A polysulfone-based hollow fiber ultrafiltration membrane, its preparation method and application

By designing a multilayer structure and a reasonable pore size distribution for polysulfone hollow fiber ultrafiltration membranes, the contradiction between high retention efficiency and high flux of ultrafiltration membranes was resolved, achieving efficient preparation and stable filtration of ultrapure water.

CN117463171BActive Publication Date: 2026-11-17HANGZHOU COBETTER SEMICONDUCTOR SEPARATION MEMBRANE CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202311539733.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-18
Publication Date
2026-11-17
Estimated Expiration
2043-11-18

AI Technical Summary

Technical Problem

Existing ultrafiltration membranes struggle to simultaneously achieve high retention efficiency and high flux when preparing ultrapure water, and the membrane pores are susceptible to defects, resulting in impurities remaining in the ultrapure water and affecting its application.

Method used

The ultrafiltration membrane is made of polysulfone hollow fiber and has a multi-layer structure, including an outer skin layer, a first intermediate layer and an inner skin layer, all of which are tortuous channels. The outer and inner surfaces have finger-like pore structures with different pore sizes to ensure high retention efficiency and high porosity. The membrane is integrally molded to improve mechanical strength.

Benefits of technology

It achieves efficient retention of nanoscale impurities, ensuring high purity and high throughput of ultrapure water, making it suitable for terminal filtration of ultrapure water, and extending the stability and service life of the membrane structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117463171B_ABST
    Figure CN117463171B_ABST
Patent Text Reader

Abstract

This invention discloses a polysulfone hollow fiber ultrafiltration membrane, its preparation method, and its application. The ultrafiltration membrane includes a main body, with one side being an inner surface facing the inner cavity and the other side being an outer surface. From the outer surface to the inner surface, the main body sequentially includes an outer skin layer, an outer pore layer, a first intermediate layer, an inner pore layer, and an inner skin layer. The outer skin layer, the first intermediate layer, and the inner skin layer all have tortuous pathways, serving as regions for trapping impurity particles, and each layer has a thickness of not less than 1 μm. Both the outer and inner pore layers have finger-like pore structures. The average SEM pore size of the outer surface is not greater than 60 nm. This ultrafiltration membrane has an ideal membrane structure, with suitable pore sizes on both the inner and outer surfaces and a high overall porosity, thus ensuring high retention efficiency for various nanoscale impurities in water, while also exhibiting high flux, making it particularly suitable for terminal filtration of ultrapure water.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of membrane materials technology, and more specifically to a polysulfone hollow fiber ultrafiltration membrane, its preparation method, and its application. Background Technology

[0002] Ultrapure water, also known as high-purity water, refers to water in which almost all conductive media have been removed, and non-dissociated colloidal substances, gases, and organic matter have been removed to very low levels. Ultrapure water has a salt content below 0.1 mg / L and a conductivity less than 0.1 μS / cm. The main applications of ultrapure water include: ① electronics, power, electroplating, lighting appliances, laboratories, food, papermaking, daily chemicals, building materials, paint manufacturing, batteries, testing, biology, pharmaceuticals, petroleum, chemicals, steel, and glass industries; ② process water for chemical products, pharmaceuticals, and cosmetics; ③ pure water for the production processes of single-crystal silicon, semiconductor wafer cutting, semiconductor chips, semiconductor packaging, lead frame racks, integrated circuits, liquid crystal displays, conductive glass, picture tubes, circuit boards, optical communication, computer components, capacitors, and various other clean products and components; ④ cleaning of high-voltage transformers, etc. Due to the wide range of applications of ultrapure water, how to efficiently obtain high-performance ultrapure water has always been a focus of research and development.

[0003] The process of preparing ultrapure water mainly consists of three steps: pretreatment, desalination, and purification. For example, Chinese patent application CN202180044389.8 (applied by Organo Corporation) "Ultrapure Water Manufacturing Apparatus" describes each step in detail. A crucial step is removing various tiny impurities remaining in the water through an ultrafiltration membrane (these impurities can adversely affect the subsequent practical application of ultrapure water). The particle size of these impurities is generally only tens or even hundreds of nanometers, making removal difficult and requiring a retention efficiency of over 95%. This poses a significant challenge to ultrafiltration membranes. Currently, ordinary filter membranes on the market only achieve a retention efficiency of 90% (because small defects can easily occur during membrane manufacturing, which can significantly affect the high retention efficiency of the membrane). At the same time, while making the membrane pores very small can ensure a high retention efficiency, it will result in very low membrane porosity, leading to low membrane flux and significantly affecting the preparation of ultrapure water, thus hindering its widespread application. Summary of the Invention

[0004] To address the shortcomings of existing technologies, the present invention aims to provide a polysulfone hollow fiber ultrafiltration membrane, its preparation method, and its application. This ultrafiltration membrane has an ideal membrane structure, with suitable pore sizes on both its inner and outer surfaces and a high overall porosity. It also has at least three regions capable of trapping tiny impurities in water, thereby ensuring that the membrane has high retention efficiency for various nanoscale impurities in water. In addition, it also has high flux, making it particularly suitable for terminal filtration of ultrapure water.

[0005] To achieve the above objectives, the present invention provides the following technical solution: a polysulfone hollow fiber ultrafiltration membrane, comprising a body, one side of which is an inner surface facing the inner cavity, and the other side of which is an outer surface. In the direction from the outer surface to the inner surface, the body sequentially comprises an outer skin layer, an outer void layer, a first intermediate layer, an inner void layer, and an inner skin layer; one side of the outer skin layer is the outer surface; one side of the inner skin layer is the inner surface; wherein the outer skin layer, the first intermediate layer, and the inner skin layer all have tortuous pathways, which are regions for trapping impurity particles, and the thickness of each layer is not less than 1 μm; the outer void layer and the inner void layer both have finger-like pore structures; the SEM average pore size of the outer surface is not greater than 60 nm; the SEM average pore size of the inner surface is 20-250 nm; and the SEM average pore size of the inner surface is greater than the SEM average pore size of the outer surface; the overall porosity of the filter membrane is not less than 50%.

[0006] When filtering ultrapure water at the terminal, a key indicator of the filter membrane is the retention efficiency, which requires a retention efficiency of more than 95% for impurities (at this point, a retention efficiency of more than 90% is no longer sufficient to meet the requirements). That is, it is necessary to ensure that there are as few impurity particles as possible in the ultrapure water, because even a small number of impurity particles can greatly affect the various applications of ultrapure water.

[0007] During membrane fabrication, defects of varying sizes are inevitable. Even very small defects (invisible to the naked eye) can affect the membrane's retention efficiency, thus impacting the preparation of ultrapure water (i.e., after ultrafiltration, the ultrapure water still contains a small amount of impurity particles). This invention utilizes at least three layers capable of retaining impurities: an outer skin layer, a first intermediate layer, and an inner skin layer. These layers each possess non-directional tortuous pathways (referring to randomly oriented groove structures and / or discretely distributed pore structures, with each pathway interconnected), and each region has a certain thickness (not less than 1 μm). By ensuring that each region can retain nanoscale impurities, i.e., through multi-stage retention, even with minor membrane defects, highly efficient and stable retention can still be guaranteed, resulting in ultrapure water with extremely high purity. Even with the same total thickness of the retention layer, the retention efficiency of the three-layer region is greater than that of a single layer. This is because defects are easily generated during membrane fabrication. In a single-layer retention layer, these defects will inevitably affect the retention effect, especially when such high retention efficiency is required. However, the retention efficiency of the three-layer region is largely unaffected by minor defects. Therefore, this membrane is particularly suitable for terminal filtration of ultrapure water.

[0008] In this invention, the filter membrane has a certain number of pores on both its inner and outer surfaces. These pores are used to trap various tiny impurities while facilitating fluid passage. Research shows that the pore size on the outer surface of the filter membrane is very small (and smaller than the pore size on the inner surface), with an average SEM pore size of no more than 60 nm. This small pore size ensures sufficient impurity trapping; the outer skin layer is the most critical area for impurity trapping, and impurities are primarily trapped there. Since impurities are mainly trapped within the outer skin layer, the fluid carries away the impurity particles during the ultrafiltration process. This prevents a large accumulation of impurities within the outer skin layer, thus avoiding a rapid decrease in membrane flux. This allows the filter membrane to maintain a high flux for an extended period, resulting in a longer service life. Simultaneously, the small pore size on the outer surface facilitates cleaning before actual use, ensuring that the membrane fibers themselves are virtually free of impurities (TOC and metal ion content are very low, preventing contamination of ultrapure water). Furthermore, the average SEM pore size on the inner surface of the membrane fibers... The SEM average pore size of the inner surface is larger than that of the outer surface (i.e., the membrane pores on the inner surface are slightly larger), which is beneficial to improving the flux of the membrane fibers. However, it cannot be too large. Studies have shown that the SEM average pore size of the inner surface is 20-250 nm. At this pore size, it can further retain impurity particles and reduce TOC leaching (i.e., during filtration, a small amount of TOC dissolves from the membrane itself, and the inner surface can also retain these substances, further ensuring low leaching of the membrane fibers). In existing technologies, if the pore size of the inner and outer surfaces is small, it is easy to cause the overall porosity of the membrane to be low, which in turn leads to a low overall flux, still unable to meet the needs of practical applications. In this invention, both the outer and inner void layers have finger-like pore structures. The presence of finger-like pore structures greatly improves the overall porosity of the membrane. The overall porosity of the membrane fibers in this invention is not less than 50%, thereby ensuring that the membrane fibers have a high flux and can filter ultrapure water quickly, ensuring the preparation of high-purity ultrapure water in a short time.

[0009] In summary, the present invention, through the combined effect of at least three layers with regions for trapping minute impurities, suitable pore sizes on both the inner and outer surfaces, and high overall porosity, ensures that the membrane has high trapping efficiency for various nanoscale impurities in water, while also having high flux, making it particularly suitable for terminal filtration of ultrapure water.

[0010] Furthermore, the ultrafiltration membrane of the present invention is integrally formed, meaning that the entire structure of the membrane fibers is made of the same material and is formed directly during the membrane preparation process; in the transition from the membrane thickness direction, there is only a change in the membrane structure, which is an asymmetric membrane; in contrast, for example, composite membranes have a multi-layer structure, which is made by applying a dense layer, which serves as the retention layer, onto a porous layer or porous membrane, often a microporous support layer or support membrane, in a separate process step; the materials constituting the support layer and the retention layer in a composite membrane are often different; the integrally formed porous membrane has higher mechanical strength than the composite membrane and has almost no risk of delamination.

[0011] In this invention, the average pore size of the outer surface and the average pore size of the inner surface of the filter membrane, as well as the subsequent pore area ratio of the inner and outer surfaces, can all be characterized by scanning electron microscopy (SEM) of the membrane structure, followed by measurement and calculation using computer software (such as Matlab, NIS-Elements, etc.) or manually. During the membrane fabrication process, in the direction perpendicular to the membrane thickness (if the membrane is a flat sheet, this direction is planar; if the membrane is a hollow fiber membrane, this direction is perpendicular to the radius), the pore size and pore distribution are generally uniform and consistent. Therefore, the overall pore size and pore area ratio on the corresponding plane can be reflected by the pore size and pore area ratio of a certain area on that plane. In actual measurement, the inner and outer surfaces of the filter membrane can be characterized using an electron microscope to obtain the corresponding SEM images. Since the pore size and pore distribution on the inner and outer surfaces are generally uniform, a certain area, such as 1 μm, can be selected. 2 (1μm x 1μm) or 100μm 2 (10μm x 10μm) or, the specific area size depends on the actual situation. Then, use appropriate computer software or manual measurement to determine the membrane pore size and pore area ratio on that area. Perform several tests and take the average value to obtain the SEM average pore size and pore area ratio of the inner and outer surfaces of the filter membrane. Of course, those skilled in the art can also obtain the above parameters through other measurement methods. The above measurement methods are for reference only.

[0012] As a further improvement of the present invention, the SEM average pore size of the outer surface is 1-50 nm, and the pore area ratio is 0.1%-10%.

[0013] To ensure efficient retention of various minute impurities in the water, the SEM average pore size of the outer surface of the filter membrane is preferably 1-50 nm. This facilitates more thorough impurity retention (the outer skin layer is the most critical area for impurity retention; therefore, appropriately adjusting the pore size of the outer surface membrane can further guarantee retention efficiency while having minimal impact on the overall membrane flux). Simultaneously, the pore area ratio on the outer surface is very low, ranging from 0.1% to 10%. This is because in ultrapure water filtration, the outer surface serves as both the inlet and pressure-bearing surface, requiring higher pressure resistance. Pressure resistance is particularly important for such high-precision retention. (Pressure resistance) The pore size is not high. During ultrafiltration, the membrane pores either deform, affecting the retention efficiency, or collapse, affecting the flux. At the same time, since ultrapure water is already relatively clean during terminal filtration, the number of fine impurities contained inside is not large, so a large number of membrane pores is not required. That is, the pore size and pore area ratio of the outer surface membrane of this invention are closely related to ultrapure water applications and are quite unique. In this invention, by having a suitable pore size and a suitable number of pores on the outer surface of the filter membrane, the retention efficiency is guaranteed while also having good mechanical strength (pressure resistance) and minimal impact on membrane flux, making it particularly suitable for use in ultrapure water terminal filtration.

[0014] As a further improvement of the present invention, the ratio of the SEM average aperture of the inner surface to the SEM average aperture of the outer surface is 2-15.

[0015] The pore area ratio of the inner surface is 2%-15% larger than that of the outer surface.

[0016] The ultrapure water filtration of this invention is an external pressure filtration, meaning the fluid first passes through the outer surface, then the inner surface, and then flows out. Therefore, the membrane pores on the inner surface do not need to be very small; they can be slightly larger than those on the outer surface. Preferably, the ratio of the average SEM pore size of the inner surface to that of the outer surface is 2-15. On the one hand, under the combined effect of a certain thickness and tortuous pathway, the slightly larger inner surface membrane pores can still play a retention role (retaining tiny impurities in the fluid and various dissolutions), while also ensuring good overall membrane flux. Furthermore, if the membrane pores on the inner and outer surfaces are as small, the inner surface is difficult to clean, easily causing rapid clogging of the membrane pores and affecting its service life. When the inner surface membrane pores are too small, the overall membrane flux will decrease, and the filtration speed of the filter membrane for ultrapure water will slow down. On the other hand, when the inner surface membrane pores are too large, they cannot play a retention role, easily leading to low overall retention efficiency of the filter membrane, resulting in insufficient cleanliness of the ultrapure water, making it unusable.

[0017] Furthermore, compared to the outer surface, the membrane pores on the inner surface are slightly larger and the pore area ratio is slightly higher (a low pore area ratio on the inner surface will result in a lower overall membrane flux; a high pore area ratio on the inner surface will result in lower pressure resistance near the inner surface of the membrane and lower overall mechanical strength of the membrane). This ensures a longer service life (more than 5 years) while maintaining retention efficiency, slowing down flux decay, and providing good mechanical strength (the membrane pore size on the inner surface remains stable during long-term filtration, and the flux and retention efficiency remain basically unchanged).

[0018] As a further improvement of the present invention, the main body further includes an intermediate void layer and a second intermediate layer. The intermediate void layer is located on the side of the first intermediate layer opposite to the outer void layer. The second intermediate layer is located between the intermediate void layer and the inner void layer. The second intermediate layer has a tortuous path, which is a region for trapping impurity particles. The thickness of the intermediate void layer is 15-45 μm, and its SEM average pore size is 3-35 μm.

[0019] The thickness of the second intermediate layer is 0.5-10 μm.

[0020] Ultrapure water contains various fine particulate impurities (such as organic matter, endotoxins, and other inorganic particulate impurities). The presence of these impurities leads to insufficient purity of the ultrapure water, affecting its subsequent use. This invention utilizes a three-layer system—an outer skin layer, a first intermediate layer, and an inner skin layer—to efficiently capture these fine particulate impurities, ensuring the ultrapure water meets the requirements of practical applications. However, in certain specialized fields, such as ultra-high precision semiconductors, the requirements for ultrapure water are even higher, as even trace amounts of impurities can contaminate the chip, leading to… This renders the chip unusable; therefore, a higher retention efficiency (retention efficiency of over 99%) is required for the filter membrane. Research has revealed that some filter membranes contain four retention layers, including a second intermediate layer. One side of the second intermediate layer is close to the inner void layer, and the second intermediate layer contains tortuous pathways with a thickness of 0.5-10 μm. Under the combined effect of the tortuous pathways and a certain thickness, various tiny impurities are further captured, thus enabling the filter membrane to have an ultra-high retention efficiency while ensuring that the ultrapure water has a higher purity, making it applicable in fields such as semiconductors where ultrapure water requirements are extremely stringent.

[0021] When the thickness of the second intermediate layer is too small, it cannot effectively capture fine impurities; when the thickness of the second intermediate layer is too large, it will significantly reduce the overall membrane flux. Furthermore, since ultrapure water terminal filtration is relatively clean with few fine impurities, the second intermediate layer does not need to be very thick. Therefore, the thickness of the second intermediate layer in this invention is synergistic with the application of ultrapure water terminal filtration. Because of the addition of a second intermediate layer with relatively small pores within the filter membrane, the overall membrane flux may decrease rapidly. However, the filter membrane in this invention still maintains a high flux. This is achieved, firstly, through the thickness of the second intermediate layer, which is not excessive; and secondly, through the existence of an intermediate void layer between the first and second intermediate layers. This void layer has a continuous region on one side with the first intermediate layer and on the other side with the second intermediate layer. The pores in this void layer are relatively large, with an average SEM pore size of 3-35 μm and a thickness of 15-45 μm, effectively acting as a "compensation" layer, thus ensuring that the overall membrane flux remains high. When the pores or thickness of the intermediate void layer are too large, the overall mechanical strength of the membrane is greatly reduced, failing to meet the requirements of various processing applications. Conversely, when the pores or thickness of the intermediate void layer are too small, the membrane flux remains low, hindering rapid filtration. This invention, through the presence of an intermediate void layer and a second intermediate layer, with the intermediate void layer having suitable pore size and thickness, and the second intermediate layer having suitable thickness, further improves the membrane's retention efficiency, ensuring that the produced ultrapure water has higher crystallinity while maintaining good flux for rapid fluid filtration. Simultaneously, it has minimal impact on the membrane's mechanical strength, maintaining good tensile strength and elongation at break. The presence of the second intermediate layer in this invention further enhances the membrane's retention efficiency; therefore, it is preferable that the second intermediate layer is continuous, meaning it has a retention effect in all regions. However, the second intermediate layer can also be discontinuous, with certain defects (equivalent to large pores) at some locations that hinder retention but still provide retention in defect-free areas, thereby appropriately improving the membrane's retention efficiency.

[0022] As a further improvement of the present invention, the ratio of the thickness of the intermediate void layer to the thickness of the second intermediate layer is 3-10; the sum of the thickness of the intermediate void layer and the thickness of the second intermediate layer is 5%-20% of the overall thickness of the film; and the ratio of the average SEM pore size of the intermediate void layer to the average SEM pore size of the second intermediate layer is 10-80.

[0023] The intermediate void layer is located between the first and second intermediate layers. During the fluid flow from the outer surface to the inner surface, the second intermediate layer provides support for the intermediate void layer, preventing the membrane pores within the void layer from collapsing or shrinking, which could render the membrane fibers unusable. Therefore, the thickness ratio between the intermediate void layer and the second intermediate layer is appropriate, as are the pore sizes. This allows the second intermediate layer to better support the intermediate void layer, improving retention efficiency while having minimal impact on flux. Furthermore, by controlling the thickness and proportion of the intermediate void layer and the second intermediate layer to a small percentage of the overall membrane thickness, the intermediate void layer and the second intermediate layer primarily play an auxiliary role, mainly to further improve the overall membrane retention efficiency, but with minimal impact on membrane flux and membrane mechanical strength.

[0024] As a further improvement of the present invention, the second intermediate layer has a second supporting fiber for forming a porous structure, the SEM average diameter of the second supporting fiber is 30-600 nm; the SEM average pore size of the second intermediate layer is 60-800 nm.

[0025] The second intermediate layer is used to further supplement and retain various fine impurities in ultrapure water. Studies have shown that when the average pore size of the membrane pores in the second intermediate layer is 60-800 nm, combined with the tortuous pathways and corresponding thickness within the region, it can further enhance the high-efficiency retention of various fine impurities in ultrapure water, achieving a retention efficiency of over 99%. In addition, under such pore size and thickness, the impact on the overall membrane flux is relatively small.

[0026] Furthermore, research has revealed that the average SEM diameter of the second supporting fiber is 30-600 nm. Under the action of such a coarse second supporting fiber, on the one hand, it can support the membrane pores inside the second intermediate layer, preventing collapse or shrinkage during the filtration process. In other words, the second intermediate layer can efficiently trap fine impurities for a long time. On the other hand, the second supporting fiber can also provide some support to the intermediate void layer, thereby ensuring that the membrane has a high flux for a long time and a long service life, generally more than 5 years.

[0027] In this invention, the SEM average diameter and other characteristics of the second supporting fiber can be obtained by characterizing the morphology of the membrane cross-section using a scanning electron microscope, then selecting a certain area and measuring it using computer software (such as Matlab, NIS-Elements, etc.) or manually to obtain the diameter of the second supporting fiber, taking the average value, and then further calculating the corresponding SEM average diameter; of course, it is understood that those skilled in the art can also obtain the above parameters through other measurement methods.

[0028] As a further improvement of the present invention, the thickness of the outer epidermis is 2-12 μm; the thickness of the inner epidermis is 1.5-10 μm.

[0029] The outer skin layer is a crucial area for retaining various fine impurities in ultrapure water. Most fine impurities are retained in the outer skin layer, therefore, the outer skin layer needs to have a certain thickness. If the thickness is too small, the membrane's retention efficiency will be greatly reduced, and the membrane's flux will also be greatly reduced (i.e., its service life will be shorter), failing to meet the needs of practical applications. In order to ensure retention efficiency, the internal pores of the outer skin layer must be relatively small, and the porosity must be low. Therefore, when the outer skin layer is too thick, the overall membrane flux will be significantly reduced. Meanwhile, during the terminal filtration of ultrapure water, the membrane itself is relatively clean, containing few impurity particles, and a very thick layer is not required. Therefore, the preferred thickness of the outer skin layer is 2-12 μm.

[0030] The inner skin layer is designed to further ensure the membrane's retention efficiency and reduce its own leaching, thus guaranteeing high retention efficiency. Therefore, the inner skin layer also needs to have a certain thickness. Furthermore, although the pores on the inner surface are slightly larger than those on the outer surface, the pore size within the inner skin layer is still relatively small, resulting in lower porosity. Therefore, the inner skin layer cannot be too thick, otherwise the overall membrane flux will be significantly reduced. The thickness of the inner skin layer is preferably 1.5-10 μm. Moreover, the outer skin layer is the main area for retaining impurity particles; therefore, the thickness of the outer skin layer is preferably greater than that of the inner skin layer, with the difference preferably being 0.5-5 μm. This further ensures that the membrane has high retention efficiency, high flux, and excellent mechanical strength.

[0031] The thickness of the outer epidermis and the inner epidermis, etc., of the present invention can be obtained by characterizing the morphology of the membrane cross section using a scanning electron microscope, and then selecting a certain area and measuring it using computer software (such as Matlab, NIS-Elements, etc.) or manually. The average value is then taken to further calculate the corresponding thickness value. Of course, it is understood that those skilled in the art can also obtain the above parameters through other measurement methods.

[0032] As a further improvement of the present invention, the outer skin layer includes an outer dense region and an outer porous region, the outer dense region includes an outer surface, and the outer porous region is located between the outer dense region and the outer void layer;

[0033] The thickness of the outer dense region is 0.2-2 μm; the ratio of the thickness of the outer dense region to the thickness of the outer porous region is 2%-20%; the outer porous region contains a first porous fiber forming a porous structure, and the SEM average diameter of the first porous fiber is 20-150 nm.

[0034] When ultrapure water undergoes terminal filtration, it is relatively clean, meaning it contains few minute impurities. Since some ultrapure water fluids contain very few impurity particles, a thick outer skin layer is unnecessary. Furthermore, the entire outer skin layer does not need to be dense (if the entire outer skin layer is thick and dense, it can easily reduce membrane flux). In other words, some areas can be less dense, especially the area near the outer porous layer. Preferably, the outer skin layer of a portion of the filter membrane includes an outer dense region and an outer porous region. The outer dense region includes the outer surface, while the outer porous region is located between the outer dense region and the outer porous layer. The outer dense region is the first part of the membrane bulk to come into contact with the fluid and is used to retain the fluid. The region containing fine impurities needs to be relatively dense to ensure high membrane retention efficiency, but its thickness does not need to be large. Preferably, it is 0.2-2 μm, and the ratio of the thickness of the outer dense region to the thickness of the outer porous region is 2%-20%. This density and ratio of the dense region ensures that the membrane not only has high retention efficiency and high flux, but also high mechanical strength. Most of the outer skin layer is the outer porous region, and its pores are not so dense. The average SEM diameter of the first porous fiber constituting the porous structure is 20-150 nm. The first fiber of this size can make the outer surface and the outer skin layer have good compressive strength, thereby ensuring that the membrane as a whole has high mechanical strength.

[0035] As a further improvement of the present invention, the inner epidermis layer includes an inner dense region and an inner porous region, the inner dense region includes an inner surface, and the inner porous region is located between the inner dense region and the inner void layer; the thickness of the inner dense region is 0.2-2 μm; the ratio of the thickness of the inner dense region to the thickness of the inner porous region is 4%-25%; the inner porous region has a second porous fiber forming a porous structure, and the SEM average diameter of the second porous fiber is 30-200 nm.

[0036] In some ultrapure water terminal filtration processes, both the outer and inner skin layers do not need to be entirely dense. A portion of the inner surface needs to be relatively dense (referred to as the inner dense region). This ensures sufficient retention of fine impurities in the ultrapure water and impurities dissolved from the membrane itself, resulting in highly clean ultrapure water suitable for applications in semiconductors and other fields. Research indicates that the thickness of the inner dense region is preferably 0.2-2 μm, and the ratio of its thickness to the thickness of the inner porous region is 4%-25%. This approach effectively retains various impurities while minimizing impact on flux. The remaining areas of the inner skin layer (referred to as the inner porous region) do not need to be as dense, which helps maintain flux.

[0037] The average SEM diameter of the second porous fiber constituting the porous structure in this region is 30-200 nm. The second fiber of such a fineness enables both the inner surface and the inner skin layer to have good compressive strength, thereby further ensuring that the membrane as a whole has high mechanical strength.

[0038] As a further improvement of the present invention, the thickness of the first intermediate layer is 3-20 μm and the average SEM pore size is 80-900 nm; the first intermediate layer has a first supporting fiber for forming a porous structure, and the average SEM diameter of the first supporting fiber is 20-500 nm.

[0039] The first intermediate layer is used to retain various tiny impurities in ultrapure water. Since ultrapure water itself is relatively clean (containing a small number of tiny impurities), most of the impurities it contains are already retained when the fluid passes through the outer skin layer. Therefore, the first intermediate layer does not need to be too thick, and its SEM average pore size does not need to be very small, otherwise it will have a certain impact on the overall membrane flux. After research, the preferred thickness of the first intermediate layer is 3-20 μm, and the SEM average pore size is 80-900 nm. With such thickness and membrane pore size working together, the overall membrane retention efficiency can be further guaranteed, resulting in a high overall membrane retention efficiency, while also ensuring good flux.

[0040] Compared to single-finger pore structures, membranes with double-finger pore structures exhibit better mechanical strength. This is because a relatively dense first intermediate layer exists between the outer and inner pore layers. The thickness of this first intermediate layer and the diameter of its internal fibers both affect the pore structure of the outer and inner pore layers and the overall mechanical strength of the membrane. In this invention, the average SEM diameter of the first supporting fiber is 20-500 nm. With the combined effect of this thickness, the stability of the pore structure of the outer and inner pore layers is ensured, enabling long-term high-efficiency filtration. Furthermore, the membrane as a whole possesses high mechanical strength, meeting the requirements of various processing methods and terminal filtration of ultrapure water under high pressure.

[0041] As a further improvement of the present invention, the outer void layer has a plurality of first finger-shaped pores distributed along the circumference of the membrane, and the inner void layer has a plurality of second finger-shaped pores distributed along the circumference of the membrane; the extension direction of the major axis of the first and second finger-shaped pores is radial to the hollow fiber membrane, and the extension direction of the minor axis of the first and second finger-shaped pores is circumferential to the hollow fiber membrane; the SEM average major axis of the first finger-shaped pores is 65-100 μm; and the SEM average major axis of the second finger-shaped pores is 40-80 μm.

[0042] Since the outer skin layer, the first intermediate layer, and the inner skin layer are all designed to trap minute impurities, the porosity of these regions is relatively low. To ensure the overall membrane has high porosity and thus high flux, this invention employs a finger-like pore structure for both the outer and inner pore layers. Specifically, the outer pore layer has a certain number of first finger-like pores (similar to finger-shaped holes with high internal porosity), and the inner pore layer has a certain number of second finger-like pores. Furthermore, a first intermediate layer exists between the outer and inner pore layers. This structure can be considered a double-finger-like pore structure. Compared to a single-finger-like pore structure, the membrane with the double-finger-like pore structure has higher mechanical strength and can... Maintaining membrane pore stability during long-term filtration (the lifespan of components in ultrapure water terminal filtration is generally calculated in years) and efficiently retaining various fine impurities is crucial. Simultaneously, both the first and second finger-shaped pores need suitable lengths and diameters. If the length and diameter are too large, it indicates excessively large pores in that area, causing the internal pores to easily collapse when fluid passes through, rendering the membrane fibers unusable. Furthermore, it also leads to low overall mechanical strength of the membrane, significantly increasing the difficulty of processing the membrane fibers into components and reducing its practicality. Conversely, if the length and diameter are too small, the overall membrane flux will still be relatively low, failing to meet actual application requirements.

[0043] As a further improvement of the present invention, the ratio of the SEM average major diameter of the first finger-shaped aperture to its SEM average minor diameter is 8-20; the ratio of the SEM average major diameter of the second finger-shaped aperture to its SEM average minor diameter is 7-23.

[0044] The ratio of the average major diameter of the first finger-shaped aperture to the average major diameter of the second finger-shaped aperture is 1.1-2.2; the ratio of the average major diameter of the second finger-shaped aperture to the average pore size of the intermediate void layer is 1.5-5.

[0045] Besides the influence of the long axis of the finger-shaped pores on the membrane's flux and mechanical strength, the short axis of the finger-shaped pores also affects these factors to some extent. Research has shown that by controlling the ratio of the SEM average long axis to the SEM average short axis of the first finger-shaped pore to 8-20 (i.e., the first finger-shaped pore has a suitable short axis, and the ratio of the long axis to the short axis is within a suitable range), the membrane can achieve a high flux, allowing fluid to pass through the membrane body in a shorter time. Simultaneously, this also ensures good pressure resistance of the outer void layer and high overall mechanical strength of the membrane. Similarly, by controlling the ratio of the SEM average long axis to the SEM average short axis of the second finger-shaped pores to 7-23, the inner void layer also exhibits good pressure resistance. Pressure strength; meanwhile, preferably, the ratio of the SEM average major diameter of the first finger pore to the SEM average major diameter of the second finger pore is 1.1-2.2, that is, the major diameter of the first finger pore is slightly longer than that of the second finger pore. This improves fluid filtration and ensures that the filter membrane can efficiently retain various fine impurities for a long time, resulting in a long service life. In addition, if there is an intermediate void layer in the filter membrane, it is preferable that the ratio of the SEM average major diameter of the second finger pore to the SEM average pore size of the intermediate void layer is 1.5-5. At this ratio, it is more conducive to ensuring that the membrane has both ultra-high retention efficiency and excellent flux, while also having low dissolution, making it particularly suitable for terminal filtration of ultrapure water.

[0046] As a further improvement of the present invention, the distance between two adjacent first finger-shaped holes is a first distance, and the average SEM length of the first distance is 0.5-5μm; the distance between two adjacent second finger-shaped holes is a second distance, and the average SEM length of the second distance is 0.2-3μm.

[0047] The first and second finger-shaped orifices contain regions with relatively large pores, while the regions between adjacent first finger-shaped orifices and adjacent second finger-shaped orifices contain regions with relatively small pores. The existence of these regions ensures that the fluid is less likely to collapse when passing through the first and second finger-shaped orifices. In other words, the present invention ensures that the outer void layer has good mechanical strength through an appropriate first distance, preventing the membrane pore structure from collapsing under pressure in the first finger-shaped orifices; and ensures that the inner void layer has good mechanical strength through an appropriate second distance, preventing the membrane pore structure from collapsing under pressure in the second finger-shaped orifices. The combined effect of the first and second distances maintains the stability of the membrane pores inside the outer and inner void layers, ensuring that the membrane has both high flux and good mechanical strength.

[0048] As a further improvement of the present invention, the filter membrane has a thickness of 120-300 μm and a porosity of 60%-90%; the filter membrane has a retention efficiency of greater than 95%, preferably greater than 99%, for impurity particles with a particle size of 2-100 nm; and the water flux of the filter membrane is not less than 25 L*h. -1*m -2 @psi;

[0049] The filter membrane has a tensile strength greater than 2 MPa and an elongation of 40%-70%.

[0050] The membrane thickness can be determined by characterizing the membrane structure using a scanning electron microscope, followed by calculation using computer software (such as Matlab, NIS-Elements, etc.) or manual measurement. When the membrane thickness is too small, its mechanical strength will be low, and the filtration time will be too short, resulting in ineffective filtration. Conversely, when the membrane thickness is too large, the filtration time will be too long, leading to excessive time costs. The filter membrane of this invention has a thickness of 120-300 μm, which is relatively large, ensuring not only high mechanical strength but also effective filtration and high retention efficiency. Commonly used porosity testing methods include mercury intrusion porosimetry, density method, and wet / dry membrane weighing method. Of course, those skilled in the art can also obtain the above parameters through other measurement methods; these methods are for reference only. Testing shows that the porosity of this filter membrane is 60%-90%, ensuring both high overall flux and fast filtration speed, while also having a high dirt-holding capacity, retaining a large number of impurity particles, and a long service life. This is used to evaluate the filter membrane machine. The key indicators of mechanical strength are the tensile strength and elongation at break of the filter membrane. Under certain conditions, the greater the tensile strength of the membrane, the better its mechanical strength. Tensile strength refers to the membrane's ability to withstand parallel tensile forces. During testing under certain conditions, the membrane sample is subjected to a tensile load until it breaks. Based on the maximum tensile load at the point of failure and the change in the membrane sample's dimensions (length), the tensile strength and elongation at break can be calculated. Both tensile strength and elongation at break can be measured using a universal tensile testing machine. The testing method for tensile strength is well-known in the field; for example, ASTM D790 or ISO 178 details the procedure for tensile strength testing. In this invention, the filter membrane exhibits a tensile strength greater than 2 MPa and an elongation at break of 40%-70%. This indicates that the ultrafiltration membrane of this invention possesses good tensile strength and elongation at break, demonstrating good mechanical properties, high industrial practical value, and the ability to fully meet market demands. Retention tests revealed that the filter membrane exhibits a retention efficiency greater than 95% for impurity particles with a diameter of 2-100 nm, with some membranes exceeding 99%, demonstrating exceptionally high retention efficiency. This makes it particularly suitable for terminal filtration of ultrapure water, resulting in highly purified ultrapure water. Water flux tests showed that the filter membrane of this invention has a water flux of no less than 25 L / h. -1 *m -2 @psi indicates a high flux, meaning the filter membrane has a good filtration speed and can produce a large volume of high-purity ultrapure water in a short time, resulting in high economic benefits.

[0051] In addition, the present invention also provides a method for preparing a polysulfone hollow fiber ultrafiltration membrane, comprising the following steps:

[0052] Step 1: Preparation of casting solution and core solution: The casting solution comprises the following components by weight: 15-25 parts of polysulfone, 15-40 parts of additives; 45-85 parts of a first organic solvent; the viscosity of the casting solution is 10,000-100,000 cps; the polysulfone is at least one of polyethersulfone, polysulfone, and polyphenylsulfone; the additive is an alcohol with a number average molecular weight of less than 1w; the core solution comprises a second organic solvent and a non-solvent; the content of the non-solvent in the core solution is 30%-60%; the non-solvent is water;

[0053] Step 2: Spinning: The casting solution and the core solution are extruded together from the die head, and the casting solution forms a molded product with an inner surface and an outer surface in the die head;

[0054] Step 3: Pretreatment: The molded article is placed in a treatment bath for pretreatment for 10-40 seconds; the treatment bath is at least one of polyvinyl alcohol, ethylene glycol, propylene glycol, isopropanol, diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, dipropylene glycol, tripropylene glycol, polypropylene glycol, glycerin, ethylene glycol monomethyl ether, ethylene glycol dimethyl ether, and diethylene glycol;

[0055] Step 4: Phase Separation: The pretreated molded product is placed in a gel bath for phase separation to form a biological film. The phase separation time is 60-180 seconds. The gel bath is water.

[0056] Step 5: Wash the raw membrane in water and dry it to obtain a hollow fiber ultrafiltration membrane.

[0057] As a further improvement of the present invention, the first organic solvent and the second organic solvent are both at least one of dimethyl sulfoxide, dimethylformamide, N-ethylpyrrolidone, dimethylacetamide, and N-methylpyrrolidone; the additive is at least one of polyvinyl alcohol, ethylene glycol, propylene glycol, isopropanol, diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, dipropylene glycol, tripropylene glycol, polypropylene glycol, glycerol, ethylene glycol monomethyl ether, ethylene glycol dimethyl ether, and diethylene glycol.

[0058] As a further improvement of the present invention, the temperature of the casting solution is 35-45°C, the temperature of the core solution is 20-30°C, and the temperature of the gel bath is 25-65°C.

[0059] As a further improvement of the present invention, the die head stretch ratio is 2-5 and the winding speed is 5-20m / min during spinning.

[0060] In preparing the polysulfone-based hollow fiber ultrafiltration membrane of the present invention, a casting solution is first prepared. The casting solution includes a membrane-forming substance, a polysulfone substance (at least one of polyethersulfone, polysulfone, and polyphenylsulfone), an organic solvent (for dissolving the polysulfone substance), and an additive. As one of the key points of the present invention, the additive is an alcohol with a number average molecular weight of less than 1w (it can be a polymeric alcohol or a small molecule alcohol, preferably with a molecular weight of less than 1000). Preferably, the additive is at least one of polyvinyl alcohol, ethylene glycol, propylene glycol, isopropanol, diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, dipropylene glycol, tripropylene glycol, polypropylene glycol, glycerol, ethylene glycol monomethyl ether, ethylene glycol dimethyl ether, and diethylene glycol (it can be one type or more). (Multiple substances are combined); by adding a certain mass of additives to the casting solution and then performing a suitable phase separation process, a double-finger pore structure is formed, thereby forming an ultrafiltration membrane with at least three retention layers; at the same time, studies have found that the addition of additives has a certain improvement effect on the membrane flux and mechanical strength; the viscosity of the casting solution needs to be controlled at 10,000-100,000 cps, as the viscosity of the casting solution has a significant impact on the structure and performance of the final filter membrane, such as affecting the pore size, thickness, and flow rate; thus ensuring that the final filter membrane has an ideal pore structure and pore size, and can then be applied to terminal ultrapure water filtration; in addition, the hollow fiber membrane extrusion process in this invention uses a liquid core.

[0061] Therefore, it is necessary to select a suitable core solution, which includes organic solvents and non-solvents. The organic solvent is preferably the organic solvent in the casting solution, but other solvents that can dissolve the membrane-forming substances can also be used. The non-solvent is water. By selecting a suitable core solution (the corresponding substances and their proportions), on the one hand, it is possible to ensure that the pressure inside the hollow fiber membrane cavity is balanced with the external pressure, thereby stabilizing the cavity of the hollow fiber membrane and making the wall thickness of the hollow fiber membrane basically the same. On the other hand, the core solution also affects the pore size and pore size distribution on the inner surface. Under the combined action of conditions such as the coagulation bath, by controlling the changes in the membrane phase separation process, a filter membrane with an ideal inner surface pore structure can be manufactured, making the filter membrane suitable for ultrapure water terminal filtration.

[0062] The second step is spinning: the casting solution and the core solution are extruded together from the die head, and the casting solution forms a molded product with an inner surface and an outer surface in the die head; this molded product is a hollow fiber membrane; the extruded hollow fiber membrane has a surface facing the cavity, i.e., the inner surface, and a surface opposite to the cavity, i.e., the outer surface; in ultrapure water terminal filtration, one of the most important performance characteristics is the retention efficiency, and some defects generated during the membrane making process can affect the retention efficiency, so it is necessary to minimize the defects generated during the membrane making process; in this invention, the outer skin layer is the key to retaining tiny impurities in ultrapure water. Therefore, during film fabrication, it is essential to ensure that the outer skin layer of the film is virtually free of defects. Through research, this invention utilizes a two-bath method to prepare asymmetric films with virtually defect-free outer skin layers. The key to this process is to first pre-treat the molded product in a treatment bath for 10-40 seconds. The treatment bath contains at least one of the following: polyvinyl alcohol, ethylene glycol, propylene glycol, isopropanol, diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, dipropylene glycol, tripropylene glycol, polypropylene glycol, glycerol, ethylene glycol monomethyl ether, ethylene glycol dimethyl ether, and diethylene glycol. Through this appropriate treatment, a high polymer concentration can be achieved on the outer surface of the membrane. Then, a gel bath gelation (phase separation) is performed, resulting in relatively small pores on the outer surface and a virtually defect-free outer skin layer. The formation of the intermediate void layer occurs because when both the inner and outer surfaces of the membrane are relatively dense, the solvent in the middle layer has difficulty diffusing, the phase separation rate becomes very slow, and relatively large pores are formed. Finally, the membrane is washed in water to further remove organic solvents and other substances contained in the membrane fibers, and then dried (either naturally or by other methods), resulting in the final membrane. A hollow fiber ultrafiltration membrane is obtained, which has at least three retention layers, and its outer surface and outer skin layer are basically free of defects, thus ensuring that the membrane has an ultra-high retention efficiency. Preferably, the casting solution temperature is 35-45℃, the core solution temperature is 20-30℃, and the gel bath temperature is 25-65℃. Under such temperature conditions, combined with the appropriate casting solution formulation and the dual-bath effect, ideal pore size and pore area ratio are achieved on both the inner and outer surfaces. This further ensures the membrane's retention efficiency, while also giving the membrane good flux and excellent mechanical strength. Preferably, the die stretch ratio during spinning is 2-5, and the winding speed is 5-20 m / min. Studies have shown that the die stretch ratio and winding speed have a certain impact on the uniformity of membrane pores. Under such stretch ratio and winding speed, combined with the corresponding casting solution formula and phase separation process, the membrane pores can be made more uniform, without the appearance of particularly small or large pores (fewer defects), thus ensuring that the filter membrane has both high retention efficiency and good filtration speed.

[0063] As a further improvement of the present invention, an application of a polysulfone hollow fiber ultrafiltration membrane is provided, wherein the ultrafiltration membrane is used for terminal filtration in the preparation of ultrapure water.

[0064] The beneficial effects of this invention are as follows: The polysulfone hollow fiber ultrafiltration membrane provided by this invention is made of polysulfone materials and has a certain degree of hydrophilicity, making it easy to be quickly wetted by ultrapure water, thereby achieving stable filtration. The membrane comprises a main body, which includes at least an outer skin layer, an outer pore layer, a first intermediate layer, an inner pore layer, and an inner skin layer. The outer skin layer, the first intermediate layer, and the inner skin layer all have tortuous pathways, serving as regions for trapping impurity particles, and each layer has a thickness of not less than 1 μm. Furthermore, the average SEM pore size of the outer surface is not greater than 60 nm; the average SEM pore size of the inner surface is... The hollow fiber membrane has a pore size of 20-250 nm. By having suitable pore sizes on both its inner and outer surfaces, and by including at least three layers of regions capable of trapping various fine impurities, the membrane achieves high efficiency in trapping various fine impurities in ultrapure water, with a trapping efficiency greater than 95%, preferably greater than 99%. Simultaneously, both the outer and inner pore layers have finger-like pore structures, and the overall porosity of the hollow fiber membrane is not less than 50%, ensuring high flux. This ideal membrane structure makes the ultrafiltration membrane particularly suitable for terminal filtration of ultrapure water, ensuring the preparation of ultrapure water with high purity. This hollow fiber membrane has an ideal membrane structure, with suitable pore sizes on both its inner and outer surfaces and a high overall porosity, ensuring high trapping efficiency for various nanoscale impurities in water, while also having high flux, making it particularly suitable for terminal filtration of ultrapure water. The preparation method provided by this invention can conveniently, quickly, and effectively prepare the above-mentioned polysulfone hollow fiber ultrafiltration membrane. Attached Figure Description

[0065] Figure 1 A scanning electron microscope (SEM) image of the overall cross-section of the ultrafiltration membrane was prepared for Example 6, with a magnification of 50×.

[0066] Figure 2 The image shown is a scanning electron microscope (SEM) image of the outer skin layer (which includes an outer dense region and an outer porous region) of the ultrafiltration membrane prepared in Example 6, with a magnification of 10K×.

[0067] Figure 3 The image shows a scanning electron microscope (SEM) image of the first intermediate layer in the ultrafiltration membrane prepared in Example 6, with a magnification of 20K×.

[0068] Figure 4 The image shown is a scanning electron microscope (SEM) image of the inner skin layer (which includes an inner dense region and an inner porous region) of the ultrafiltration membrane prepared in Example 6, with a magnification of 20K×.

[0069] Figure 5 A scanning electron microscope (SEM) image of the overall cross-section of the ultrafiltration membrane was prepared for Example 8, with a magnification of 500×; (the boxes in the image represent the intermediate void layer and the second intermediate layer);

[0070] Figure 6 The image shows a scanning electron microscope (SEM) image of the outer surface of the ultrafiltration membrane prepared in Example 3, with a magnification of 50K×.

[0071] Figure 7 The image shows a scanning electron microscope (SEM) image of the inner surface of the ultrafiltration membrane prepared in Example 3, with a magnification of 20K×.

[0072] Figure 8 This is a schematic diagram of the hollow fiber ultrafiltration membrane flux testing device of the present invention. Detailed Implementation

[0073] To more clearly illustrate the overall concept of this application, detailed descriptions are provided below using embodiments. Unless otherwise specified, the raw materials and equipment used to prepare the filter membrane in the following embodiments are commercially available. Specifically, a Hitachi S-5500 scanning electron microscope was used to characterize the structural morphology of the filter membrane.

[0074] Example 1: A method for preparing a polysulfone hollow fiber ultrafiltration membrane, comprising the following steps:

[0075] Step 1: Preparation of casting solution and core solution: The casting solution consists of the following components by weight: 25 parts polysulfone, 36 parts additives, 50 parts first organic solvent; the viscosity of the casting solution is 80,000 cps;

[0076] The polysulfone substance is polyethersulfone; the additive is polyvinyl alcohol.

[0077] The core fluid includes a second organic solvent and a non-solvent; the content of the non-solvent in the core fluid is 55%; the non-solvent is water;

[0078] Both the first and second organic solvents are dimethyl sulfoxide;

[0079] The casting solution temperature is 40℃, the core solution temperature is 25℃, and the gel bath temperature is 25℃.

[0080] Step 2: Spinning: The casting solution and the core solution are extruded together from the die head, and the casting solution forms a molded product with an inner surface and an outer surface in the die head; during spinning, the die head has a stretch ratio of 2 and a winding speed of 18m / min;

[0081] Step 3: Pretreatment: Place the molded article in a treatment bath for pretreatment for 10-40 seconds; the treatment bath is polyvinyl alcohol.

[0082] Step 4: Phase Separation: The pretreated molded product is placed in a gel bath for phase separation to form a biological film. The phase separation time is 65 seconds. The gel bath is water.

[0083] Step 5: Wash the raw membrane in water and dry it to obtain a hollow fiber ultrafiltration membrane.

[0084] Example 2: A method for preparing a polysulfone hollow fiber ultrafiltration membrane, comprising the following steps:

[0085] Step 1: Preparation of casting solution and core solution: The casting solution comprises the following components by weight: 22 parts polysulfone, 20 parts additives; 55 parts first organic solvent; the viscosity of the casting solution is 60,000 cps; the polysulfone is polyethersulfone; the core solution comprises a second organic solvent and a non-solvent; the content of the non-solvent in the core solution is 50%; the non-solvent is water; both the first and second organic solvents are dimethylformamide; the additive is ethylene glycol; the temperature of the casting solution is 40°C, the temperature of the core solution is 25°C; the temperature of the gel bath is 35°C.

[0086] Step 2: Spinning: The casting solution and the core solution are extruded together from the die head, and the casting solution forms a molded product with an inner surface and an outer surface in the die head; the die head stretch ratio is 2 and the winding speed is 16m / min during spinning;

[0087] Step 3: Pretreatment: Place the molded article in a treatment bath for pretreatment for 30 seconds; the treatment bath is ethylene glycol.

[0088] Step 4: Phase Separation: Place the pretreated molded product into a gel bath for phase separation to form a biological film. The phase separation time is 70 seconds. The gel bath is water.

[0089] Step 5: Wash the raw membrane in water and dry it to obtain a hollow fiber ultrafiltration membrane.

[0090] Example 3: A method for preparing a polysulfone hollow fiber ultrafiltration membrane, comprising the following steps:

[0091] Step 1: Preparation of casting solution and core solution: The casting solution comprises the following components by weight: 20 parts polysulfone, 34 parts additives; 60 parts first organic solvent; the viscosity of the casting solution is 60,000 cps; the polysulfone is polyethersulfone; the core solution comprises a second organic solvent and a non-solvent; the content of the non-solvent in the core solution is 45%; the non-solvent is water; both the first and second organic solvents are N-ethylpyrrolidone; the additive is dipropylene glycol;

[0092] The casting solution temperature is 40℃; the core solution temperature is 25℃; and the gel bath temperature is 30℃.

[0093] Step 2: Spinning: The casting solution and the core solution are extruded together from the die head, and the casting solution forms a molded product with an inner surface and an outer surface in the die head; the die head stretch ratio is 3 and the winding speed is 12m / min during spinning;

[0094] Step 3: Pretreatment: The molded article is placed in a treatment bath for pretreatment for 28 seconds; the treatment bath is dipropylene glycol.

[0095] Step 4: Phase Separation: Place the pretreated molded product into a gel bath for phase separation to form a biological film. The phase separation time is 80 seconds. The gel bath is water.

[0096] Step 5: Wash the raw membrane in water and dry it to obtain a hollow fiber ultrafiltration membrane.

[0097] Example 4: A method for preparing a polysulfone hollow fiber ultrafiltration membrane, comprising the following steps:

[0098] Step 1: Preparation of casting solution and core solution: The casting solution comprises the following components by weight: 18 parts polysulfone, 25 parts additives; 65 parts first organic solvent; the viscosity of the casting solution is 40000 cps; the polysulfone is polysulfone; the core solution comprises a second organic solvent and a non-solvent; the content of the non-solvent in the core solution is 40%; the non-solvent is water; both the first and second organic solvents are dimethylacetamide; the additive is polyethylene glycol-600;

[0099] The casting solution temperature is 35℃, the core solution temperature is 20℃, and the gel bath temperature is 45℃.

[0100] Step 2: Spinning: The casting solution and the core solution are extruded together from the die head, and the casting solution forms a molded product with an inner surface and an outer surface in the die head; during spinning, the die head has a stretch ratio of 3 and a winding speed of 15m / min;

[0101] Step 3: Pretreatment: Place the molded product in a treatment bath for pretreatment for 25 seconds; the treatment bath is polyethylene glycol.

[0102] Step 4: Phase Separation: Place the pretreated molded product into a gel bath for phase separation to form a biological film. The phase separation time is 100 seconds. The gel bath is water.

[0103] Step 5: Wash the raw membrane in water and dry it to obtain a hollow fiber ultrafiltration membrane.

[0104] Example 5: A method for preparing a polysulfone-based hollow fiber ultrafiltration membrane, comprising the following steps:

[0105] Step 1: Preparation of casting solution and core solution: The casting solution comprises the following components by weight: 18 parts polysulfone, 32 parts additives; 70 parts first organic solvent; the viscosity of the casting solution is 40000 cps; the polysulfone is polysulfone; the core solution comprises a second organic solvent and a non-solvent; the content of the non-solvent in the core solution is 35%; the non-solvent is water; both the first and second organic solvents are N-methylpyrrolidone; the additive is glycerol;

[0106] The casting solution temperature is 35℃, the core solution temperature is 20℃, and the gel bath temperature is 40℃.

[0107] Step 2: Spinning: The casting solution and the core solution are extruded together from the die head, and the casting solution forms a molded product with an inner surface and an outer surface in the die head; during spinning, the die head has a stretch ratio of 3 and a winding speed of 9 m / min;

[0108] Step 3: Pretreatment: Place the molded article in a treatment bath for pretreatment for 20 seconds; the treatment bath is glycerin.

[0109] Step 4: Phase Separation: The pretreated molded product is placed in a gel bath for phase separation to form a biological film. The phase separation time is 120 seconds. The gel bath is water.

[0110] Step 5: Wash the raw membrane in water and dry it to obtain a hollow fiber ultrafiltration membrane.

[0111] Example 6: A method for preparing a polysulfone hollow fiber ultrafiltration membrane, comprising the following steps:

[0112] Step 1: Preparation of casting solution and core solution: The casting solution comprises the following components by weight: 16 parts polysulfone, 18 parts additives; 80 parts first organic solvent; the viscosity of the casting solution is 20000 cps; the polysulfone is polyethersulfone; the core solution includes a second organic solvent and a non-solvent; the content of water in the non-solvent of the core solution is 30%; the first organic solvent is N-methylpyrrolidone; the second organic solvent is N-ethylpyrrolidone; the additive is ethylene glycol monomethyl ether; the temperature of the casting solution is 45℃; the temperature of the core solution is 30℃; the temperature of the gel bath is 50℃.

[0113] Step 2: Spinning: The casting solution and the core solution are extruded together from the die head, and the casting solution forms a molded product with an inner surface and an outer surface in the die head; during spinning, the die head has a stretch ratio of 4 and a winding speed of 8 m / min;

[0114] Step 3: Pretreatment: The molded article is placed in a treatment bath for pretreatment for 14 seconds; the treatment bath is ethylene glycol monomethyl ether.

[0115] Step 4: Phase Separation: The pretreated molded product is placed in a gel bath for phase separation to form a biological film. The phase separation time is 150 seconds. The gel bath is water.

[0116] Step 5: Wash the raw membrane in water and dry it to obtain a hollow fiber ultrafiltration membrane.

[0117] Example 7: A method for preparing a polysulfone hollow fiber ultrafiltration membrane, comprising the following steps:

[0118] Step 1: Preparation of casting solution and core solution: The casting solution comprises the following components by weight: 15 parts polyphenylsulfone (PPS), 22 parts additives; 85 parts first organic solvent; the viscosity of the casting solution is 20,000 cps; the core solution comprises a second organic solvent and a non-solvent; the content of water in the non-solvent of the core solution is 35%; the first organic solvent is dimethylacetamide; the second organic solvent is dimethylformamide; the additive is diethylene glycol.

[0119] The casting solution temperature is 45℃; the core solution temperature is 30℃; and the gel bath temperature is 55℃.

[0120] Step 2: Spinning: The casting solution and the core solution are extruded together from the die head, and the casting solution forms a molded product with an inner surface and an outer surface in the die head; during spinning, the die head has a stretch ratio of 4 and a winding speed of 8 m / min;

[0121] Step 3: Pretreatment: The molded article is placed in a treatment bath for pretreatment for 12 seconds; the treatment bath is diethylene glycol.

[0122] Step 4: Phase Separation: The pretreated molded product is placed in a gel bath for phase separation to form a biological film. The phase separation time is 160 seconds. The gel bath is water.

[0123] Step 5: Wash the raw membrane in water and dry it to obtain a hollow fiber ultrafiltration membrane.

[0124] Example 8: A method for preparing a polysulfone hollow fiber ultrafiltration membrane, comprising the following steps:

[0125] Step 1: Preparation of casting solution and core solution: The casting solution comprises the following components by weight: 17 parts polysulfone, 28 parts additives; 75 parts first organic solvent; the viscosity of the casting solution is 25000 cps; the polysulfone is polysulfone; the core solution comprises a second organic solvent and a non-solvent; the content of the non-solvent in the core solution is 35%; the non-solvent is water; both the first and second organic solvents are N-ethylpyrrolidone; the additive is isopropanol;

[0126] The casting solution temperature was 42℃; the core solution temperature was 28℃; and the gel bath temperature was 53℃.

[0127] Step 2: Spinning: The casting solution and the core solution are extruded together from the die head. The casting solution forms a molded product with an inner surface and an outer surface in the die head. During spinning, the die head stretch ratio is 4 and the winding speed is 6m / min.

[0128] Step 3: Pretreatment: The molded article is placed in a treatment bath for pretreatment for 11 seconds; the treatment bath is isopropanol.

[0129] Step 4: Phase Separation: Place the pretreated molded product into a gel bath for phase separation to form a biological film. The phase separation time is 170 seconds. The gel bath is water.

[0130] Step 5: Wash the raw membrane in water and dry it to obtain a hollow fiber ultrafiltration membrane.

[0131] Observation revealed that the ultrafiltration membrane prepared in Example 8 also has four regions for retaining colloidal gold, namely, an outer skin layer, a first intermediate layer, a second intermediate layer, and an inner skin layer; however, the second intermediate layer is not continuous, and some areas cannot retain the corresponding fine impurities, but most areas can retain fine impurities, thus still improving the membrane's retention efficiency.

[0132] Comparative Example 1: A method for preparing a polysulfone-based hollow fiber ultrafiltration membrane, comprising the following steps:

[0133] Step 1: Preparation of casting solution and core solution: The casting solution comprises the following components by weight: 15 parts polysulfone, 22 parts additives; 85 parts first organic solvent; the viscosity of the casting solution is 20000 cps; the polysulfone is polyphenylsulfone; the core solution comprises a second organic solvent and a non-solvent; the content of the non-solvent in the core solution is 20%; the non-solvent is water; the first organic solvent is dimethylacetamide; the second organic solvent is dimethylformamide;

[0134] The additive is diethylene glycol; the casting solution temperature, core solution temperature, and gel bath temperature are all 40°C.

[0135] Step 2: Spinning: The casting solution and the core solution are extruded together from the die head, and the casting solution forms a molded product with an inner surface and an outer surface in the die head; during spinning, the die head has a stretch ratio of 8 and a winding speed of 16 m / min;

[0136] Step 3: Phase separation: The pretreated molded product is placed in a gel bath for phase separation to form a biological film. The phase separation time is 160 seconds. The gel bath is water.

[0137] Step 4: Wash the raw membrane in water and dry it to obtain a hollow fiber ultrafiltration membrane with a double-finger pore structure.

[0138] Comparative Example 2: A method for preparing a polysulfone-based hollow fiber ultrafiltration membrane, comprising the following steps:

[0139] Step 1: Preparation of casting solution and core solution: The casting solution comprises the following components by weight: 18 parts polysulfone, 85 parts first organic solvent; the viscosity of the casting solution is 30000 cps; the polysulfone is polyphenylsulfone; the core solution comprises a second organic solvent and a non-solvent; the content of the non-solvent in the core solution is 35%; the non-solvent is water; the first organic solvent is dimethylacetamide; the second organic solvent is dimethylformamide; the temperature of the casting solution, the core solution, and the gel bath are all 45℃.

[0140] Step 2: Spinning: The casting solution and the core solution are extruded together from the die head, and the casting solution forms a molded product with an inner surface and an outer surface in the die head; during spinning, the die head has a stretch ratio of 8 and a winding speed of 16m / min.

[0141] Step 3: Pretreatment: The molded article is placed in a treatment bath for pretreatment for 12 seconds; the treatment bath is diethylene glycol.

[0142] Step 4: Phase Separation: The pretreated molded product is placed in a gel bath for phase separation to form a biological film. The phase separation time is 160 seconds. The gel bath is water.

[0143] Step 5: Wash the raw membrane in water and dry it to obtain a hollow fiber ultrafiltration membrane. Because no alcohol additives were added to the formula, the final ultrafiltration membrane lacks a double-finger pore structure, resulting in a retention efficiency of less than 95% for 50nm impurity particles, and its flux is far less than 25 L*h. -1 *m -2 @psi, therefore this ultrafiltration membrane has no practical value and cannot be used for terminal filtration of ultrapure water.

[0144] 1. Structural Characterization

[0145] The morphology of the PES hollow fiber membranes obtained in each embodiment was characterized using scanning electron microscopy, and the required data were then obtained; the specific results are shown in the table below:

[0146] Table 1:

[0147]

[0148] Table 2

[0149]

[0150]

[0151] Table 3

[0152]

[0153] Table 4

[0154]

[0155] The filter membranes prepared in Examples 1, 3, 5 and 8 all have an intermediate void layer and a second intermediate layer, that is, they have four regions for trapping tiny impurity particles, which is beneficial to obtaining higher trapping efficiency.

[0156] Table 5

[0157]

[0158] As shown in Tables 1-5, the hollow fiber ultrafiltration membranes prepared in Examples 1-8 of this invention are all integrally formed without composite processes, making the preparation process simple and suitable for large-scale application. Furthermore, the ultrafiltration membranes prepared in Examples 1-8 all have ideal membrane structures, with suitable pore sizes and pore areas on both the inner and outer surfaces, and at least three layers of retention areas, ensuring high-quality retention of various impurities. Their retention efficiency reaches over 95%, preferably over 99%, making them particularly suitable for terminal filtration of ultrapure water.

[0159] Performance characteristics

[0160] Membrane flux is calculated as follows: The formula for calculating membrane flux (J) is: J = V / (T × A) Where:

[0161] J -- Membrane flux unit: L*h -1 *m -2

[0162] V -- Sampling volume (L); T -- Sampling time (h); A -- Effective membrane area (m2)

[0163] The operating conditions used for measuring the membrane separation performance in this invention are as follows: the feed solution is deionized water, the operating pressure is 1 psi, the operating temperature is 25°C, and the solution pH is 7; Figure 8 As shown;

[0164] Retention test: The retention efficiency of the filter membranes obtained in each example was tested; wherein: the particle size of the material retained in Example 1 was 5 nm; the particle size of the material retained in Examples 2 and 3 was 10 nm; the particle size of the material retained in Examples 4 and 5 was 20 nm; and the particle size of the material retained in Examples 6, 7, 8 and Comparative Example 1 was 50 nm.

[0165]

[0166] As shown in the table above, the hollow fiber ultrafiltration membranes prepared in Examples 1-8 of this invention have high flux and high retention efficiency, as well as good mechanical strength, making them particularly suitable for terminal filtration of ultrapure water. In addition, various leaching tests were conducted, and the tests showed that TOC leaching was less than 0.5 ppb and metal ion precipitation was less than 1 ppt. The membrane fibers themselves are very clean and will not introduce new impurities, further ensuring the production of ultrapure water with high purity.

[0167] The above description is merely a preferred embodiment of the present invention. The scope of protection of the present invention is not limited to the above embodiments. All technical solutions falling within the scope of the present invention's concept are within the scope of protection of the present invention. It should be noted that for those skilled in the art, any improvements and modifications made without departing from the principles of the present invention should also be considered within the scope of protection of the present invention.

Claims

1. A polysulfone hollow fiber ultrafiltration membrane, comprising a body, wherein one side of the body is an inner surface facing the inner lumen, and the other side of the body is an outer surface, characterized in that, In the direction from the outer surface to the inner surface, the main body sequentially includes an outer skin layer, an outer void layer, a first intermediate layer, an inner void layer, and an inner skin layer; one side of the outer skin layer is the outer surface; One side of the inner epidermis is the inner surface; The outer epidermis, the first intermediate layer and the inner epidermis all have tortuous pathways, which are all regions used to trap impurity particles, and the thickness of each layer is not less than 1 μm. Both the outer void layer and the inner void layer have a finger-shaped pore structure; The average SEM pore size of the outer surface is no greater than 60 nm; The average SEM pore size of the inner surface is 20-250 nm; and the average SEM pore size of the inner surface is greater than that of the outer surface. The overall porosity of the filter membrane is not less than 50%; The filter membrane is an external pressure ultrafiltration membrane; The thickness of the first intermediate layer is 3-20 μm, and the average pore size under SEM is 80-900 nm; the first intermediate layer contains a first supporting fiber for forming a porous structure, and the average diameter of the first supporting fiber under SEM is 20-500 nm.

2. The polysulfone hollow fiber ultrafiltration membrane according to claim 1, characterized in that, The average SEM pore size of the outer surface is 1-50 nm, and the pore area ratio is 0.1%-10%.

3. The polysulfone hollow fiber ultrafiltration membrane according to claim 1, characterized in that, The ratio of the average SEM aperture of the inner surface to the average SEM aperture of the outer surface is 2-15. The pore area ratio of the inner surface is 2%-15% larger than that of the outer surface.

4. The polysulfone hollow fiber ultrafiltration membrane according to claim 1, characterized in that, The main body also includes an intermediate void layer and a second intermediate layer. The intermediate void layer is located on the side of the first intermediate layer away from the outer void layer. The second intermediate layer is located between the intermediate void layer and the inner void layer. The second intermediate layer has tortuous pathways, which are areas for trapping impurity particles. The thickness of the intermediate void layer is 15-45 μm, and its average SEM pore size is 3-35 μm. The thickness of the second intermediate layer is 0.5-10 μm.

5. The polysulfone hollow fiber ultrafiltration membrane according to claim 4, characterized in that, The ratio of the thickness of the intermediate void layer to the thickness of the second intermediate layer is 3-10; The sum of the thickness of the intermediate void layer and the thickness of the second intermediate layer is 5%-20% of the total thickness of the membrane; The ratio of the average SEM pore size of the intermediate void layer to the average SEM pore size of the second intermediate layer is 10-80.

6. The polysulfone hollow fiber ultrafiltration membrane according to claim 4, characterized in that, The second intermediate layer contains a second supporting fiber for forming a porous structure, the SEM average diameter of the second supporting fiber is 30-600 nm; the SEM average pore size of the second intermediate layer is 60-800 nm.

7. The polysulfone hollow fiber ultrafiltration membrane according to claim 1, characterized in that, The outer epidermis has a thickness of 2-12 μm; the inner epidermis has a thickness of 1.5-10 μm.

8. The polysulfone hollow fiber ultrafiltration membrane according to claim 1, characterized in that, The outer skin layer includes an outer dense region and an outer porous region. The outer dense region includes an outer surface, and the outer porous region is located between the outer dense region and the outer void layer. The thickness of the outer dense region is 0.2-2 μm; the ratio of the thickness of the outer dense region to the thickness of the outer porous region is 2%-20%. The outer porous region contains a first porous fiber forming a porous structure, and the SEM average diameter of the first porous fiber is 20-150 nm.

9. A polysulfone hollow fiber ultrafiltration membrane according to claim 1, characterized in that, The inner epidermis layer includes an inner dense region and an inner porous region. The inner dense region includes an inner surface, and the inner porous region is located between the inner dense region and the inner void layer. The thickness of the inner dense region is 0.2-2 μm; the ratio of the thickness of the inner dense region to the thickness of the inner porous region is 4%-25%. The inner porous region contains a second porous fiber that forms a porous structure, and the SEM average diameter of the second porous fiber is 30-200 nm.

10. A polysulfone hollow fiber ultrafiltration membrane according to claim 4, characterized in that, The outer void layer has a plurality of first finger-shaped pores distributed along the circumference of the membrane, and the inner void layer has a plurality of second finger-shaped pores distributed along the circumference of the membrane. The major axis of the first and second finger-shaped pores extends in the radial direction of the hollow fiber ultrafiltration membrane, and the minor axis of the first and second finger-shaped pores extends in the circumferential direction of the hollow fiber ultrafiltration membrane. The average major diameter of the first finger-shaped aperture is 65-100 μm according to SEM. The average major diameter of the second finger-shaped aperture is 40-80 μm according to SEM.

11. A polysulfone hollow fiber ultrafiltration membrane according to claim 10, characterized in that, The ratio of the SEM average major axis to the SEM average minor axis of the first finger-shaped aperture is 8-20. The ratio of the SEM average major axis to the SEM average minor axis of the second finger-shaped aperture is 7-23. The ratio of the average major diameter of the first finger-shaped aperture to the average major diameter of the second finger-shaped aperture via SEM is 1.1-2.

2. The ratio of the average major diameter of the second finger-shaped hole to the average pore diameter of the intermediate void layer is 1.5-5.

12. The polysulfone hollow fiber ultrafiltration membrane according to claim 10, characterized in that, The distance between two adjacent first finger-shaped apertures is the first distance, and the average length of the first distance in SEM is 0.5-5μm; The distance between two adjacent second finger-shaped apertures is called the second distance, and the average length of the second distance in SEM is 0.2-3 μm.

13. The polysulfone hollow fiber ultrafiltration membrane according to claim 1, characterized in that, The filter membrane has a thickness of 120-300 μm and a porosity of 60%-90%. The filter membrane has a rejection efficiency of more than 95% for impurity particles with a diameter of 2-100 nm. The water flux of the filter membrane is not less than 25 L*h -1 *m -2 @psi; The filter membrane has a tensile strength greater than 2 MPa and an elongation of 40%-70%.

14. The polysulfone hollow fiber ultrafiltration membrane according to claim 13, characterized in that, The filter membrane has a rejection efficiency of more than 99% for impurity particles with a diameter of 2-100 nm.

15. A method for preparing a polysulfone hollow fiber ultrafiltration membrane according to any one of claims 1-14, characterized in that, Includes the following steps: Step 1: Preparation of casting solution and core solution: The casting solution comprises the following components by weight: 15-25 parts of polysulfone, 15-40 parts of additives, and 45-85 parts of a first organic solvent; the viscosity of the casting solution is 10,000-100,000 cps. The polysulfone is at least one of polyethersulfone, polysulfone and polyphenylsulfone; The additive is an alcohol with a number average molecular weight of less than 1w; The core fluid includes a second organic solvent and a non-solvent; the content of the non-solvent in the core fluid is 30%-60%; the non-solvent is water; Step 2: Spinning: The casting solution and the core solution are extruded together from the die head, and the casting solution forms a molded product with an inner surface and an outer surface in the die head; Step 3: Pretreatment: The molded article is placed in a treatment bath for pretreatment for 10-40 seconds; the treatment bath is at least one of polyvinyl alcohol, ethylene glycol, propylene glycol, isopropanol, diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, dipropylene glycol, tripropylene glycol, polypropylene glycol, glycerol, ethylene glycol monomethyl ether, ethylene glycol dimethyl ether, and diethylene glycol; Step 4: Phase separation: The pretreated molded product is placed in a gel bath for phase separation to form a biological film. The phase separation time is 60-180 seconds. The gel bath is water. Step 5: Wash the raw membrane in water and dry it to obtain a hollow fiber ultrafiltration membrane.

16. The method for preparing a polysulfone hollow fiber ultrafiltration membrane according to claim 15, characterized in that, Both the first organic solvent and the second organic solvent are at least one selected from dimethyl sulfoxide, dimethylformamide, N-ethylpyrrolidone, dimethylacetamide, and N-methylpyrrolidone; The additive is at least one of polyvinyl alcohol, ethylene glycol, propylene glycol, isopropanol, diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, dipropylene glycol, tripropylene glycol, polypropylene glycol, glycerin, ethylene glycol monomethyl ether, ethylene glycol dimethyl ether, and diethylene glycol.

17. The method for preparing a polysulfone hollow fiber ultrafiltration membrane according to claim 15, characterized in that, The temperature of the casting solution is 35-45℃, the temperature of the core solution is 20-30℃, and the temperature of the gel bath is 25-65℃.

18. The method for preparing a polysulfone hollow fiber ultrafiltration membrane according to claim 15, characterized in that, During spinning, the die head has a stretch ratio of 2-5 and a winding speed of 5-20 m / min.

19. The application of a polysulfone hollow fiber ultrafiltration membrane according to any one of claims 1-14, characterized in that, The ultrafiltration membrane is used for terminal filtration in the preparation of ultrapure water.

Citation Information

Patent Citations

  • Ultrapure water manufacturing device

    CN115702120A

  • Polycrylonitrlle-based hollow-fiber filtration membrane

    CN1234748A

  • Polysulfone hollow fiber membrane

    JP1990026627A

  • Polysulfone hollow fiber separation membrane

    JP1990164428A