A coaxial copper conductor cable with high electromagnetic shielding effectiveness and preparation method thereof
Through the combination of modified nano-zinc oxide and silane coupling agent-treated zirconia fiber membrane and silver-loaded zirconia powder, the problem of reduced bendability caused by the thick shielding layer of coaxial cables is solved, and high electromagnetic shielding efficiency is achieved and good thermal temperature performance.
Patent Information
- Application Number
- CN202311393135.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-25
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-10-25
AI Technical Summary
The thick shielding layer of coaxial cable reduces its bendability, limiting its use in applications with high electromagnetic shielding requirements.
The zirconia fiber membrane treated with modified nano-zinc oxide and silane coupling agent is used as the shielding membrane. A three-layer structure shielding membrane is prepared through electrostatic spinning and hot pressing composite technology, combined with silver-loaded zirconia powder and adhesive film. Improve electromagnetic shielding effectiveness.
It achieves higher electromagnetic shielding effectiveness without increasing the thickness of the shielding layer, and improves the bendability and thermal temperature performance of the coaxial copper conductor cable.
Smart Images

Figure BDA0004513091840000101
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of coaxial cables, and in particular relates to a coaxial copper conductor cable with high electromagnetic shielding effectiveness and a preparation method thereof. Background Art
[0002] Coaxial cable is a cable mainly used for signal transmission. Its application scenarios include cable TV transmission, long-distance telephone transmission, short-distance connection between computer systems, and local area networks. It is generally composed of four layers of materials, from the outside to the inside, the sheath, the mesh conductor, the insulation layer, and the center conductor. The center conductor of a coaxial copper conductor cable is usually made of copper, because copper has good conductivity and can efficiently transmit electrical signals. The insulation layer is used to isolate the center conductor and the shielding layer, and is usually made of insulating materials such as polyethylene and polypropylene. The mesh conductor serves as a shielding layer, which is usually woven from thin metal wires, or it can be a metal foil wrapped around the outside of the insulation layer. Finally, the outer sheath is used to protect the cable from physical damage, and is usually made of materials such as PVC or polyvinyl chloride.
[0003] The shielding layer can provide electromagnetic shielding performance, prevent the intrusion of external interference signals and prevent the leakage of internal signals and thus interfere with nearby devices, which helps to improve signal quality. However, in some application scenarios with high shielding requirements, the shielding layer of the coaxial cable is generally set thicker, which limits the bendability of the coaxial cable and makes it inconvenient to use. Summary of the invention
[0004] One of the purposes of the present invention is to provide a coaxial copper conductor cable with high electromagnetic shielding effectiveness to solve the problem that the bendability of the coaxial cable is reduced due to the thick shielding layer. The second purpose is to provide a method for preparing a coaxial copper conductor cable with high electromagnetic shielding effectiveness.
[0005] The purpose of the present invention can be achieved by the following technical solutions:
[0006] A coaxial copper conductor cable with high electromagnetic shielding effectiveness, with a copper conductor at the center and outwardly including an insulating layer, a shielding film, a mesh conductor and a rubber sheath in sequence; wherein the shielding film is prepared by the following steps:
[0007] Step 1: Add nano zinc oxide, isopropanol and water into a reaction kettle, add silane coupling agent after ultrasonic dispersion for 15-30 minutes, stir for 30-60 minutes at 25-30° C., filter and dry to obtain modified nano zinc oxide;
[0008] Step 2: Add the modified nano zinc oxide modified by N,N-dimethylformamide and silane coupling agent into the reactor, ultrasonically disperse for 20-30 minutes, add 4,4'-diaminodiphenyl ether into the reactor at 5-10°C, stir for 15-20 minutes at 200-500r / min, then add pyromellitic anhydride into the reactor and continue stirring for 2-3 hours to obtain a spinning solution;
[0009] Step 3: Under the conditions of an ambient temperature of 25±5°C and an ambient humidity of 35±2%, the spinning solution is passed through an electrospinning machine to form a fiber membrane; the working parameters of the electrospinning machine are: a voltage of 18 kV, a speed of a receiving device of 40 r / min, and a receiving distance of 15 cm;
[0010] Step 4: placing the fiber membrane in a vacuum tube sintering furnace, keeping the temperature at 150-180°C for 30-45 minutes under nitrogen protection, then heating to 250-260°C at a rate of 2°C / min, keeping the temperature for 30-45 minutes, then heating to 340-350°C at a rate of 2°C / min, keeping the temperature for 45-60 minutes, and cooling naturally to obtain a zinc oxide-polyimide fiber membrane;
[0011] Step 5: Mix zirconia fibers with a length of 3-6 μm and deionized water, and obtain a zirconia fiber dispersion with a mass fraction of 20% after ultrasonic dispersion for 15-30 minutes, then add 25% alkaline silica sol, boric acid and soluble starch, stir for 30-45 minutes, and then ultrasonically disperse for 15-30 minutes to obtain a mixed slurry; pour the mixed slurry into a mold, vacuum filter, and vacuum dry at 80-90° C. to obtain a porous green body, keep the porous green body at 1300-1450° C. for 30-50 minutes, cool naturally, and crush to obtain a flower-shaped zirconia powder;
[0012] Step 6: Mix the flower-shaped zirconium oxide powder and deionized water, and obtain a 5% flower-shaped zirconium oxide dispersion liquid after ultrasonic dispersion for 15-30 minutes, then add a 60% silver nitrate solution, a 4% ammonia solution and a 5% glucose solution, react at 60±5° C. for 25-35 minutes, filter, wash the filter cake with deionized water for 3-5 times, and dry to obtain silver-loaded zirconium oxide powder;
[0013] Step 8: Dissolve the maleic anhydride grafted polyolefin with xylene by stirring, then add the modified silver-loaded zirconium oxide powder modified by the silane coupling agent, and ultrasonically disperse it in a closed container for 30-60 minutes to obtain a casting solution, and then scrape the casting solution flat on a polytetrafluoroethylene plate and dry it to obtain a film;
[0014] Step 7: Add silver-loaded zirconium oxide powder, isopropanol and water into a reaction kettle, add a silane coupling agent after ultrasonic dispersion for 15-30 minutes, stir for 30-60 minutes at 25-30° C., filter and dry to obtain modified silver-loaded zirconium oxide powder;
[0015] Step nine: stack the first layer of zinc oxide-polyimide fiber membrane, the adhesive film and the second layer of zinc oxide-polyimide fiber membrane in sequence, with the adhesive film located between the two layers of zinc oxide-polyimide fiber membranes, and hot-press and laminate them at 110-120°C to obtain a three-layer shielding membrane.
[0016] Furthermore, the dosage ratio of nano zinc oxide, isopropyl alcohol, water and silane coupling agent is 2-5g: 18-25mL: 2-3mL: 2-2.5mL.
[0017] Furthermore, the dosage ratio of N,N-dimethylformamide, modified nano zinc oxide, 4,4'-diaminodiphenyl ether and pyromellitic anhydride is 100-120 mL: 5-6 g: 9.87-11.84 g: 10.85-13.03 g.
[0018] Furthermore, the usage ratio of the zirconium oxide fiber dispersion, the alkaline silica sol, the boric acid and the soluble starch is 50g:9g:1g:2g.
[0019] Furthermore, the dosage ratio of the flower-shaped zirconium oxide dispersion, the silver nitrate solution, the ammonia water and the glucose solution is 80 g: 20 mL: 160 mL: 0.5-0.8 mL.
[0020] Furthermore, the usage ratio of silver-loaded zirconium oxide powder, isopropyl alcohol, water and silane coupling agent is 4-5 g: 18-25 mL: 2-3 mL: 2-2.5 mL.
[0021] Furthermore, the usage ratio of maleic anhydride grafted polyolefin, xylene and modified silver-loaded zirconium oxide powder is 5-6g:95g:1.2-1.5g.
[0022] Furthermore, the silane coupling agent is any one of silane coupling agent KH550, silane coupling agent KH560 and silane coupling agent KH570.
[0023] Furthermore, the thickness ratio of the single-layer zinc oxide-polyimide fiber film and the adhesive film is 2:1.
[0024] Beneficial effects of the present invention:
[0025] The shielding film used in the coaxial copper conductor cable with high electromagnetic shielding effectiveness of the present invention has a higher shielding coefficient than ordinary aluminum-plated films, and the coaxial copper conductor cable can obtain higher electromagnetic shielding effectiveness without using a thicker shielding layer.
[0026] The middle layer of the shielding film is a film, and both sides of the film are zinc oxide-polyimide fiber films. The substrate of the film is maleic anhydride grafted polyolefin, which has high polarity compared with ordinary polyolefin, and is conducive to bonding and compounding with polyimide materials; the film is prepared by casting film, and the modified silver-loaded zirconium oxide powder is modified by silane coupling agent, which has better dispersibility. The matrix of the modified silver-loaded zirconium oxide powder is flower-shaped zirconium oxide powder, which is prepared by zirconium oxide fiber and alkaline silica sol and other bonding materials. During the vacuum filtration process, deionized water and part of the bonding materials are extracted, and the overlapping parts of the porous blank are bonded by alkaline silica sol and the like, which is not easy to collapse. After sintering and crushing, the flower-shaped zirconium oxide powder with more fiber branches is obtained, which has a larger specific surface area and can load more silver through the silver mirror reaction, which helps to absorb more electromagnetic waves, thereby helping to improve the electromagnetic shielding effectiveness of the film.
[0027] The zinc oxide-polyimide fiber membrane is prepared by electrostatic spinning, and the nano zinc oxide contained in it is also treated with a silane coupling agent, which has better dispersibility and helps to improve its electromagnetic shielding performance; the zinc oxide-polyimide fiber membrane has good heat resistance, and the adhesion between the fiber membrane and the adhesive film is better, and the thermal temperature performance of the shielding membrane is better. DETAILED DESCRIPTION
[0028] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Example 1
[0030] This embodiment provides a coaxial copper conductor cable with high electromagnetic shielding effectiveness, including the following implementation steps:
[0031] A coaxial copper conductor cable with high electromagnetic shielding effectiveness, with a copper conductor at the center and outwardly including an insulating layer, a shielding film, a mesh conductor and a rubber sheath in sequence; wherein the shielding film is prepared by the following steps:
[0032] Step 1: Add 20 kg of nano zinc oxide, 180 L of isopropanol and 20 L of water into a reactor, add 20 L of silane coupling agent KH550 after ultrasonic dispersion for 15 min, stir at 25 ° C for 30 min, filter and dry to obtain modified nano zinc oxide.
[0033] Step 2: Add 100L N,N-dimethylformamide and 5kg of modified nano zinc oxide modified by silane coupling agent into the reactor, ultrasonically disperse for 20 minutes, add 9.87kg of 4,4'-diaminodiphenyl ether into the reactor at 5°C, stir for 15 minutes at 200r / min, then add 10.85kg of pyromellitic anhydride into the reactor and continue stirring for 2h to obtain the spinning solution.
[0034] Step 3: Under the conditions of an ambient temperature of 25±5°C and an ambient humidity of 35±2%, the spinning solution is passed through an electrospinning machine to form a fiber membrane; the working parameters of the electrospinning machine are: voltage of 18kV, a speed of the receiving device of 40r / min, and a receiving distance of 15cm; the fiber membrane is placed in a vacuum tube sintering furnace, kept warm for 30 minutes under nitrogen protection and 150°C, then heated to 250°C at a rate of 2°C / min, kept warm for 30 minutes, then heated to 340°C at a rate of 2°C / min, kept warm for 45 minutes, and naturally cooled to obtain a zinc oxide-polyimide fiber membrane.
[0035] Step 4: Mix zirconia fibers with a length of 3-6 μm and deionized water, and obtain a zirconia fiber dispersion with a mass fraction of 20% after ultrasonic dispersion for 15 minutes, then add 9 kg of alkaline silica sol with a mass fraction of 25%, 1 kg of boric acid and 2 kg of soluble starch to 50 kg of the zirconia fiber dispersion, stir for 30 minutes and then ultrasonically disperse for 15 minutes to obtain a mixed slurry; pour the mixed slurry into a mold, vacuum filter, and vacuum dry at 80°C to obtain a porous green body, keep the porous green body at 1300°C for 30 minutes, cool naturally, and crush to obtain a flower-shaped zirconia powder.
[0036] Step 5: Mix the flower-shaped zirconia powder and deionized water, and obtain a 5% flower-shaped zirconia dispersion liquid after ultrasonic dispersion for 15 minutes. Then, add 20L of 60% silver nitrate solution, 160L of 4% ammonia water and 0.5L of 5% glucose solution to 80kg of the flower-shaped zirconia dispersion liquid, react at 60±5°C for 25 minutes, filter, wash the filter cake with deionized water 3 times, and dry to obtain silver-loaded zirconia powder.
[0037] Step 6: Add 2 kg of silver-loaded zirconia powder, 9 L of isopropanol and 1 L of water into a reactor, add 1 L of silane coupling agent KH550 after ultrasonic dispersion for 15 min, stir at 25 ° C for 30 min, filter and dry to obtain modified silver-loaded zirconia powder.
[0038] Step 7: Dissolve 5 kg of maleic anhydride grafted polyolefin with 95 kg of xylene by stirring, then add 1.2 kg of modified silver-loaded zirconia powder modified by silane coupling agent, and ultrasonically disperse in a sealed container for 30 minutes to obtain a casting solution, scrape the casting solution flat on a polytetrafluoroethylene plate, and dry to obtain a film.
[0039] Step 8: stack the first layer of zinc oxide-polyimide fiber membrane, the adhesive film and the second layer of zinc oxide-polyimide fiber membrane in sequence, and hot-press and laminate them at 110° C. to obtain a three-layer shielding membrane.
[0040] Step nine: Extrusion-coat the surface of the copper conductor with an insulating layer, then coat the outside of the insulating layer with a shielding film, coat the outside of the shielding film with a mesh conductor, and extrude a rubber sheath on the outside of the mesh conductor to obtain a coaxial copper conductor cable with high electromagnetic shielding efficiency.
[0041] Example 2
[0042] This embodiment provides a coaxial copper conductor cable with high electromagnetic shielding effectiveness, including the following implementation steps:
[0043] A coaxial copper conductor cable with high electromagnetic shielding effectiveness, with a copper conductor at the center and outwardly including an insulating layer, a shielding film, a mesh conductor and a rubber sheath in sequence; wherein the shielding film is prepared by the following steps:
[0044] Step 1: Add 35 kg of nano zinc oxide, 215 L of isopropanol and 25 L of water into a reactor, add 22.5 L of silane coupling agent KH560 after ultrasonic dispersion for 20 minutes, stir at 28°C for 45 minutes, filter and dry to obtain modified nano zinc oxide.
[0045] Step 2: Add 110L N,N-dimethylformamide and 5.5kg of modified nano zinc oxide modified by silane coupling agent into the reactor, ultrasonically disperse for 25 minutes, add 10kg of 4,4'-diaminodiphenyl ether into the reactor at 8°C, stir for 18 minutes at 350r / min, then add 12kg of pyromellitic anhydride into the reactor and continue stirring for 2.5h to obtain the spinning solution.
[0046] Step 3: Under the conditions of an ambient temperature of 25±5°C and an ambient humidity of 35±2%, the spinning solution is passed through an electrospinning machine to form a fiber membrane; the working parameters of the electrospinning machine are: voltage of 18kV, a speed of the receiving device of 40r / min, and a receiving distance of 15cm; the fiber membrane is placed in a vacuum tube sintering furnace, kept warm for 40 minutes under nitrogen protection and 165°C, then heated to 255°C at a rate of 2°C / min, kept warm for 40 minutes, then heated to 345°C at a rate of 2°C / min, kept warm for 50 minutes, and naturally cooled to obtain a zinc oxide-polyimide fiber membrane.
[0047] Step 4: Mix zirconia fibers with a length of 3-6 μm and deionized water, and obtain a zirconia fiber dispersion with a mass fraction of 20% after ultrasonic dispersion for 20 minutes, then add 9 kg of alkaline silica sol with a mass fraction of 25%, 1 kg of boric acid and 2 kg of soluble starch to 50 kg of zirconia fiber dispersion, stir for 40 minutes and then ultrasonically disperse for 20 minutes to obtain a mixed slurry; pour the mixed slurry into a mold, vacuum filter, and vacuum dry at 85°C to obtain a porous green body, keep the porous green body at 1400°C for 40 minutes, cool naturally, and crush to obtain a flower-shaped zirconia powder.
[0048] Step 5: Mix the flower-shaped zirconia powder and deionized water, and obtain a 5% flower-shaped zirconia dispersion liquid after ultrasonic dispersion for 20 minutes. Then, add 20L of 60% silver nitrate solution, 160L of 4% ammonia water and 0.6L of 5% glucose solution to 80kg of the flower-shaped zirconia dispersion liquid, react at 60±5°C for 30 minutes, filter, wash the filter cake with deionized water 4 times, and dry to obtain silver-loaded zirconia powder.
[0049] Step 6: Add 2.25 kg of silver-loaded zirconia powder, 11 L of isopropanol and 1.25 L of water into a reactor, add 1.15 L of silane coupling agent KH560 after ultrasonic dispersion for 20 min, stir at 28 ° C for 45 min, filter and dry to obtain modified silver-loaded zirconia powder.
[0050] Step 7: Dissolve 5.5 kg of maleic anhydride grafted polyolefin with 95 kg of xylene by stirring, then add 1.35 kg of modified silver-loaded zirconium oxide powder modified by silane coupling agent, and ultrasonically disperse in a sealed container for 45 minutes to obtain a casting solution, scrape the casting solution flat on a polytetrafluoroethylene plate, and dry to obtain a film.
[0051] Step 8: stack the first layer of zinc oxide-polyimide fiber membrane, the adhesive film and the second layer of zinc oxide-polyimide fiber membrane in sequence, and hot-press and laminate them at 115° C. to obtain a three-layer shielding membrane.
[0052] Step nine: Extrusion-coat the surface of the copper conductor with an insulating layer, then coat the outside of the insulating layer with a shielding film, coat the outside of the shielding film with a mesh conductor, and extrude a rubber sheath on the outside of the mesh conductor to obtain a coaxial copper conductor cable with high electromagnetic shielding efficiency.
[0053] Example 3
[0054] This embodiment provides a coaxial copper conductor cable with high electromagnetic shielding effectiveness, including the following implementation steps:
[0055] A coaxial copper conductor cable with high electromagnetic shielding effectiveness, with a copper conductor at the center and outwardly including an insulating layer, a shielding film, a mesh conductor and a rubber sheath in sequence; wherein the shielding film is prepared by the following steps:
[0056] Step 1: Add 50 kg of nano zinc oxide, 250 L of isopropanol and 30 L of water into a reactor, add 25 L of silane coupling agent KH570 after ultrasonic dispersion for 30 min, stir at 30 ° C for 60 min, filter and dry to obtain modified nano zinc oxide.
[0057] Step 2: Add 120L N,N-dimethylformamide and 6kg of modified nano zinc oxide modified by silane coupling agent into the reactor, ultrasonically disperse for 30 minutes, add 11.84kg of 4,4'-diaminodiphenyl ether into the reactor at 10°C, stir for 20 minutes at 500r / min, then add 13.03kg of pyromellitic anhydride into the reactor and continue stirring for 3 hours to obtain a spinning solution.
[0058] Step 3: Under the conditions of an ambient temperature of 25±5°C and an ambient humidity of 35±2%, the spinning solution is passed through an electrospinning machine to form a fiber membrane; the working parameters of the electrospinning machine are: voltage of 18kV, a speed of the receiving device of 40r / min, and a receiving distance of 15cm; the fiber membrane is placed in a vacuum tube sintering furnace, kept warm for 45 minutes under nitrogen protection and 180°C, then heated to 260°C at a rate of 2°C / min, kept warm for 45 minutes, then heated to 350°C at a rate of 2°C / min, kept warm for 60 minutes, and naturally cooled to obtain a zinc oxide-polyimide fiber membrane.
[0059] Step 4: Mix zirconia fibers with a length of 3-6 μm and deionized water, and obtain a zirconia fiber dispersion with a mass fraction of 20% after ultrasonic dispersion for 30 minutes, then add 9 kg of alkaline silica sol with a mass fraction of 25%, 1 kg of boric acid and 2 kg of soluble starch to 50 kg of zirconia fiber dispersion, stir for 45 minutes and then ultrasonically disperse for 30 minutes to obtain a mixed slurry; pour the mixed slurry into a mold, vacuum filter, and vacuum dry at 90°C to obtain a porous green body, keep the porous green body at 1450°C for 50 minutes, cool naturally, and crush to obtain a flower-shaped zirconia powder.
[0060] Step 5: Mix the flower-shaped zirconia powder and deionized water, and obtain a 5% flower-shaped zirconia dispersion liquid after ultrasonic dispersion for 30 minutes. Then, add 20L of 60% silver nitrate solution, 160L of 4% ammonia water and 0.8L of 5% glucose solution to 80kg of the flower-shaped zirconia dispersion liquid, react at 60±5°C for 35 minutes, filter, wash the filter cake with deionized water 5 times, and dry to obtain silver-loaded zirconia powder.
[0061] Step 6: Add 2.5 kg of silver-loaded zirconia powder, 12.5 L of isopropanol and 1.5 L of water into a reactor, add 1.25 L of silane coupling agent KH570 after ultrasonic dispersion for 30 min, stir at 30° C. for 60 min, filter and dry to obtain modified silver-loaded zirconia powder.
[0062] Step 7: Dissolve 6 kg of maleic anhydride grafted polyolefin with 95 kg of xylene by stirring, then add 1.5 kg of modified silver-loaded zirconia powder modified by silane coupling agent, and ultrasonically disperse in a sealed container for 60 minutes to obtain a casting solution, scrape the casting solution flat on a polytetrafluoroethylene plate, and dry to obtain a film.
[0063] Step 8: stack the first layer of zinc oxide-polyimide fiber membrane, the adhesive film and the second layer of zinc oxide-polyimide fiber membrane in sequence, and hot-press and laminate them at 120° C. to obtain a three-layer shielding membrane.
[0064] Step nine: Extrusion-coat the surface of the copper conductor with an insulating layer, then coat the outside of the insulating layer with a shielding film, coat the outside of the shielding film with a mesh conductor, and extrude a rubber sheath on the outside of the mesh conductor to obtain a coaxial copper conductor cable with high electromagnetic shielding efficiency.
[0065] Comparative Example 1: Based on Example 3, zinc oxide-polyimide fiber film is directly used as the shielding film, and the other steps remain unchanged to prepare a coaxial copper conductor cable.
[0066] Comparative Example 2: Based on Example 3, the modified silver-loaded zirconia powder in step 7 was directly replaced with the silver powder of the same proportion and mass, and the other steps remained unchanged to prepare a coaxial copper conductor cable.
[0067] Performance tests were performed on Examples 1 to 3 and Comparative Examples 1 to 2. For uniform testing, the thickness of the shielding films used was 0.1 mm. The shielding efficiency of different coaxial copper conductor cables was tested. The results are shown in Table 1:
[0068] Table 1
[0069]
[0070] It can be seen from Table 1 that the coaxial copper conductor cables in Examples 1 to 3 have higher electromagnetic shielding effectiveness.
[0071] It should be noted that, in this article, terms such as "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.
[0072] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A coaxial copper conductor cable with high electromagnetic shielding effectiveness, characterized in that: The center is a copper conductor, and outwards it includes an insulating layer, a shielding film, a mesh conductor and a rubber sheath; The shielding film is prepared by the following steps: Step 1: Mix the flower-shaped zirconium oxide powder and deionized water, and ultrasonically disperse them into a 5wt% flower-shaped zirconium oxide dispersion, then add 60wt% silver nitrate solution, 4wt% ammonia water and 5wt% glucose solution, react at 60±5℃ for 25-35min, filter, wash and dry to obtain silver-loaded zirconium oxide powder; Step 2: dissolving the maleic anhydride grafted polyolefin with xylene by stirring, then adding the modified silver-loaded zirconium oxide powder modified by the silane coupling agent, and ultrasonically dispersing it in a closed container for 30-60 minutes to obtain a casting solution, and then scraping the casting solution on a polytetrafluoroethylene plate and drying it to obtain a film; Step 3: stacking the first layer of zinc oxide-polyimide fiber film, the adhesive film and the second layer of zinc oxide-polyimide fiber film in sequence, and hot pressing and compounding them at 110-120° C. to obtain a three-layer shielding film; The thickness ratio of the single-layer zinc oxide-polyimide fiber film to the adhesive film is 2:1; The flower-shaped zirconium oxide powder is prepared by the following steps: Zirconia fibers with a length of 3-6 μm are mixed with deionized water, and ultrasonically dispersed into a 20wt% zirconia fiber dispersion. 25wt% alkaline silica sol, boric acid and soluble starch are added, stirred for 30-45 minutes, and then ultrasonically dispersed for 15-30 minutes. After the mixed slurry is obtained, it is poured into a mold, vacuum filtered, and vacuum dried at 80-90°C. After obtaining a porous green body, it is kept warm at 1300-1450°C for 30-50 minutes, naturally cooled, and crushed to obtain a flower-shaped zirconia powder.
2. A coaxial copper conductor cable with high electromagnetic shielding effectiveness according to claim 1, characterized in that: The dosage ratio of the flower-shaped zirconium oxide dispersion, the silver nitrate solution, the ammonia water and the glucose solution is 80 g: 20 mL: 160 mL: 0.5-0.8 mL.
3. The coaxial copper conductor cable with high electromagnetic shielding effectiveness according to claim 1, characterized in that: The usage ratio of the maleic anhydride grafted polyolefin, xylene and modified silver-loaded zirconium oxide powder is 5-6g:95g:1.2-1.5g.
4. The coaxial copper conductor cable with high electromagnetic shielding effectiveness according to claim 1, characterized in that: The usage ratio of the zirconium oxide fiber dispersion, alkaline silica sol, boric acid and soluble starch is 50g:9g:1g:2g.
5. The coaxial copper conductor cable with high electromagnetic shielding effectiveness according to claim 1, characterized in that: The zinc oxide-polyimide fiber membrane is prepared by the following steps: Step 1: Add the modified nano zinc oxide modified by N,N-dimethylformamide and silane coupling agent into the reactor, ultrasonically disperse for 20-30 minutes, add 4,4'-diaminodiphenyl ether at 5-10°C, stir at 200-500r / min for 15-20 minutes, then add pyromellitic anhydride and continue stirring for 2-3 hours to obtain a spinning solution, and use an electrostatic spinning machine to form a fiber membrane; Step 2: Keep the fiber membrane at 150-180°C for 30-45 minutes under nitrogen protection, increase the temperature to 250-260°C at a rate of 2°C / min, keep it for 30-45 minutes, increase the temperature to 340-350°C at a rate of 2°C / min, keep it for 45-60 minutes, and cool naturally to obtain a zinc oxide-polyimide fiber membrane.
6. A coaxial copper conductor cable with high electromagnetic shielding effectiveness according to claim 5, characterized in that: The dosage ratio of N,N-dimethylformamide, modified nano zinc oxide, 4,4'-diaminodiphenyl ether and pyromellitic anhydride is 100-120 mL: 5-6 g: 9.87-11.84g:10.85-13.03g.
7. The coaxial copper conductor cable with high electromagnetic shielding effectiveness according to claim 5, characterized in that: The working parameters of the electrostatic spinning machine are: voltage of 18 kV, speed of the receiving device of 40 r / min, and receiving distance of 15 cm.
8. The coaxial copper conductor cable with high electromagnetic shielding effectiveness according to claim 1, characterized in that: The specific method of modifying the silver-loaded zirconium oxide powder by a silane coupling agent is as follows: Silver-loaded zirconium oxide powder, isopropanol and water are added into a reaction kettle, and a silane coupling agent is added after ultrasonic dispersion for 15-30 minutes, and the mixture is stirred at 25-30° C. for 30-60 minutes, filtered and dried to obtain modified silver-loaded zirconium oxide powder; the dosage ratio of the silver-loaded zirconium oxide powder, isopropanol, water and silane coupling agent is 4-5 g: 18-25 mL: 2-3 mL: 2-2.5 mL.
9. The method for preparing a coaxial copper conductor cable with high electromagnetic shielding effectiveness according to claim 1, characterized in that: The steps include: An insulating layer is extruded and coated on the surface of the copper conductor, a shielding film is then coated on the outside of the insulating layer, a mesh conductor is coated on the outside of the shielding film, and a rubber sheath is extruded and coated on the outside of the mesh conductor to obtain a coaxial copper conductor cable with high electromagnetic shielding efficiency.
Citation Information
Patent Citations
Airborne early warning radar low-loss stable-phase cable and preparation method thereof
CN112164497A
Broadband cable with good shielding effect and processing technology thereof
CN115482957A
Silicon PU composite material for plastic track and preparation method of silicon PU composite material
CN116769303A
High-performance bending-resistant coaxial cable and preparation method thereof
CN116936180A
Coaxial cable, manufacturing device of the coaxial cable, and manufacturing method of the coaxial cable
JP2005093369A