDA0004475282560000071 
Figure BDA0004475282560000081
Abstract
Description
Technical Field
[0001] This invention belongs to the field of iron and steel metallurgy and steelmaking, and particularly relates to an RH furnace alloy calcification model and a method for direct calcification smelting using calcium-containing alloys. Background Technology
[0002] The main purpose of calcium treatment in refining furnaces is to control alumina inclusions in molten steel: firstly, to reduce the total amount of inclusions; secondly, to change the morphology of inclusions; and thirdly, to reduce clogging and blockage at the tundish nozzle. Currently, most domestic enterprises mainly utilize calcium wire to modify Al2O3 inclusions. Calcium is a volatile metal with a melting point of 850℃ and a boiling point of 1492℃, far lower than typical steelmaking temperatures. Its density is 1.55 g / cm³. 3 It is 1 / 5 the volume of calcium in steel. From the relationship between calcium vapor pressure and temperature, we know that the vapor pressure at 1600℃ is 0.18 MPa, and it vaporizes immediately upon contact with molten steel. Therefore, adding calcium to steel using conventional methods is very difficult. These difficulties can be overcome by using injection metallurgy methods and wire feeding methods to inject calcium powder deep into the molten steel.
[0003] Most steel mills currently use a traditional wire feeder to feed pure calcium-coated wire into molten steel, followed by soft blowing to remove non-metallic inclusions. The effectiveness of calcium treatment depends primarily on the type of cored wire, the feeding speed, and the feeding position. The calcium treatment method involves directly adding pure calcium-coated wire into the molten steel via a wire feeder. To ensure a suitable calcium yield, the feeding speed must be controlled, typically between 1.5 and 3.0 m / min. However, because the slag surface of the ladle in an RH furnace (vacuum circulating degassing refining furnace) is essentially crusted (solid slag) after vacuum treatment, a large amount of argon gas is needed to blow open the slag surface before wire feeding. Simultaneously, during the feeding process, the calcium violently boils and splashes in the molten steel, increasing the likelihood of secondary oxidation, nitrogen absorption, and slag entrapment leading to large inclusions. This is detrimental to the control of steel purity, generates significant dust affecting the steel mill's environmental quality control, and increases the smelting cycle of the RH furnace, hindering smelting efficiency.
[0004] Therefore, it is urgent to find a solution that optimizes the existing calcium treatment process in RH furnaces, avoids the drawbacks of calcium treatment, and reduces steelmaking costs and improves smelting efficiency. Summary of the Invention
[0005] In view of this, the purpose of this invention is to provide an RH furnace alloy calcification model and a method for direct calcification smelting using calcium-containing alloys. This invention can effectively avoid the drawbacks of current calcium treatment methods. It utilizes the addition of required alloys or supplementary calcium alloys in the steel composition to achieve direct calcium treatment in the RH furnace. Based on the calcium yield law of calcium alloys, a steel alloying and calcium treatment addition model is formed according to the differences in manganese and silicon ratios of different steel grades. This invention can significantly reduce the cost of current steelmaking processes, shorten the smelting cycle, avoid the environmental impact of calcium treatment on steelmaking, and further improve the quality of molten steel.
[0006] This invention provides an RH furnace alloy calcification model, comprising:
[0007] When the manganese / silicon ratio is ≤4.5, and the steel grade (Si) 目标 -Mn 目标 When ( / 4.5) < 0.15, silicon-manganese alloying is used, and calcium treatment is performed using ferrosilicon + silicon-calcium-barium alloy.
[0008] When the manganese / silicon ratio is ≤4.5, and the steel grade (Si) 目标 -Mn 目标 When / 4.5)≥0.15, silicon-manganese alloying is used, and ferrosilicon alloy is used for calcium treatment;
[0009] When the manganese / silicon ratio is greater than 4.5, silicon-manganese alloy with high manganese is used for alloying, and silicon-calcium-barium alloy is used for calcium treatment.
[0010] In this invention, the manganese / silicon ratio is the ratio of manganese to silicon in the target steel composition.
[0011] Preferably, 4.5 < manganese / silicon ratio ≤ 6; or 3 ≤ manganese / silicon ratio ≤ 4.3; more preferably, 4.5 < manganese / silicon ratio ≤ 5.8; or 3 ≤ manganese / silicon ratio ≤ 4.16. In a specific embodiment, the manganese / silicon ratio = 3, and Si 目标 -Mn 目标 / 4.5=0.10<0.15 The converter uses silicon-manganese alloying; or the manganese / silicon ratio = 5.8, the converter uses silicon-manganese + high manganese alloying; or the manganese / silicon ratio = 4.16, and Si 目标 -Mn 目标 / 4.5 = 0.022 < 0.15, therefore the converter uses silicon-manganese alloying.
[0012] This invention provides a method for direct calcification smelting using calcium-containing alloys, comprising:
[0013] 1) The converter uses silicon-manganese + high-manganese or silicon-manganese alloying according to the manganese / silicon ratio of the steel composition system, so as to meet the steel composition requirements for manganese content;
[0014] 2) In the LF refining furnace, the temperature and composition of the molten steel are adjusted according to the requirements of the steel grade, and when the manganese / silicon ratio is ≤4.5 and the steel grade (Si) is... 目标 -Mn 目标 When ( / 4.5)≥0.15, the silicon element addition amount in the LF furnace is (Si 目标 -Mn 目标 / 4.5-0.15)%, other cases do not adjust silicon content, steel is tapped after yellow-white slag;
[0015] 3) Vacuum circulating degassing refining (RH) furnace is used for vacuum degassing and removal of inclusions. After circulation, ferrosilicon or ferrosilicon + calcium-barium silicon or calcium-barium silicon is added for alloying and calcification treatment. After pure circulation, it is soft blown out of the station.
[0016] Preferably, when the manganese / silicon ratio is ≤4.5, and the steel grade (Si) 目标 -Mn 目标 When ( / 4.5) < 0.15, the converter alloy is alloyed with silicon-manganese, and the RH furnace is treated with ferrosilicon + silicon-calcium-barium alloy for calcium treatment.
[0017] When the manganese / silicon ratio is ≤4.5, and the steel grade (Si) 目标 -Mn 目标 When / 4.5)≥0.15, the converter alloy is alloyed with silicon-manganese, and the RH furnace is treated with ferrosilicon alloy for calcium treatment;
[0018] When the manganese / silicon ratio is greater than 4.5, the converter uses silicon-manganese + high manganese for alloying, and the RH furnace uses silicon-calcium-barium for calcium treatment.
[0019] Preferably, the amount of calcium-based alloy added in the RH furnace is required to be as follows:
[0020] 1) When the manganese / silicon ratio is ≤4.5, and the steel grade (Si) 目标 -Mn 目标 When (4.5) < 0.15, the amount of ferrosilicon added to the RH furnace is (Si 目标 -Mn 目标 / 4.5)×10 / 0.75 / 0.8kg / ton of steel, the amount of silicon-calcium-barium added is {15-[(Si 目标 -Mn 目标 / 4.5)×10 / 0.75 / 0.8 / 2.5×15]}×1.2 / 15kg / ton of steel;
[0021] 2) When the manganese / silicon ratio is ≤4.5, and the steel grade (Si) 目标 -Mn 目标 When / 4.5)≥0.15, add 2~2.5kg / ton of ferrosilicon alloy to the RH furnace for calcium treatment;
[0022] 3) When the manganese / silicon ratio is >4.5, add 1.0 to 1.2 kg / ton of silicon-calcium-barium alloy to the RH furnace for calcium treatment.
[0023] Preferably, the RH furnace calcification alloy is added through a high-level silo, and the alloy is added aligning with the vacuum tank downcomer, with the circulation flow rate controlled at 120 m³ / s. 3 The circulation flow rate is above 120 m³ / h, the vacuum degree is controlled below 133 Pa, and the slag thickness in the ladle is controlled below 100 mm. In a specific embodiment, the circulation flow rate is 120 m³ / h. 3 / h or 125m 3 / h; vacuum degree is 67Pa, 100Pa or 25Pa, ladle slag thickness is 80mm, 90mm or 70mm;
[0024] Preferably, the circulation time is greater than or equal to 15 minutes;
[0025] The duration of soft blowing is 8 to 12 minutes.
[0026] Preferably, the calcium content in ferrosilicon is between 1% and 1.5%, and the calcium content after refining is 45% to 50%.
[0027] The calcium content in silicon-calcium-barium alloy is between 11% and 13%, and the calcium content in refined alloy is 10% to 15%.
[0028] Preferably, the steel grade is selected from Q355NHD weathering steel, P355GH pressure vessel steel plate, or smelting steel grade Q355B.
[0029] Preferably, the pure circulation exits the station after 5-6 minutes.
[0030] This invention provides an RH furnace alloy calcification model, comprising: when the manganese / silicon ratio is ≤4.5, and the steel grade (Si) 目标 -Mn 目标 When the manganese / silicon ratio is less than 0.15, silicon-manganese alloying is used, and calcium treatment is performed using a silicon-iron + silicon-calcium-barium alloy; when the manganese / silicon ratio is ≤ 4.5, and the steel grade (Si) is... 目标 -Mn 目标 When the manganese / silicon ratio is ≥0.15, silicon-manganese alloying is used, and ferrosilicon alloying is used for calcium treatment. When the manganese / silicon ratio is >4.5, silicon-manganese + high-manganese alloying is used, and silicon-calcium-barium alloying is used for calcium treatment. This invention applies the above model to the calcination smelting of calcium-containing alloys. The smelting process is organized using a converter-LF-RH furnace-continuous casting process. It utilizes the addition of the required alloys or supplementary calcium alloys in the steel composition to achieve direct calcium treatment in the RH furnace. Based on the calcium yield law of calcium alloys, a model for steel alloying and calcium treatment is formed for the differences in manganese-silicon ratios of different steel grades. This invention utilizes the alloys (ferrosilicon) required by the steel composition itself or supplementary silicon-calcium-barium alloys for direct calcination; it reduces environmental pollution and steel pollution caused by calcination, while shortening the RH furnace smelting cycle, creating better technical conditions for reducing steelmaking costs and improving smelting efficiency. Detailed Implementation
[0031] To further illustrate the present invention, the following detailed description, in conjunction with embodiments, of an RH furnace alloy calcification model and a method for direct calcification smelting using calcium-containing alloys provided by the present invention, should not be construed as limiting the scope of protection of the present invention.
[0032] This invention provides an RH furnace alloy calcification model, comprising:
[0033] When the manganese / silicon ratio is ≤4.5, and the steel grade (Si) 目标 -Mn 目标 When ( / 4.5) < 0.15, silicon-manganese alloying is used, and calcium treatment is performed using ferrosilicon + silicon-calcium-barium alloy.
[0034] When the manganese / silicon ratio is ≤4.5, and the steel grade (Si) 目标 -Mn 目标 When / 4.5)≥0.15, silicon-manganese alloying is used, and ferrosilicon alloy is used for calcium treatment;
[0035] When the manganese / silicon ratio is greater than 4.5, silicon-manganese alloy with high manganese is used for alloying, and silicon-calcium-barium alloy is used for calcium treatment.
[0036] This invention employs a converter-LF-RH furnace-continuous casting process for smelting, producing steel grades including wear-resistant, high-strength, bridge, and ship plate steels. The invention utilizes the alloys (ferrosilicon) required by the steel composition itself, or adds a portion of silicon-calcium-barium alloy, for direct calcification. This reduces environmental and steel pollution caused by calcification, while shortening the RH furnace smelting cycle, creating favorable technical conditions for reducing steelmaking costs and improving smelting efficiency.
[0037] This invention provides a method for direct calcification smelting using calcium-containing alloys, comprising:
[0038] 1) The converter uses silicon-manganese + high-manganese or silicon-manganese alloying according to the manganese / silicon ratio of the steel composition system, so as to meet the steel composition requirements for manganese content;
[0039] 2) In the LF refining furnace, the temperature and composition of the molten steel are adjusted according to the requirements of the steel grade, and when the manganese / silicon ratio is ≤4.5 and the steel grade (Si) is... 目标 -Mn 目标 When ( / 4.5)≥0.15, the silicon element addition amount in the LF furnace is (Si 目标 -Mn 目标 / 4.5-0.15)%, other cases do not adjust silicon content, steel is tapped after yellow-white slag;
[0040] 3) Vacuum circulating degassing refining (RH) furnace is used for vacuum degassing and removal of inclusions. After circulation, ferrosilicon or ferrosilicon + calcium-barium silicon or calcium-barium silicon is added for alloying and calcification treatment. After pure circulation, it is soft blown out of the station.
[0041] In a specific embodiment, the method includes the following steps:
[0042] 1) The converter alloy composition is based on a manganese / silicon ratio of 4.5; when the manganese / silicon ratio is ≤4.5, and the steel grade (Si) 目标 -Mn 目标 When the manganese / silicon ratio is less than 0.15, the converter alloy is alloyed using silicon-manganese; when the manganese / silicon ratio is ≤ 4.5, and the steel grade (Si) is... 目标 -Mn 目标 When the manganese / silicon ratio is ≥0.15, the converter alloy is also alloyed using silicon-manganese; when the manganese / silicon ratio is >4.5, the converter uses silicon-manganese + high manganese for alloying.
[0043] 2) LF refining adjusts the molten steel temperature and composition according to the steel grade requirements, and when the manganese / silicon ratio is ≤4.5 and the steel grade (Si) is... 目标 -Mn 目标 When ( / 4.5)≥0.15, the silicon element addition amount in the LF furnace is (Si 目标 -Mn 目标 / 4.5-0.15)%, other cases do not adjust silicon content, steel is tapped after yellow-white slag;
[0044] 3) The RH furnace uses this treatment mode for vacuum degassing and inclusion removal. After 15 minutes of circulation, ferrosilicon or ferrosilicon + silicon-calcium-barium or silicon-calcium-barium alloying and calcification are added. The steelmaking alloy addition and alloy calcification are based on a manganese / silicon ratio of 4.5 in the steel grade composition. When the manganese / silicon ratio is ≤4.5, and the steel grade (Si... 目标 -Mn 目标 When the manganese / silicon ratio is less than 0.15, the RH furnace uses ferrosilicon + silicon-calcium-barium alloy for calcium treatment; when the manganese / silicon ratio is ≤4.5, and the steel grade (Si) is... 目标 -Mn 目标 When the manganese / silicon ratio is greater than 4.5, the RH furnace uses ferrosilicon alloy for calcium treatment; when the manganese / silicon ratio is greater than 4.5, the RH furnace uses silicon-calcium-barium alloy for calcium treatment; after pure circulation for 5-6 minutes, the furnace exits the station for soft blowing, which takes 8-12 minutes.
[0045] In this invention, when the manganese / silicon ratio is ≤4.5, and the steel grade (Si) 目标 -Mn 目标 When ( / 4.5) < 0.15, the converter alloy is alloyed with silicon-manganese, and the RH furnace is treated with ferrosilicon + silicon-calcium-barium alloy for calcium treatment.
[0046] When the manganese / silicon ratio is ≤4.5, and the steel grade (Si) 目标 -Mn目标 When / 4.5)≥0.15, the converter alloy is alloyed with silicon-manganese, and the RH furnace is treated with ferrosilicon alloy for calcium treatment;
[0047] When the manganese / silicon ratio is greater than 4.5, the converter uses silicon-manganese + high manganese for alloying, and the RH furnace uses silicon-calcium-barium for calcium treatment.
[0048] In this invention, the required amount of calcium-based alloy added to the RH furnace is as follows:
[0049] 1) When the manganese / silicon ratio is ≤4.5, and the steel grade (Si) 目标 -Mn 目标 When (4.5) < 0.15, the amount of ferrosilicon added to the RH furnace is (Si 目标 -Mn 目标 / 4.5)×10 / 0.75 / 0.8kg / ton of steel, the amount of silicon-calcium-barium added is {15-[(Si 目标 -Mn 目标 / 4.5)×10 / 0.75 / 0.8 / 2.5×15]}×1.2 / 15kg / ton of steel;
[0050] 2) When the manganese / silicon ratio is ≤4.5, and the steel grade (Si) 目标 -Mn 目标 When / 4.5)≥0.15, add 2~2.5kg / ton of ferrosilicon alloy to the RH furnace for calcium treatment;
[0051] 3) When the manganese / silicon ratio is >4.5, add 1.0 to 1.2 kg / ton of silicon-calcium-barium alloy to the RH furnace for calcium treatment.
[0052] In this invention, the RH furnace calcification alloy is added through a high-level silo, and the alloy is added precisely to the vacuum tank downcomer, with the circulation flow rate controlled at 120 m³ / s. 3 The vacuum degree is controlled within 133 Pa and the slag thickness in the ladle is controlled within 100 mm.
[0053] In this invention, the circulation time is greater than or equal to 15 minutes;
[0054] The duration of soft blowing is 8 to 12 minutes.
[0055] In this invention, the calcium content in ferrosilicon is between 1 and 1.5 wt%, and the calcium content after refining is 45 to 50%.
[0056] The calcium content in silicon-calcium-barium alloy is between 11 and 13 wt%, and the calcium yield from refining is 10 to 15%.
[0057] In this invention, the steel grade is selected from Q355NHD weathering steel, P355GH pressure vessel steel plate, or smelting steel grade Q355B.
[0058] Compared with the prior art, the advantages of the present invention are:
[0059] This invention eliminates the current smelting technology using calcium wire treatment. Starting from the steel's inherent composition, it changes the timing of adding calcium-containing alloy ferrosilicon during steelmaking. Instead of adding it during converter tapping, it shifts to adding it later in the RH furnace treatment process. This fully utilizes the beneficial calcium element in the alloy, achieving calcium treatment of the molten steel during alloying, thus avoiding the drawbacks of existing calcium wire treatment and opening up new avenues for calcium treatment in steelmaking. Furthermore, based on different steel compositions, this invention establishes requirements for the types of alloys used in converter alloying, RH furnace alloying, and calcium treatment, as well as the required amount of calcium alloy added. It forms a smelting model for direct calcium treatment of calcium-based alloys in an RH furnace, enabling calcium-based alloys to be applied to different steel composition systems. This invention can significantly improve steel purity and reduce steelmaking costs, offering environmental benefits.
[0060] This invention utilizes a direct feeding method from the high-level hopper of an RH furnace, with the material added precisely to the vacuum trough downcomer. This allows the silicon-calcium-barium alloy to come into direct contact with the molten steel, reducing calcium loss. Furthermore, it fully leverages the molten steel flow velocity (greater than 1.5 m / s) in the downcomer to carry the calcium alloy deep into the molten steel, thereby utilizing the static pressure of the molten steel to achieve full absorption of calcium and improve the calcium recovery rate of the calcium alloy. On the other hand, silicon can reduce the activity of calcium in the molten droplets, preventing calcium oxidation.
[0061] Example 1
[0062] A model and smelting method for direct calcification treatment using calcium-containing alloys are disclosed. The smelting process employs a converter-LF-RH furnace-continuous casting workflow. The calcium content in ferrosilicon is 1.2%, with a calcium recovery rate of 50%; the calcium content in silicon-calcium-barium alloy is 12%, with a calcium recovery rate of 13%. The smelted steel grade is Q355NHD weathering steel, with the following composition:
[0063] Table 1
[0064]
[0065] 1) The manganese / silicon ratio of Q355NHD weathering steel is 3; therefore, the manganese / silicon ratio is ≤4.5, and Si 目标 -Mn 目标 / 4.5=0.10<0.15 The converter uses silicon-manganese alloying;
[0066] 2) LF refining adjusts the temperature and composition of molten steel according to the requirements of the steel grade, but does not adjust the silicon content. The steel is tapped after the yellow-white slag is produced.
[0067] 3) The RH furnace uses this processing mode (dehydrogenation treatment) for vacuum degassing and inclusion removal, therefore the manganese / silicon ratio is ≤4.5, and Si目标 -Mn 目标 / 4.5=0.10<0.15, after 15 minutes of circulation, ferrosilicon + barium silicate is added for alloying and calcification treatment. The amount of ferrosilicon added to the RH furnace is (Si 目标 -Mn 目标 / 4.5)×10 / 0.75 / 0.8kg / ton of steel=1.6kg / ton of steel, the amount of silicon-calcium-barium added is {15-[(Si 目标 -Mn 目标 / 4.5)×10 / 0.75 / 0.8 / 2.5×15]}×1.2 / 15kg / ton of steel=0.4kg / ton of steel; after pure circulation for 6 minutes, soft blowing is performed at the station, and the soft blowing time is 12 minutes; the RH furnace calcification alloy is added through the high-level silo, and the alloy is added aligned with the vacuum trough downcomer position, with a circulation flow rate of 120m³. 3 / h, vacuum degree is 67Pa, ladle slag thickness is 80mm;
[0068] Theoretical calculation of calcium content at the final stage of molten steel:
[0069] Calcium % = 1.6 × 1.2% × 50% / 10% + 0.4 × 12% × 13% / 10% = 0.0016%;
[0070] The actual measured calcium content at the endpoint was 15 ppm, which meets the requirements for calcium treatment of steel grades.
[0071] Example 2
[0072] The smelting process adopts a converter-LF-RH furnace-continuous casting process. The calcium content in ferrosilicon is 1.0%, with a calcium recovery rate of 50%; the calcium content in silicon-calcium-barium is 12%, with a calcium recovery rate of 13%. The composition of the smelted steel grade P355GH pressure vessel steel plate is shown in Table 2 below.
[0073] Table 2
[0074]
[0075] 1) The manganese / silicon ratio of the P355GH pressure vessel is 5.8; when the manganese / silicon ratio is ≥4.5, the converter uses silicon-manganese + high manganese alloying.
[0076] 2) LF refining adjusts the temperature and composition of molten steel according to the requirements of the steel grade, but does not adjust the silicon content, and taps the steel after producing yellow-white slag;
[0077] 3) The RH furnace uses this treatment mode for vacuum degassing and inclusion removal. After 15 minutes of circulation, ferrosilicon or ferrosilicon + silicon-calcium-barium alloy is added for alloying and calcification. When the manganese / silicon ratio is ≥4.5, 1.2 kg / ton of silicon-calcium-barium alloy is added to the RH furnace for calcium treatment. After 6 minutes of pure circulation, the furnace exits for soft blowing for 10 minutes. The calcification alloy in the RH furnace is added through a high-level silo, aligned with the vacuum tank downcomer. The circulation flow rate is controlled at 120 m³ / ton. 3 / h, vacuum degree is 100Pa, ladle slag thickness is 90mm;
[0078] Theoretical calculation of calcium content at the final stage of molten steel:
[0079] Calcium % = 1.2 × 12% × 13% / 10% = 0.0018%;
[0080] The measured calcium content at the endpoint was 15 ppm, which meets the requirements for calcium treatment of steel grades.
[0081] Example 3
[0082] The smelting process adopts a converter-LF refining-RH furnace-continuous casting process. The calcium content in ferrosilicon is 1.3%, with a calcium recovery rate of 50%; the calcium content in silicon-calcium-barium is 11.8%, with a calcium recovery rate of 13%. The smelted steel grade is Q355B, and its composition is shown in Table 3 below.
[0083] Table 3
[0084]
[0085] 1) Q355B has a manganese / silicon ratio of 4.16; therefore, the manganese / silicon ratio is ≤4.5, and Si 目标 -Mn 目标 / 4.5=0.022<0.15, the converter uses silicon-manganese alloying;
[0086] 2) LF refining adjusts the temperature and composition of molten steel according to the requirements of the steel grade, but does not adjust the silicon content. The steel is tapped after the yellow-white slag is produced.
[0087] 3) The RH furnace uses this processing mode for vacuum degassing and inclusion removal. When the manganese / silicon ratio is ≤4.5, and Si 目标 -Mn 目标 / 4.5=0.022<0.15, after 15 minutes of circulation, ferrosilicon + barium silicate is added for alloying and calcification treatment. The ferrosilicon added to the RH furnace is (Si 目标 -Mn 目标 / 4.5)×10 / 0.75 / 0.8kg / ton of steel=0.36kg / ton of steel, the amount of silicon-calcium-barium added is {15-[(Si 目标 -Mn 目标 / 4.5)×10 / 0.75 / 0.8 / 2.5×15]}×1.2 / 15kg / ton of steel=1.02kg / ton of steel; after 6 minutes of pure circulation, soft blowing is performed at the station, with a soft blowing time of 12 minutes; the RH furnace calcification alloy is added through the high-level silo, and the alloy is added aligned with the vacuum trough downcomer position, with a circulation flow rate of 125m³ / h. 3 / h, vacuum degree is 25pa, ladle slag thickness is 70mm;
[0088] Theoretical calculation of calcium content at the final stage of molten steel:
[0089] Calcium % = 0.36 × 1.3% × 50 / 10% + 1.02 × 11.8% × 13% / 10% = 0.0018%;
[0090] The measured calcium content at the endpoint was 16 ppm, which meets the requirements for calcium treatment of steel grades.
[0091] As can be seen from the above embodiments, the calcium treatment effect of using the alloy calcium treatment model for different steel grades is good. The theoretical data of calcium treatment is not much different from the actual calcium content measured in steelmaking, and both meet the technical requirements of calcium treatment for steel grades. Therefore, this invention can achieve precise calcium treatment of steel grades and can completely replace the current calcium feeding line for calcium treatment process technology.
[0092] This invention utilizes the beneficial calcium element in alloys for calcification treatment of different steel grades in steelmaking, offering significant advantages over calcium treatment via a calcium-feeding wire. Firstly, by using an alloy required for the steel grade itself for calcification, the cost of the steelmaking process can be significantly reduced. Secondly, by eliminating the need for wire-feeding calcium treatment, refining time is significantly shortened, greatly improving refining capacity and creating better technical conditions for increasing the casting speed of continuous casting machines. Furthermore, by using calcium-containing alloys for direct calcification in an RH vacuum tank (the container used for RH steelmaking), air pollution is minimized, and this calcification technology also offers significant advantages in improving steel quality.
[0093] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A RH furnace alloy calciumization model, comprising: When the manganese / silicon ratio is ≤ 4.5, and the steel grade (Si 目标 - Mn 目标 / 4.5) < 0.15, alloying is performed using silicon manganese, and calcium treatment is performed using ferrosilicon + calcium-silicon-barium alloy; When the Mn / Si ratio is ≤ 4.5, and the steel grade (Si 目标 -Mn 目标 When the Mn / Si ratio is > 4.5, and the steel grade (Si / 4.5) is ≥ 0.15, alloying is performed with silicon manganese, and calcium treatment is performed with ferrosilicon. When the manganese / silicon ratio is >4.5, silicon manganese + high manganese is used for alloying, and silicon calcium barium is used for calcium treatment.
2. The RH ladle alloy calcification model of claim 1, wherein, 4.5 < manganese / silicon ratio ≤5.8; or 3 ≤ manganese / silicon ratio ≤4.
16.
3. A method for direct calciumization smelting by using calcium-containing alloy, comprising: 1) The converter is alloyed with silicon manganese + high manganese or silicon manganese according to the manganese / silicon ratio of the steel grade composition system, and the manganese element is matched to meet the steel grade composition requirements; 2) Adjust the temperature and composition of the molten steel in the LF refining furnace according to the requirements of the steel grade, and when the Mn / Si ratio is ≤4.5 and the steel grade (Si 目标 -Mn 目标 / 4.5) ≥0.15, the LF furnace silicon element addition amount is (Si 目标 -Mn 目标 / 4.5-0.15)%, and in other cases, the silicon element is not adjusted, and the molten steel is tapped after yellow-white slagging. 3) The vacuum circulating degassing refining (RH) furnace is used for vacuum degassing and inclusion removal, and after circulation, silicon iron or silicon iron + silicon calcium barium or silicon calcium barium is added for alloying and calcium treatment, and after pure circulation, soft blowing is performed.
4. The method of claim 3, wherein, When the manganese / silicon ratio is ≤ 4.5, and the steel grade (Si 目标 -Mn 目标 When the manganese / silicon ratio is > 4.5 and < 0.15, the converter alloy is alloyed with silicon manganese, and the RH furnace is calcium treated with ferrosilicon + calcium-silicon-barium alloy; When the manganese / silicon ratio is ≤ 4.5, and the steel grade (Si 目标 -Mn 目标 / 4.5)≥0.15, the converter alloy is alloyed with silicon manganese, and the RH furnace is calcium treated with ferrosilicon alloy; When the manganese / silicon ratio is >4.5, the converter is alloyed with silicon manganese + high manganese, and the RH furnace is calcium treated with silicon calcium barium.
5. The method of claim 3, wherein, The addition amount of calcium-based alloy in the RH furnace is as follows: 1) when Mn / Si ratio ≤ 4.5, and steel grade (Si 目标 -Mn 目标 / 4.5) < 0.15, the amount of ferrosilicon added in RH furnace is (Si 目标 -Mn 目标 / 4.5) x 10 / 0.75 / 0.8 kg / ton of steel, and the amount of silicon calcium barium added is {15 - [(Si 目标 -Mn 目标 / 4.5) x 10 / 0.75 / 0.8 / 2.5 x 15]} x 1.2 / 15 kg / ton of steel; 2) When the Mn / Si ratio is < 4.5, and the steel grade (Si 目标 - Mn 目标 / 4.5) > 0.15, RH furnace addition of ferrosilicon 2-2.5 kg / ton of steel for calcium treatment; 3) When the manganese / silicon ratio is >4.5, 1.0-1.2 kg / ton of steel of silicon calcium barium alloy is added in the RH furnace for calcium treatment.
6. The method of claim 3, wherein, RH furnace calcium alloy is added through high-position stock bin, and the alloy is added in alignment with the position of the vacuum tank descending pipe, the ring flow is controlled at 120 m 3 / h or more, the vacuum degree is controlled within 133 Pa, and the ladle slag thickness is controlled within 100 mm.
7. The method of claim 3, wherein, The circulation time is greater than or equal to 15 min; The soft blowing time is 8-12 min.
8. The method of claim 3, wherein, The calcium element in silicon iron is between 1-1.5%, and the refining calcium element yield is 45-50%; The calcium element in silicon calcium barium is between 11-13%, and the refining calcium element yield is 10-15%.
9. The method of claim 3, wherein, The steel grade is selected from Q355NHD weathering steel, P355GH pressure vessel steel plate, or smelted steel grade Q355B.
10. The method of claim 3, wherein, After pure circulation for 5-6 min, the station is out.
Citation Information
Patent Citations
Method for carrying out molten steel silicon alloying and calcium treatment by using metal-calcium-containing silicon-iron alloy
CN108642239A
Method for improving smelting purity of weathering steel
CN115232920A