A high-temperature resistant sintered NdFeB magnet, its preparation method and application
By adjusting the composition and preparation process of sintered NdFeB magnets, controlling the difference in thermal expansion coefficients, and combining grain boundary diffusion technology, the problem of high-temperature demagnetization of permanent magnet materials was solved, and the coercivity at high temperatures was improved.
Patent Information
- Application Number
- CN202311275411.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-28
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-09-28
AI Technical Summary
Existing permanent magnet materials are prone to demagnetization at high temperatures, leading to reduced performance. Current methods for improving coercivity mostly use heavy rare earth elements, which are costly.
By adjusting the composition and preparation process of sintered NdFeB magnets, the difference in their thermal expansion coefficients in different directions is controlled. Combined with grain boundary diffusion technology, the high-temperature stability of the magnets is improved by using less heavy rare earth elements.
It effectively improves the coercivity of sintered NdFeB magnets at high temperatures, reduces the formation of demagnetizing fields, and enhances high-temperature performance.
Smart Images

Figure CN117457308B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of NdFeB-based sintered magnet technology, specifically to a high-temperature resistant sintered NdFeB magnet, its preparation method, and its application. Background Technology
[0002] Since their invention, sintered permanent magnet materials have been rapidly adopted in numerous fields such as electronics, energy, communications, and machinery due to their excellent magnetic properties and high cost-effectiveness. In recent years, permanent magnet materials have been increasingly used in the automotive industry. However, automotive motors generate high temperatures during operation, and permanent magnet materials can demagnetize at these temperatures, leading to a decrease in their performance.
[0003] To address the issue of high-temperature demagnetization in permanent magnet materials, in addition to optimizing and upgrading the motor cooling system, improving the coercivity of permanent magnet materials is a more effective solution.
[0004] Currently, there are three main methods to improve the coercivity of permanent magnets: The first is by adding heavy rare earth elements, such as dysprosium (Dy), terbium (Tb), or holmium (Ho), to enhance the anisotropic field of the magnet, thereby increasing its coercivity. The second is grain refinement technology; as the grain size decreases, internal defects decrease, the internal demagnetizing field decreases, and the magnet's coercivity increases. The third is grain boundary diffusion technology. This technology causes heavy rare earth elements to diffuse along grain boundaries, significantly increasing the anisotropy constant at the grain boundaries, thus achieving a significant increase in magnet coercivity even with a small amount of heavy rare earth elements.
[0005] To meet the high-temperature demagnetization requirements of existing automotive motors, all three methods mentioned above use heavy rare earth elements to varying degrees. With the soaring prices of heavy rare earth elements in recent years, producing more heat-resistant permanent magnet materials using fewer heavy rare earth elements is currently a key research focus for various companies. Summary of the Invention
[0006] After in-depth research into the aforementioned problems, the inventors discovered that sintered NdFeB magnets exhibit anisotropic characteristics. This anisotropy is manifested not only in the magnetic field orientation but also in the coefficient of thermal expansion. Sintered NdFeB magnets possess different coefficients of thermal expansion in different directions. For example, along the easy magnetization axis (the orientation direction of the magnet), they expand externally with increasing temperature; while along the difficult magnetization axis (perpendicular to the orientation direction of the magnet), they contract externally with increasing temperature. This difference in expansion ratios in different directions causes changes in the sintered NdFeB grains at high temperatures. These changes may induce demagnetization, leading to a decrease in the coercivity of the NdFeB magnet at high temperatures.
[0007] To overcome the shortcomings of existing technologies, this invention provides a high-temperature resistant sintered NdFeB magnet, denoted as R-Fe-BM, which, by mass ratio of 100%, comprises:
[0008] R 29wt%~35wt%, where R is a rare earth element.
[0009] B 0.9wt%~1.3wt%;
[0010] M is less than 5 wt%, and M is selected from one or more of Ti, V, Cr, Mn, Co, Ga, Cu, Si, Al, Zr, Nb, W and Mo;
[0011] The remainder consists of iron and unavoidable impurities.
[0012] According to embodiments of the present invention, R is selected from at least one of lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), promethium (Pm), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), lutetium (Lu), scandium (Sc), and yttrium (Y). Praseodymium (Pr) and neodymium (Nd) are preferred.
[0013] According to an embodiment of the present invention, the magnet comprises, by mass percentage (100%), 30wt% to 33wt% R, where R is a rare earth element.
[0014] B 0.9wt%~1.1wt%;
[0015] M 0.5wt%~4.5wt%, M is selected from one or more of Ti, V, Cr, Mn, Co, Ga, Cu, Si, Al, Zr, Nb, W and Mo;
[0016] The remainder consists of iron and unavoidable impurities.
[0017] In this invention, the reference temperature is set to T0 (e.g., room temperature, or 20°C), and the measurement temperature is set to T (°C). The magnet dimension L0 is measured at T0, and the magnet dimension L(T) is measured after the magnet temperature is raised to T; T-T0=△T, L(T)-L0=△L. The linear expansion coefficient C of the sintered NdFeB magnet is C=[△L / L0] / △T, where the linear expansion coefficient includes C1 parallel to the magnetization direction, C2 perpendicular to the magnetization direction and parallel to the pressing direction, C3 perpendicular to the magnetization direction, and C4 the average of the linear expansion coefficients in the two directions perpendicular to the magnetization direction.
[0018] According to an embodiment of the present invention, the linear expansion coefficient C1 parallel to the magnetization direction of the magnet is (5~8)*10. -6 / ℃,
[0019] The coefficient of linear expansion C2 perpendicular to the magnetization direction and parallel to the pressing direction is (-3 to -0.6)*10. -6 / ℃,
[0020] The linear expansion coefficient C3 in the direction perpendicular to the magnetization direction is (-4 to -1)*10. -6 / ℃,
[0021] The average linear expansion coefficient C4 in the two directions perpendicular to the magnetization direction is (-3.5 to -0.8)*10. -6 / ℃, where C4=(C2+C3) / 2;
[0022] Furthermore, 1.5 ≤ |C1 / C4| ≤ 8.
[0023] In this invention, the sintered NdFeB magnet expands parallel to the magnetization direction as the temperature increases, and contracts in the other two directions perpendicular to the magnetization direction. Therefore, C1 is greater than 0, C2 is less than 0, and C3 is less than 0.
[0024] This invention also provides a method for preparing the above-mentioned sintered NdFeB magnet, the method comprising:
[0025] (1) R-Fe-BM alloy sheets were prepared from the raw materials using the rapid solidification thin strip method;
[0026] (2) Hydrogenation treatment is performed on the alloy sheet by adding hydrogen. After the hydrogenation treatment is completed, the temperature is raised to 250-350℃ for dehydrogenation treatment. After the dehydrogenation is completed, argon gas is purged to above 30kPa for heating and holding. After the holding is completed, the alloy powder is obtained by cooling.
[0027] (3) The alloy powder in step (2) is air-milled to obtain magnetic powder, and then subjected to molding, sintering and tempering to prepare the magnet.
[0028] According to an embodiment of the present invention, in step (1), the rapid coagulation thin strip method is a well-known technique in the art.
[0029] According to an embodiment of the present invention, in step (2), the hydrogen absorption pressure of the hydrogenation treatment is 100-200 kPa, preferably 140-180 kPa, and the hydrogen absorption time is 30-180 min, preferably 90-150 min.
[0030] According to an embodiment of the present invention, in step (2), the dehydrogenation time is 180 to 360 min.
[0031] According to an embodiment of the present invention, in step (2), the dehydrogenation temperature is 250°C, 260°C, 270°C, 280°C, 290°C, 300°C, 310°C, 320°C, 330°C, 340°C or 350°C.
[0032] According to an embodiment of the present invention, in step (2), after dehydrogenation is completed, argon gas is purged to a pressure of 30 kPa or higher, for example, 30-60 kPa. Exemplary values are 30 kPa, 35 kPa, 40 kPa, 45 kPa, 50 kPa, 5 kPa, or 60 kPa.
[0033] According to an embodiment of the present invention, in step (2), the heat preservation temperature is 700-800℃, for example, 720℃, 740℃, 760℃, 780℃ or 800℃.
[0034] According to an embodiment of the present invention, in step (2), the heat preservation time is 60 to 180 minutes.
[0035] According to an embodiment of the present invention, in step (2), during the cooling process, the argon pressure is ≥20 kPa, for example, 20-60 kPa, when the temperature is above 350°C. Exemplary values are 20 kPa, 30 kPa, 40 kPa, 50 kPa, or 60 kPa.
[0036] According to an embodiment of the present invention, in step (3), the alloy powder from step (2) is mixed with a lubricant and then ground by an air jet mill to obtain magnetic powder.
[0037] According to an embodiment of the present invention, in step (3), the particle size D50 of the magnetic powder is 2 to 5 μm.
[0038] According to an embodiment of the present invention, in step (3), the content of lubricant is 0.03 to 0.5 wt% of the alloy powder in step (2), preferably 0.05 to 0.1 wt%.
[0039] According to an embodiment of the present invention, in step (3), the magnetic powder is pressed into shape under magnetic field orientation. Preferably, the orientation magnetic field is 1.5 to 2.5 T.
[0040] According to an embodiment of the present invention, in step (3), the sintering temperature is 800-1200℃, preferably 900-1080℃, and the holding time is 3-20h, preferably 3-8h.
[0041] According to an embodiment of the present invention, in step (3), the tempering treatment is a two-stage tempering, for example, a two-stage tempering treatment is carried out in a vacuum tempering furnace; the first-stage tempering temperature is 700-900℃ and the holding time is 3-7h, the second-stage tempering temperature is 450-600℃ and the holding time is 3-7h.
[0042] According to an embodiment of the present invention, the method further includes step (4): performing grain boundary diffusion treatment on the magnet, wherein the diffusion source is at least one of heavy rare earth elements Dy, Tb, Ho, Nd, and Pr.
[0043] According to an embodiment of the present invention, in step (4), the content of diffused heavy rare earth elements is 0.1-1.5 wt%, preferably 0.2-1.2 wt%.
[0044] According to an embodiment of the present invention, in step (4), the diffusion temperature is 800-950°C and the diffusion time is at least 3 hours, preferably 3-30 hours.
[0045] According to an embodiment of the present invention, in step (4), the grain boundary diffusion treatment method can be at least one of thermal spraying, coating, sputtering, immersion and the like.
[0046] According to an embodiment of the present invention, in step (4), before the diffusion treatment, the magnet can also be treated with degreasing, pickling and other processes.
[0047] As an exemplary implementation of the present invention, the method for preparing the high-temperature resistant sintered NdFeB magnet specifically includes:
[0048] 1) R-Fe-BM alloy sheets were obtained using the rapid solidification strip method;
[0049] 2) The above alloy sheet is subjected to hydrogenation treatment with a hydrogen absorption pressure of 100-200 kPa and a hydrogen absorption time of 30-180 min. After hydrogen absorption, the temperature is raised to 250-350℃ for dehydrogenation treatment for 180-360 min. After dehydrogenation, argon gas is purged to above 30 kPa, and then the temperature is raised to 700-800℃ and held for 60-180 min. After holding, the sheet is cooled, wherein the argon gas pressure is ≥20 kPa when the temperature is above 350℃ during the cooling process.
[0050] 3) The above alloy powder is mixed with a lubricant and ground by an air jet mill to obtain magnetic powder; then the magnetic powder is pressed into shape under magnetic field orientation; the orientation magnetic field is 1.5~2.5T;
[0051] 4) The above-mentioned pressed blank is sintered in a vacuum sintering furnace at a temperature of 900–1080℃ for 3–8 hours. After holding at this temperature, it is cooled to ≤200℃, and then subjected to a first-stage tempering treatment at 700–900℃ for 3–7 hours. Finally, a second-stage tempering treatment is performed at 450–600℃ for 3–7 hours to prepare the sintered NdFeB magnet.
[0052] 5) Diffusion treatment of the magnet in step 4): The magnet in step 4) is processed into the required size, and after degreasing and pickling, it is subjected to grain boundary diffusion treatment; the diffusion temperature is 800-950℃, the diffusion time is at least 3h, and the diffusion source is at least one element selected from Dy, Tb, Ho, Nd and Pr.
[0053] The present invention also describes the application of the above-mentioned sintered NdFeB magnets in the new energy vehicle industry and the field of wind power generation.
[0054] The beneficial effects of this invention are:
[0055] The sintered NdFeB magnets of the present invention exhibit smaller dimensional change rates in different directions at high temperatures, reducing the probability of demagnetization formation and improving the coercivity of NdFeB magnets at high temperatures, thereby enhancing the demagnetization resistance of sintered NdFeB magnets at high temperatures. Attached Figure Description
[0056] Figure 1 This is a graph of the linear expansion coefficient C1 parallel to the magnetization direction of the magnet, as tested in Example 1; Figure 2 This is the linear expansion coefficient C2 diagram of Example 1, which is perpendicular to the magnetization direction and parallel to the pressing direction.
[0057] Figure 3 This is a graph showing the linear expansion coefficient C3 in another direction perpendicular to the magnetization direction, as tested in Example 1. Detailed Implementation
[0058] The technical solution of the present invention will be further described in detail below with reference to specific embodiments. It should be understood that the following embodiments are merely illustrative and explanatory of the present invention, and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are covered within the scope of protection intended by the present invention.
[0059] Unless otherwise stated, the raw materials and reagents used in the following examples are commercially available products or can be prepared by known methods.
[0060] Measurement of the linear expansion coefficient of the sintered NdFeB magnet of this invention:
[0061] The coefficient of linear expansion was measured using a thermomechanical analyzer, model TMA402F3. The method employed was static thermomechanical analysis, which measures the deformation of a material under non-vibrational loads as a function of temperature, under programmed temperature control. The test temperature ranged from 20°C to higher temperatures, with a heating rate of 3–5°C / min. The test directions were the three directions of the magnet.
[0062] Example 1, Comparative Examples 1-7
[0063] The alloy is prepared by high-frequency melting of NdPr, Co, Al, Fe, Cu, Ga, Ti and ferroboron in an argon atmosphere using materials with a purity of at least 99% by weight, and then casting the melt onto a quenching roller to form an alloy sheet. The contents of each raw material are 31.5% NdPr, 1.0% Co, 0.5% Al, 0.2% Cu, 0.2% Ga, 0.18% Ti, 0.98% B, with the balance being iron and unavoidable impurities.
[0064] The alloy sheet was hydrogenated at a pressure of 180 kPa for 120 min. After hydrogen absorption, the processing followed the hydrogenation process outlined in Table 1, resulting in coarse powder. This coarse powder was then milled using an air jet mill to obtain magnetic powder with a particle size D50 of 4.0 μm. 0.3 wt% lubricant was added to the milled powder, and the mixture was stirred for 2 h. The powder was then shaped under ambient temperature and a 2 T magnetic field. The blank was then placed in a vacuum sintering furnace and sintered at 1030 °C for 6 h. After holding at this temperature, it was cooled to 100 °C. The temperature was then raised to 900 °C for a first-stage tempering treatment of 3 h, followed by a second-stage tempering treatment at 520 °C for 5 h. After cooling, the neodymium iron boron magnet was obtained.
[0065] The neodymium iron boron magnets obtained above were processed into products with a size of 10⁻⁸-6 mm, and the coefficient of linear expansion in different directions was tested using a thermomechanical analyzer. The heating rate was 5℃ / min, and the test temperature ranged from 20 to 140℃. The test results are shown in Table 2.
[0066] In addition, the neodymium iron boron magnets obtained above were processed into D10-10mm products and subjected to magnetic tests at 20℃ and 140℃. The test results are shown in Table 3.
[0067] Table 1. Hydrogenation processes corresponding to Example 1 and Comparative Examples 1-7
[0068]
[0069] The products prepared in Example 1 and Comparative Examples 1-7 were subjected to linear expansion coefficient testing. The method for testing the linear expansion coefficient is as follows:
[0070] The magnet size is measured as L0 at room temperature T0. After raising the magnet temperature to the measurement temperature T (°C), the magnet size L (T) is measured. T - T0 = ΔT, L (T) - L0 = ΔL. The linear expansion coefficient of sintered NdFeB magnets is C = [ΔL / L0] / ΔT.
[0071] The test results are shown in Table 2 below.
[0072] Table 2. Coefficients of linear expansion for NdFeB products tested in Examples 1 and Comparative Examples 1-7.
[0073]
[0074] The products prepared in Example 1 and Comparative Examples 1-7 were tested for Br, Hcj (including 20℃ and 140℃) and Hcj temperature coefficient. The test results are shown in Table 3 below.
[0075] Table 3. Magnetic performance results of NdFeB products in Examples 1 and Comparative Examples 1-7
[0076] Br(T)20℃ Hcj(kA / m)20℃ Hcj(kA / m) 140℃ Hcj temperature coefficient Example 1 1.36 1569 559 -0.536 Comparative Example 1 1.361 1495 526 -0.540 Comparative Example 2 1.345 1556 517 -0.556 Comparative Example 3 1.365 1423 475 -0.555 Comparative Example 4 1.363 1460 497 -0.550 Comparative Example 5 1.36 1531 537 -0.541 Comparative Example 6 1.365 1437 500 -0.543 Comparative Example 7 1.359 1488 525 -0.539
[0077] Comparing the data from Example 1 and Comparative Example 1, it can be seen that Comparative Example 1, due to its excessively high dehydrogenation temperature exceeding the range required by the patented process, although C1, C2, C3, and C4 are all within the range, these values are all within the critical range, causing |C1 / C4| to exceed the patent range, resulting in poorer temperature resistance (a worse Hcj temperature coefficient). Simultaneously, because of the excessively high dehydrogenation temperature, the room temperature Hcj of Comparative Example 1 is already low, and coupled with the worsened temperature resistance, the high-temperature Hcj becomes even lower.
[0078] Comparing the data from Example 1 and Comparative Example 2, it can be seen that in Comparative Example 2, due to the excessively low dehydrogenation temperature, C1, C2, C3, C4, and |C1 / C4| all exceed the patent scope, resulting in poorer temperature resistance (a worse Hcj temperature coefficient). Furthermore, due to the excessively low dehydrogenation temperature, the Br content at room temperature in Comparative Example 2 decreases significantly. Moreover, this process increases the hydrogen content before sintering, leading to more cracks in the product after sintering and an increased product defect rate.
[0079] Comparing the data from Example 1 with Comparative Examples 3 and 4, it can be seen that in Comparative Example 3, the argon pressure after dehydrogenation was 0, meaning no argon was introduced. In Comparative Example 4, the argon pressure after dehydrogenation was 10 kPa, which is relatively low. Both of these comparative examples resulted in subsequent dehydrogenation of the flakes at 750°C, leading to a poorer flake pulverization effect. This resulted in C1, C2, C3, C4, and |C1 / C4| all exceeding the patent scope, leading to poorer temperature resistance (a worse Hcj temperature coefficient). In addition, due to the poor coefficient of linear expansion, the product generated too many defects during sintering and cooling, resulting in lower Hcj at room temperature in Comparative Examples 3 and 4. Combined with the poorer temperature resistance, the Hcj at high temperature became even lower.
[0080] Comparing the data from Example 1 and Comparative Example 5, it can be seen that in Comparative Example 5, due to the excessively low holding temperature, the elemental transition between grains and grain boundaries was insufficient, resulting in a metastable structure. Although C1, C2, C3, and C4 are all within the range, these values are all within the critical range. Therefore, |C1 / C4| exceeds the patent range, leading to a deterioration in temperature resistance (a deterioration in the Hcj temperature coefficient).
[0081] Comparing the data from Example 1 and Comparative Example 6, it can be seen that in Comparative Example 6, due to the excessively high insulation temperature, the grains in the flakes grew to a certain extent, resulting in a poorer flake pulverization effect. Although C1, C2, C3, and C4 are all within the range, because these values are all within the critical range, |C1 / C4| exceeds the patent scope, leading to a decrease in temperature resistance (a decrease in the Hcj temperature coefficient). In addition, because of the growth of the flake grains, the Hcj of the product at room temperature decreases, and coupled with the decrease in temperature resistance, the Hcj at high temperature becomes even lower.
[0082] Comparing the data from Example 1 and Comparative Example 7, it can be seen that in Comparative Example 7, the argon pressure introduced during the cooling process at temperatures above 350°C was too low, causing the scales to undergo dehydrogenation at higher temperatures. , Although C1, C2, C3, and C4 are all within the range, these values are all within the critical range. Therefore, |C1 / C4| exceeds the patent scope, resulting in poorer temperature resistance (a worse Hcj temperature coefficient). In addition, because Comparative Example 7 dehydrogenates at a higher temperature, the Hcj of Comparative Example 7's product at room temperature is lower. Combined with the worsened temperature resistance, the Hcj at high temperatures becomes even lower.
[0083] Example 2
[0084] The NdFeB magnets prepared in Example 1 were processed into square sheets with dimensions of 20-15-3 mm. After degreasing and pickling, the sheets underwent Dy grain boundary diffusion treatment. The diffusion amount of Dy was 0.8 wt%, the diffusion temperature was 900 °C, and the diffusion time was 15 h. In this example, the grain boundary diffusion was performed using a coating method to obtain sintered NdFeB magnets. The linear expansion coefficient of the product in different directions was tested using a thermomechanical analyzer, and the test results are shown in Table 4 below. The heating rate was 5 °C / min, and the test temperature was 20-140 °C. In addition, the NdFeB magnets obtained above were subjected to magnetic tests at 20 °C and 140 °C, and the test results are shown in Table 5 below.
[0085] Table 4 shows the linear expansion coefficients of the NdFeB products in Examples 1-2.
[0086]
[0087] Table 5. Magnetic property results of NdFeB products in Examples 1-2
[0088] Br(T)20℃ Hcj(kA / m)20℃ Hcj(kA / m) 140℃ Hcj temperature coefficient Example 1 1.36 1569 559 -0.536 Example 2 1.343 2209 960 -0.471
[0089] As can be seen from Example 2, after the blank prepared in Example 1 undergoes diffusion of heavy rare earth elements, C1, C2, C3, C4, and |C1 / C4| are all within the scope of the patent. Furthermore, when the blank prepared in Example 1 undergoes diffusion of heavy rare earth elements, the product performance is significantly improved, exhibiting better temperature resistance.
[0090] Example 3
[0091] The other steps are the same as in Example 1, except for the processing after hydrogen absorption. The dehydrogenation temperature is 350℃, the argon gas pressure after dehydrogenation is 30kPa, the holding temperature is 800℃, and the argon gas pressure during cooling is 30kPa when the temperature is above 350℃. The expansion coefficient of the tested product is shown in Table 6, and the corresponding product performance is shown in Table 7.
[0092] Table 6 shows the linear expansion coefficients of the NdFeB products in Example 3.
[0093]
[0094] Table 7. Magnetic performance results of NdFeB products in Example 3.
[0095] Br(T)20℃ Hcj(kA / m)20℃ Hcj(kA / m) 140℃ Hcj temperature coefficient Example 3 1.358 1544 547 -0.538
[0096] Example 4
[0097] The other steps are the same as in Example 1, except for the processing after hydrogen absorption. The dehydrogenation temperature is 250℃, the argon gas pressure after dehydrogenation is 35kPa, the holding temperature is 700℃, and the argon gas pressure during cooling is 20kPa when the temperature is above 350℃. The expansion coefficient of the tested products is shown in Table 8, and the corresponding product performance is shown in Table 9.
[0098] Table 8 shows the linear expansion coefficients of the NdFeB products in Example 4.
[0099]
[0100] Table 9 shows the magnetic properties of the neodymium iron boron product in Example 4.
[0101] Br(T)20℃ Hcj(kA / m)20℃ Hcj(kA / m) 140℃ Hcj temperature coefficient Example 4 1.361 1548 546 -0.539
[0102] The embodiments of the present invention have been described above by way of example. However, the scope of protection of the present invention is not limited to the above embodiments. Any modifications, equivalent substitutions, improvements, etc., made by those skilled in the art within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A high-temperature resistant sintered NdFeB magnet, characterized in that, The magnet, denoted as R-Fe-BM, comprises, by mass ratio of 100%,: R 29wt%~35wt%, where R is a rare earth element. B 0.9wt%~1.3wt%; M is less than 5 wt%, and M is selected from one or more of Ti, V, Cr, Mn, Co, Ga, Cu, Si, Al, Zr, Nb, W and Mo; The remainder consists of iron and unavoidable impurities; The linear expansion coefficient C1 parallel to the magnetization direction of the magnet is (5~8)*10. -6 / ℃, The coefficient of linear expansion C2 perpendicular to the magnetization direction and parallel to the pressing direction is (-3 to -0.6) * 10⁻⁶. -6 / ℃, The linear expansion coefficient C3 in the direction perpendicular to the magnetization direction is (-4 to -1) * 10. -6 / ℃, The average linear expansion coefficient C4 in the two directions perpendicular to the magnetization direction is (-3.5 to -0.8) * 10⁻⁶. -6 / ℃, where C4 = (C2 + C3) / 2; 1.5≤|C1 / C4|≤8.
2. The method for preparing the magnet according to claim 1, characterized in that, The method includes: (1) R-Fe-BM alloy sheets were prepared from the raw materials using the rapid solidification thin strip method; (2) Hydrogenation treatment is performed on the alloy sheet by adding hydrogen. After the hydrogenation treatment is completed, the temperature is raised to 250-350℃ for dehydrogenation treatment. After the dehydrogenation is completed, argon gas is purged to above 30 kPa for heating and heat preservation. After the heat preservation is completed, the alloy powder is obtained by cooling. (3) The alloy powder in step (2) is air-milled to obtain magnetic powder, and then subjected to molding, sintering and tempering to prepare the magnet.
3. The method according to claim 2, characterized in that, In step (2), the hydrogen absorption pressure of the hydrogenation treatment is 100-200 kPa and the hydrogen absorption time is 30-180 min.
4. The method according to claim 2, characterized in that, In step (2), the dehydrogenation time is 180 to 360 minutes.
5. The method according to claim 2, characterized in that, In step (2), after dehydrogenation is completed, argon gas is purged to 30-60 kPa.
6. The method according to claim 2, characterized in that, In step (2), the heat preservation temperature is 700-800℃; the heat preservation time is 60-180min.
7. The method according to claim 2, characterized in that, In step (2), during the cooling process, the argon pressure is ≥20kPa when the temperature is above 350℃.
8. The method according to claim 2, characterized in that, In step (3), the alloy powder from step (2) is mixed with a lubricant and then ground by an air jet mill to obtain magnetic powder.
9. The method according to claim 2, characterized in that, In step (3), the particle size D50 of the magnetic powder is 2 to 5 μm.
10. The method according to claim 8, characterized in that, In step (3), the content of lubricant is 0.03 to 0.5 wt% of the alloy powder in step (2).
11. The method according to claim 2, characterized in that, In step (3), the magnetic powder is pressed into shape under magnetic field orientation.
12. The method according to claim 11, characterized in that, The orientation magnetic field is 1.5–2.5 T.
13. The method according to claim 2, characterized in that, In step (3), the sintering temperature is 800-1200℃ and the holding time is 3-20h.
14. The method according to claim 2, characterized in that, In step (3), the tempering treatment is a two-stage tempering; the first-stage tempering temperature is 700-900℃ and the holding time is 3-7h, the second-stage tempering temperature is 450-600℃ and the holding time is 3-7h.
15. The method according to claim 2, characterized in that, The method further includes step (4): performing grain boundary diffusion treatment on the magnet, wherein the diffusion source is at least one of heavy rare earth elements Dy, Tb, Ho, Nd, and Pr.
16. The method according to claim 15, characterized in that, In step (4), the content of diffused heavy rare earth elements is 0.1-1.5 wt%.
17. The method according to claim 15, characterized in that, In step (4), the diffusion temperature is 800-950℃ and the diffusion time is at least 3 hours.
18. The application of the magnet according to claim 1 in the new energy vehicle industry and the wind power generation field.
Citation Information
Patent Citations
Preparation method of sintered neodymium-iron-boron magnet without containing heavy rare earth elements
CN105513737A
Cerium- and cobalt-doped sintered NdFeB magnet and preparation method thereof
CN106601460A