Secondary batteries and electrical devices

By adding specific hydrophobic agents and insulating materials to the insulating layer, the problem of impurities easily adhering to the surface layer of the power battery during transportation is solved, achieving excellent hydrophobic and thermal conductivity of the insulating layer, extending battery life and improving the battery's self-cleaning ability and thermal management efficiency.

CN117352924BActive Publication Date: 2026-11-10SUNWODA MOBILITY ENERGY TECHNOLOGY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311394340.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-25
Publication Date
2026-11-10
Estimated Expiration
2043-10-25

AI Technical Summary

Technical Problem

The insulating layer of the aluminum alloy surface layer of the power battery is prone to being contaminated with impurities and dirt during transportation, which affects its durability. Existing technologies are unable to effectively improve the hydrophobicity of the insulating layer to improve its self-cleaning ability.

Method used

Hydrophobic agents such as silicon boride, calcium boride, magnesium boride, barium boride, tungsten boride, titanium boride, and B-Si-Zr ternary materials are added to the insulating layer, combined with a specific ratio of prepolymer, photoinitiator, and reactive diluent, to form an insulating layer with excellent hydrophobic properties. The hydrophobic properties are characterized by controlling the contact angle and dyne ratio of the insulating layer.

Benefits of technology

The hydrophobic properties of the insulation layer were improved, reducing the risk of battery contamination during use and extending battery life. Furthermore, by optimizing the thickness of the insulation layer and the proportion of thermally conductive materials, the thermal conductivity and high-temperature resistance of the insulation layer were enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117352924B_ABST
    Figure CN117352924B_ABST
Patent Text Reader

Abstract

This invention discloses a secondary battery and its power supply device, belonging to the field of battery technology. It includes a casing, a cover plate, and an electrode assembly. The casing has a receiving cavity and an opening, which are connected. The electrode assembly is housed within the receiving cavity, and the cover plate closes the opening. The casing includes an outer surface away from the receiving cavity and an insulating layer disposed on the outer surface. The insulating layer includes an insulating material and a hydrophobic agent. The hydrophobic agent is at least partially disposed in the insulating material. The hydrophobic agent includes at least one of silicon boride, calcium boride, magnesium boride, barium boride, tungsten boride, titanium boride, and B-Si-Zr ternary materials. The contact angle of the insulating layer relative to a water solvent is α°, and the dyne value is Xdyn / cm, satisfying: H≥3, H=α / X. The insulating layer has excellent hydrophobic properties, reducing the risk of battery contamination during use and improving battery life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of battery technology, and more specifically to a secondary battery and an electrical device. Background Technology

[0002] With the rapid development of the new energy power battery industry, the requirements for battery surface technology are becoming increasingly stringent, and the technology of aluminum alloy surface layer for power batteries has begun to develop in the industry.

[0003] Typically, after an insulating layer is applied to the surface of the aluminum alloy of a power battery, there is a transfer process before assembly. During the transfer process, impurities and dirt easily adhere to the insulating layer on the surface of the battery casing, affecting the durability of the insulating layer. This application improves the self-cleaning ability of the aluminum alloy surface layer of the power battery by enhancing the hydrophobicity of the insulating layer.

[0004] Application content

[0005] The purpose of this application is to overcome the shortcomings of the existing technology and provide a secondary battery and power device. The secondary battery of this application has an insulating layer with excellent hydrophobic properties, which reduces the risk of battery contamination during use and improves battery life.

[0006] To achieve the above objectives, in a first aspect of this application, a secondary battery is provided, including a casing, a cover plate, and an electrode assembly. The casing has a receiving cavity and an opening, the receiving cavity and the opening being in communication. The electrode assembly is received within the receiving cavity, and the cover plate covers the opening. The casing includes an outer surface away from the receiving cavity and an insulating layer disposed on the outer surface. The insulating layer includes an insulating material and a hydrophobic agent. The hydrophobic agent is at least partially disposed in the insulating material. The hydrophobic agent includes at least one of silicon boride, calcium boride, magnesium boride, barium boride, tungsten boride, titanium boride, and B-Si-Zr ternary materials.

[0007] The contact angle of the insulating layer with respect to the water solvent is α°, and the dyn value is Xdyn / cm, satisfying: H≥3, H=α / X.

[0008] As an embodiment of this application, the contact angle ranges from 91° to 150°, and the dyne value ranges from 22 to 50 dyn / cm.

[0009] As an embodiment of this application, the insulating material includes a prepolymer, a photoinitiator, and an active diluent;

[0010] Based on the total mass of the insulating layer, the mass percentage of the prepolymer is 10%-50%, the mass percentage of the photoinitiator is 2%-8%, the mass percentage of the reactive diluent is 40%-80%, and the mass percentage of the hydrophobic agent is 1%-5%.

[0011] As an embodiment of this application, the content of the hydrophobic agent satisfies one of the following relationships:

[0012] Relationship 1: The hydrophobic agent includes silicon boride and calcium boride, and the mass ratio of silicon boride to calcium boride is 1:(1-4);

[0013] Relationship 2: The hydrophobic agent includes silicon boride and B-Si-Zr ternary material, and the mass ratio of silicon boride to B-Si-Zr ternary material is 1:(1-4);

[0014] Relationship 3: The hydrophobic agent includes B-Si-Zr ternary material and calcium boride, and the mass ratio of B-Si-Zr ternary material to calcium boride is 1:(1-4);

[0015] Relationship 4: The hydrophobic agent includes silicon boride, calcium boride and B-Si-Zr ternary material, and the mass ratio of silicon boride, calcium boride and B-Si-Zr ternary material is (1-4):(1-4):1.

[0016] As an embodiment of this application, the average particle size of the hydrophobic agent is 20-200 nm.

[0017] As an embodiment of this application, the insulating layer further includes a thermally conductive material, and based on the total mass of the insulating layer, the mass percentage of the prepolymer is A%, the mass percentage of the thermally conductive material is B%, the mass percentage of the hydrophobic agent in the insulating layer is D%, and the thickness of the insulating layer is C μm;

[0018] The insulating layer satisfies the following relationship: 0.0010≤(A+2B+D) / C≤0.0080.

[0019] As an embodiment of this application, the prepolymer includes at least one of polyimide resin, phenolic resin, and silicone resin.

[0020] As an embodiment of this application, the thermally conductive material includes at least one of boron nitride, silicon nitride, gallium nitride, gallium arsenide, gallium phosphide, zinc oxide, indium phosphide, beryllium oxide, magnesium oxide, and magnesium silicon nitride.

[0021] As an embodiment of this application, B% ranges from 1% to 5%.

[0022] As an embodiment of this application, the range of Cμm is 85-150μm.

[0023] As an embodiment of this application, the leakage current of the insulating layer is ≤15μA.

[0024] As an embodiment of this application, the insulation resistance of the insulating layer is >11 Gohm.

[0025] In a second aspect, this application provides an electrical device including the aforementioned secondary battery.

[0026] The beneficial effects of this application are as follows: (1) This application adds at least one of silicon boride, calcium boride, magnesium boride, barium boride, tungsten boride, titanium boride, and B-Si-Zr ternary materials to the insulating material. The borides have high bond energy, which makes the formed surface layer have low surface energy and makes the H value of the insulating layer ≥3, thereby giving the insulating layer excellent hydrophobic properties, reducing the risk of battery contamination during use, and improving battery life. This application uses the ratio of the contact angle to the dyne value of the insulating layer as a characterization method of the hydrophobic properties of the insulating layer. By using the dyne value as the denominator, it can play a certain compensating role for the hydrophobicity of the insulating layer, and its H value can more accurately reflect the hydrophobic properties of the insulating layer.

[0027] (2) Based on the thickness of the insulating layer, this application adjusts the mass percentage of high-temperature resistant resin, the mass percentage of thermally conductive material, and the mass percentage of hydrophobic agent to satisfy the following relationship: 0.0010≤(A+2B+D) / C≤0.0080, which can ensure the hydrophobic performance of the insulating layer within the corresponding thickness range, thereby optimizing the hydrophobic performance. At the same time, it makes the insulating layer have better thermal conductivity, which is conducive to transferring the heat generated by the battery to the cooling system and thus facilitating battery cooling. Attached Figure Description

[0028] Figure 1 This is a schematic diagram of the structure of a secondary battery according to one embodiment of this application.

[0029] Figure 2 This is a schematic diagram of the exploded structure of a secondary battery according to one embodiment of this application. Detailed Implementation

[0030] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions in the embodiments of this application will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments in this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.

[0031] In this application, the technical features described in an open-ended manner include both closed technical solutions composed of the listed features and open technical solutions composed of the listed features.

[0032] In this application, numerical ranges are referred to as continuous unless otherwise specified, and include the minimum and maximum values ​​of the range, as well as every value between the minimum and maximum values. Furthermore, when the range refers to integers, it includes every integer between the minimum and maximum values ​​of the range. Additionally, when multiple ranges are provided to describe a feature or characteristic, the ranges may be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges to which they are incorporated.

[0033] Unless otherwise specified, all reagents or instruments used in this application are commercially available products.

[0034] like Figures 1-2 As shown in the figure, this application provides a secondary battery, including a housing 1, a cover plate 2 and an electrode assembly. The housing 1 is provided with a receiving cavity 11 and an opening. The receiving cavity 11 and the opening are connected. The electrode assembly is housed in the receiving cavity 11, and the cover plate 2 covers the opening.

[0035] The outer casing 1 includes an outer surface away from the receiving cavity 11 and an insulating layer 3 disposed on the outer surface. The insulating layer 3 includes an insulating material and a hydrophobic agent, wherein the hydrophobic agent is at least partially disposed in the insulating material. Optionally, the hydrophobic agent and the insulating material are mixed and dispersed in the insulating material. The hydrophobic agent includes at least one selected from silicon boride, calcium boride, magnesium boride, barium boride, tungsten boride, titanium boride, and B-Si-Zr ternary materials.

[0036] The contact angle of the insulating layer with respect to the water solvent is α°, and the dyn value is Xdyn / cm, satisfying: H≥3, H=α / X. Optionally, in some specific embodiments, 3≤H≤7. The value of H can also be one of 4, 4.5, 5, 5.5, 6, 6.5 or any combination of two.

[0037] This application incorporates at least one of the following materials into the insulating material: silicon boride, calcium boride, magnesium boride, barium boride, tungsten boride, titanium boride, and a B-Si-Zr ternary material. The high bond energy of the borides results in a low surface energy for the formed surface layer, leading to an H value ≥ 3 for the insulating layer 3. This provides excellent hydrophobic properties to the insulating layer 3, making it less susceptible to contamination by impurities during battery transport and improving battery life. It should be noted that, based on the selection of the type and content of the insulating material and hydrophobic agent, as well as considerations of the ease of the preparation process, the H value is typically in the range of 3 ≤ H ≤ 7.

[0038] Based on the principle that using borides as hydrophobic agents can effectively optimize the hydrophobic properties of the battery surface, this application further characterizes the hydrophobic properties of the insulating layer 3 by using the ratio of its contact angle to its dyne value. The H value more accurately reflects the hydrophobic properties of the insulating layer 3. When H ≥ 3.0, the hydrophobic properties of the insulating layer 3 reach an optimal state, and the surface impurities and contamination issues of the insulating layer 3 are significantly improved during battery transportation.

[0039] In this application, the contact angle of the insulating layer 3 relative to the water solvent is measured using a contact angle measuring instrument according to the measurement method of GB / T 30693-2014. Specifically, the secondary battery is placed on the sample stage of the instrument with the insulating layer 3 of the secondary battery facing upward. A 1μL-2μL water droplet is suspended at the end of the needle. The sample stage is raised so that the surface of the battery contacts the suspended water droplet. Then the battery is removed to complete the transfer of the water droplet. The contact angle is measured within 60s±10s after the water droplet transfer. The pointer of the contact angle measuring instrument is adjusted so that it is tangent to the water droplet on the surface of the insulating layer 3, thereby obtaining its contact angle.

[0040] In this application, the dyne value test method for the insulating layer 3 is as follows: the test refers to the DIN ISO 8296 test method, and a dyne pen mixture solution with gradually increasing surface tension (22dyn / cm-50dyn / cm) is applied to the surface of the insulating layer 3 of the secondary battery until the dyne pen mixture solution just wets the surface of the insulating layer 3. The dyne value obtained at this time is the dyne value of the insulating layer 3.

[0041] It should be noted that the B-Si-Zr ternary material includes B2O3, SiO2, and ZrO2, and the mass ratio of B2O3, SiO2, and ZrO2 is (1-3):(1-3):1.

[0042] The B-Si-Zr ternary material is a composite material obtained by uniformly mixing B2O3, SiO2, and ZrO2 and then subjecting it to conventional heat treatment (heat treatment temperature can be 1000-1800℃, and time can be 0.5-5h).

[0043] In some embodiments, the contact angle ranges from 91° to 150°, and the dyne value ranges from 22 to 50 dyn / cm.

[0044] The contact angle ranges from 91° to 150°, for example, it can be 91°, 95°, 100°, 110°, 120°, 130°, 140°, 150° or any two of these values.

[0045] The range of dyn values ​​is 22-50 dyn / cm, for example, it can be 22 dyn / cm, 26 dyn / cm, 30 dyn / cm, 34 dyn / cm, 36 dyn / cm, 40 dyn / cm, 44 dyn / cm, 48 dyn / cm, 50 dyn / cm or any two of these values.

[0046] In some embodiments, the insulating material of the insulating layer 3 includes a prepolymer, a photoinitiator, and an active diluent;

[0047] Based on the total mass of the insulating layer 3, the mass percentage of the prepolymer is 10%-50%, for example, it can be 10%, 15%, 20%, 25%, 30%, 35%, 40%, 50%, or any two of these values.

[0048] Based on the total mass of the insulating layer 3, the mass percentage of the active diluent is 40%-80%, for example, it can be 40%, 50%, 60%, 70%, 80% or any two of these values.

[0049] Based on the total mass of the insulating layer 3, the mass percentage of the photoinitiator is 2%-8%, for example, it can be 2%, 3%, 4%, 5%, 6%, 7%, 8% or any two of these values.

[0050] Based on the total mass of the insulating layer 3, the mass percentage of the hydrophobic agent is 1%-5%, for example, it can be 1%, 2%, 3%, 4%, 5%, or any two of these values.

[0051] The insulating material of the insulating layer 3 of this application uses a reaction mixture of prepolymer, photoinitiator and reactive diluent with a specific mass percentage, so that the hydrophobic agent can be uniformly dispersed in the insulating material of the insulating layer 3, thereby giving full play to its role, improving the hydrophobic effect of the insulating layer 3, and at the same time giving the insulating layer 3 excellent pressure resistance, adhesion and corrosion resistance.

[0052] In some embodiments, the content of the hydrophobic agent satisfies one of the following relationships:

[0053] Relationship 1: The hydrophobic agent includes silicon boride and calcium boride, and the mass ratio of silicon boride to calcium boride is 1:(1-4);

[0054] Relationship 2: The hydrophobic agent includes silicon boride and B-Si-Zr ternary material, and the mass ratio of silicon boride to B-Si-Zr ternary material is 1:(1-4);

[0055] Relationship 3: The hydrophobic agent includes B-Si-Zr ternary material and calcium boride, and the mass ratio of B-Si-Zr ternary material to calcium boride is 1:(1-4);

[0056] Relationship 4: The hydrophobic agent includes silicon boride, calcium boride and B-Si-Zr ternary material, and the mass ratio of silicon boride, calcium boride and B-Si-Zr ternary material is (1-4):(1-4):1.

[0057] The inventors of this application have discovered through extensive research that when hydrophobic agents based on the aforementioned formulas 1-4 are used, the bonds formed between boron and silicon / calcium in formula 1 have high bond energies, the bonds formed between boron and silicon / zirconium in formula 2 have high bond energies, and the bonds formed between boron and silicon / zirconium / calcium in formulas 3-4 have high bond energies. This results in a lower surface energy on the surface of the insulating layer 3. Therefore, adding such substances further improves the hydrophobicity of the insulating layer 3, further enhancing its hydrophobic properties and increasing its H value. Furthermore, the inventors have found that when two or more borides based on formulas 1-4 are combined, they exhibit a significant synergistic effect in improving hydrophobicity. Compared to using a single boride, this further reduces the surface energy of the insulating layer 3, significantly improving the hydrophobic effect.

[0058] In some embodiments, the average particle size of the hydrophobic agent is 20-200 nm, for example, it can be 20 nm, 30 nm, 50 nm, 80 nm, 100 nm, 120 nm, 150 nm, 180 nm, 200 nm or any two of these values. When the average particle size of the hydrophobic agent is within this range, the hydrophobic agent can be uniformly dispersed in the insulating material of the insulating layer 3 to form a superhydrophobic structure, thereby effectively improving the hydrophobic performance.

[0059] In this application, the average particle size is the average value of the particle size distribution measured by a laser diffraction particle size distribution measuring instrument according to the particle size distribution laser diffraction method (specifically refer to GB / T19077-2016).

[0060] In some embodiments, the insulating layer 3 further includes a thermally conductive material, wherein, based on the total mass of the insulating layer 3, the mass percentage of the prepolymer is A%, the mass percentage of the thermally conductive material is B%, the mass percentage of the hydrophobic agent in the insulating layer 3 is D%, and the thickness of the insulating layer is C μm;

[0061] The insulating layer 3 satisfies the following relationship: 0.0010≤(A+2B+D) / C≤0.0080.

[0062] The inventors of this application have discovered through extensive research that the hydrophobicity, pressure resistance, high temperature resistance, and thermal conductivity of the insulating layer 3 are significantly correlated with the mass percentage of prepolymer, thermally conductive material, and hydrophobic agent in the insulating layer 3, as well as the thickness of the insulating layer 3. This application significantly improves the hydrophobicity of the insulating layer 3 by controlling the mass percentage of prepolymer, thermally conductive material, hydrophobic agent, and the thickness of the insulating layer 3 to satisfy the following relationship: 0.0010≤(A+2B+D) / C≤0.0080. This allows the thermally conductive material and hydrophobic agent to penetrate and disperse in the reactants of resin, initiator, and reactive diluent, forming a superhydrophobic structure. This not only improves the hydrophobicity of the insulating layer 3 but also enhances its pressure resistance, high temperature resistance, and thermal conductivity.

[0063] In some embodiments, the prepolymer includes at least one of polyimide resin, phenolic resin, and silicone resin.

[0064] In some embodiments, the thermally conductive material includes at least one of boron nitride, silicon nitride, gallium nitride, gallium arsenide, gallium phosphide, zinc oxide, indium phosphide, beryllium oxide, magnesium oxide, and magnesium silicon nitride, wherein B% ranges from 1% to 5%, for example, it can be 1%, 2%, 3%, 4%, 5%, or any two of these values.

[0065] In some embodiments, the range of Cμm is 85-150μm, for example, it can be 85μm, 90μm, 100μm, 120μm, 140μm, 150μm or any two of these values.

[0066] In some embodiments, the leakage current of the insulating layer 3 is ≤15μA, which makes the battery safer and avoids the risk of leakage or short circuit.

[0067] In some embodiments, the insulation resistance of the insulating layer 3 is >11 Gohm, the insulation performance of the battery reaches a superior level, it has high withstand voltage performance, and the safety of battery use is guaranteed.

[0068] In some embodiments, the reactive diluent includes at least one of benzyl acrylate, phenoxyethyl acrylate, and 1,6-hexanediol diacrylate.

[0069] In some embodiments, the photoinitiator includes at least one of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide and 1-hydroxycyclohexylphenyl ketone.

[0070] In some embodiments, the insulating layer 3 may further include pigments and additives.

[0071] When the insulating layer 3 includes pigment, the pigment mass percentage is 0.1-5% based on the total mass of the insulating layer 3, for example, it can be 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5% or any two of these values.

[0072] When the insulating layer 3 includes a pigment, suitable pigments include, but are not limited to, phthalocyanine blue, indigo anthrone, and combinations thereof.

[0073] When the insulating layer 3 includes additives, the mass percentage of the additives is 0.1-5% based on the total mass of the insulating layer 3, for example, it can be 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5% or any two of these values.

[0074] When the insulating layer 3 includes additives, suitable additives include, but are not limited to, defoamers, leveling agents, dispersants, and combinations thereof.

[0075] It should be noted that this application does not limit the preparation method of the insulating layer 3. Those skilled in the art can prepare the insulating layer 3 according to conventional methods and the method disclosed in this application.

[0076] For example, the method for preparing the insulating layer 3 is as follows:

[0077] (1) Mix the raw materials of the insulating material and the hydrophobic agent evenly to obtain a mixture;

[0078] (2) The outer surface of the secondary battery is sandblasted, and the mixture is sprayed onto the outer surface of the secondary battery using a UV spraying device. It is then cured by ultraviolet light (350-400nm) and left to stand for 24 hours to obtain the insulating layer 3.

[0079] One embodiment of this application provides an electrical device including the secondary battery described above.

[0080] For example, the aforementioned electrical devices may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto.

[0081] The present application is further illustrated below with specific embodiments:

[0082] Examples 1-28, Comparative Example 1

[0083] The insulating layer 3 of the secondary battery in the embodiments and comparative examples of this application is prepared by a method including the following steps:

[0084] Polyimide resin, thermally conductive material, hydrophobic agent, 5% 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, and the balance phenoxyethyl acrylate were mixed evenly. The outer surface of the secondary battery was sandblasted. The mixture was then sprayed onto the outer surface of the secondary battery using a UV spraying device, cured with ultraviolet light (380nm), and left to stand for 24 hours to obtain insulating layer 3.

[0085] The B-Si-Zr ternary material used in the embodiments includes B2O3, SiO2, and ZrO2, and the mass ratio of B2O3, SiO2, and ZrO2 is 3:1:1.

[0086] The content of polyimide resin, the type and content of thermally conductive material, and the content and type of hydrophobic agent in the insulating layer 3 of the examples and comparative examples are shown in Table 1 (all percentages in the table are by mass).

[0087] Table 1

[0088]

[0089]

[0090] Performance testing

[0091] 1. Hydrophobicity (H value, the larger the H value, the better the hydrophobicity), H = α / X, where α° is the contact angle of the insulating layer 3 relative to the water solvent, and Xdyn / cm is the dyn value of the insulating layer 3.

[0092] 2. High temperature resistance test: The secondary battery was stored at 120℃ for 12 hours. After storage, the leakage current was tested under DC 3150V conditions.

[0093] 3. Insulation withstand voltage test: Using Chroma insulation withstand voltage test equipment, at DC 3150V, test time 5s, leakage current ≤15μA, and at DC 1000V, perform insulation resistance test, which is qualified if greater than 11Gohm.

[0094] 4. Neutral salt spray test, using GB / T 10125-2021 test standard, is considered qualified if no deformation, shrinkage, bubbling, or cracking occurs after 15-12 hours.

[0095] Table 2

[0096]

[0097] As shown in Table 1, the insulating layer 3 of the secondary battery described in this application has excellent hydrophobic properties, which makes the battery less susceptible to contamination by impurities during transportation. At the same time, it ensures that the insulating layer 3 has excellent pressure resistance, high temperature resistance and corrosion resistance, thereby improving the battery's service life. It also has good thermal conductivity, which helps to transfer the heat generated by the battery during operation to the cooling system.

[0098] Comparing Examples 1-11 and Comparative Example 1, it can be seen that by adding a hydrophobic agent to the insulating layer 3, the hydrophobic properties of Examples 1-11 are all greater than 3, while the hydrophobic value of Comparative Example 1 is 2, which is significantly lower than 3. In addition, looking at the contact angle alone, we found that the contact angle of Comparative Example 1 is 89.8°, which is at the boundary between hydrophobic and hydrophilic as we normally understand it. Compared with the change in H value, the contact angle alone is not conducive to evaluating the hydrophobicity of the insulating layer 3.

[0099] Comparing Examples 1-3, Examples 12-14, and Examples 17, 20, and 21, where Examples 1-3 added a single hydrophobic agent at a dosage of 2%, Examples 12-14 added a single hydrophobic agent at a dosage of 4%, and Examples 17, 20, and 21 added any two hydrophobic agents from silicon boride, calcium boride, and B-Si-Zr ternary materials, respectively, with the dosage of hydrophobic agents being the same as in Examples 12-14 (all 4%), the data show that when any two hydrophobic agents from silicon boride, calcium boride, and B-Si-Zr ternary materials are used, they have a synergistic effect in improving hydrophobic performance, which is superior to the hydrophobic performance of adding a single hydrophobic agent.

[0100] Comparing Examples 1-22 with Examples 23-28, it can be seen that by adding thermally conductive materials and controlling the ratio of 0.0010≤(A+2B+D) / C≤0.0080, the hydrophobicity, pressure resistance, high temperature resistance, and thermal conductivity of the insulating layer 3 are improved.

[0101] Comparing Examples 29-30, it can be seen that if (A+2B+D) / C is not within the scope of this application, the hydrophobicity still meets the requirements.

[0102] As can be seen from the comparison of Examples 31-32, when the contact angle of the insulating layer is outside the set range and the dyne value is also outside the set range, the hydrophobicity still meets the requirements.

[0103] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this application and are not intended to limit the scope of protection of this application. Although this application has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of this application without departing from the substance and scope of the technical solutions of this application.

Claims

1. A secondary battery, comprising a casing, a cover plate, and an electrode assembly, wherein the casing has a receiving cavity and an opening, the receiving cavity and the opening are in communication, the electrode assembly is received within the receiving cavity, the cover plate covers the opening, and the casing includes an outer surface remote from the receiving cavity, characterized in that, The outer surface is provided with an insulating layer, the insulating layer comprising an insulating material and a hydrophobic agent, wherein the hydrophobic agent is at least partially disposed in the insulating material; The content of the hydrophobic agent satisfies one of the following relationships: Relationship 1: The hydrophobic agent includes silicon boride and calcium boride, and the mass ratio of silicon boride to calcium boride is 1:(1-4). Relationship 2: The hydrophobic agent includes silicon boride and B–Si–Zr ternary material, and the mass ratio of silicon boride to B–Si–Zr ternary material is 1:(1-4). Relationship 3: The hydrophobic agent includes a B–Si–Zr ternary material and calcium boride, wherein the mass ratio of the B–Si–Zr ternary material to calcium boride is 1:(1-4). Relationship 4: The hydrophobic agent comprises silicon boride, calcium boride, and a B-Si-Zr ternary material, wherein the mass ratio of the silicon boride, calcium boride, and B-Si-Zr ternary material is (1-4):(1-4):

1. The contact angle of the insulating layer with water is α°, and the dyn value is Xdyn / cm, satisfying: 3≤H≤7, H=α / X.

2. The secondary battery according to claim 1, characterized in that, The contact angle ranges from 91° to 150°, and the dyne value ranges from 22 to 50 dyn / cm.

3. The secondary battery according to claim 1, characterized in that, The insulating material includes a prepolymer, a photoinitiator, and an active diluent; Based on the total mass of the insulating layer, the mass percentage of the prepolymer is 10%-50%, the mass percentage of the photoinitiator is 2%-8%, the mass percentage of the reactive diluent is 40%-80%, and the mass percentage of the hydrophobic agent is 1%-5%.

4. The secondary battery according to claim 3, characterized in that, The insulating layer also includes a thermally conductive material. Based on the total mass of the insulating layer, the mass percentage of the prepolymer is A%, the mass percentage of the thermally conductive material is B%, the mass percentage of the hydrophobic agent in the insulating layer is D%, and the thickness of the insulating layer is C μm. The insulating layer satisfies the following relationship: 0.0010 ≤ (A+2B+D) / C ≤ 0.0080.

5. The secondary battery according to claim 4, characterized in that, The prepolymer includes at least one of polyimide resin, phenolic resin, and silicone resin.

6. The secondary battery according to claim 4, characterized in that, The thermally conductive material includes at least one of boron nitride, silicon nitride, gallium nitride, gallium arsenide, gallium phosphide, zinc oxide, indium phosphide, beryllium oxide, magnesium oxide, and magnesium silicon nitride.

7. The secondary battery according to claim 4, characterized in that, The mass percentage (B%) of the thermally conductive material ranges from 1% to 5%.

8. The secondary battery according to claim 4, characterized in that, The thickness Cμm of the insulating layer ranges from 85 to 150μm.

9. The secondary battery according to claim 1, characterized in that, The average particle size of the hydrophobic agent is 20-200 nm.

10. The secondary battery according to claim 1, characterized in that, The leakage current of the insulating layer is ≤15μA.

11. The secondary battery according to claim 1, characterized in that, The insulation resistance of the insulating layer is >11 Gohm.

12. An electrical appliance, characterized in that, Includes the secondary battery as described in any one of claims 1-11.

Citation Information

Patent Citations

  • Fluorine-containing silane / titanium boride modified wear-resistant hydrophobic flame-retardant silicone rubber and preparation method thereof

    CN114276683A

  • Insulating spraying battery shell

    CN114914592A