Polarizing film, its preparation method, and display device

By using a multi-layer film structure and controlling the light transmittance ratio, the problem of dark-state light leakage caused by the unsatisfactory polarization effect of the polarizer film was solved, thus improving the display effect and overall performance of the display panel.

CN117492123BActive Publication Date: 2026-11-17TCL CHINA STAR OPTOELECTRONICS TECHNOLOGY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310547512.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-15
Publication Date
2026-11-17
Estimated Expiration
2043-05-15

AI Technical Summary

Technical Problem

The polarizer film layer prepared in the existing technology has an unsatisfactory polarization effect on light, which leads to light leakage in the display panel in the dark, reducing the display effect and overall performance.

Method used

A multilayer film structure is adopted, including a first protective layer, a polarizing layer and a second protective layer. By controlling the transmittance ratio of the polarizing layer to different wavelengths of light to be 0.1 < Ts(450)/Ts(550) < 0.8, combined with the processing technology of polyvinyl alcohol film and iodine molecular dye, effective polarization of light is achieved.

Benefits of technology

It effectively improves the polarization effect of the polarizer, avoids light leakage in dark states, and enhances the contrast and display effect of the display panel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117492123B_ABST
    Figure CN117492123B_ABST
Patent Text Reader

Abstract

This invention provides a polarizer, a method for fabricating the polarizer, and a display device. The polarizer includes a first protective layer, a polarizing layer, and a second protective layer. The polarizing layer is disposed on the first protective layer, and the second protective layer is disposed on the polarizing layer. The ratio of the transmittance of the polarizer for light with a wavelength of 450 nm to the transmittance for light with a wavelength of 550 nm is greater than 0.1 and less than 0.8. In this embodiment, by controlling the transmittance of the polarizing layer for light of different wavelengths, the absorption spectrum of the polarizer in the short wavelengths of visible light is controlled, effectively avoiding display problems such as dark-state light leakage in the display device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of display technology, and in particular to a polarizer, a method for preparing the polarizer, and a display device. Background Technology

[0002] With the development of display panel manufacturing technology, people have put forward higher requirements for the display effect and overall performance of display panels and display devices.

[0003] In the process of fabricating a display panel, a series of functional film layers are typically formed and combined to create a usable display panel. Each functional film layer performs a different function. For example, a polarizer layer on the display panel can polarize different types of light to obtain the desired light and ensure the display effect. However, in existing technologies, the polarization effect of the polarizer layer is not ideal. When light passes through the polarizer layer and exits from the display panel surface, users may observe blue light leakage in dark conditions, reducing the display effect and overall performance of the display panel and hindering further improvements in the overall performance of the display panel and device.

[0004] In summary, in the existing technology, the polarizer film layer used to form the display panel does not have an ideal effect on the polarization of light. As a result, the panel is prone to light leakage when displaying in the dark, which reduces the display effect of the display panel. Summary of the Invention

[0005] This invention provides a polarizer, a method for preparing a polarizer, and a display device, which effectively improves the problem in the prior art where the polarizer's polarization effect on light is not ideal and dark-state light leakage is prone to occur when preparing the polarizer film layer to form a display panel.

[0006] To solve the above-mentioned technical problems, embodiments of the present invention provide a polarizer, comprising:

[0007] First protective layer;

[0008] A polarizing layer is disposed on the first protective layer; and,

[0009] A second protective layer is disposed on the polarization layer;

[0010] The ratio of the transmittance of the polarizer for light with a wavelength of 450nm to the transmittance for light with a wavelength of 550nm is greater than 0.1 and less than 0.8.

[0011] According to one embodiment of the present invention, the polarizing layer comprises a polyvinyl alcohol film and iodine molecules dispersed in the polyvinyl alcohol film, as well as a direct yellow or orange dye.

[0012] According to one embodiment of the present invention, the unidirectional elongation of the polarization layer is set to 300%-650%.

[0013] According to one embodiment of the present invention, the materials of the first protective layer and the second protective layer are any one of cellulose triacetate, amorphous cyclic olefin polymer, polymethyl methacrylate and polyethylene terephthalate.

[0014] According to one embodiment of the present invention, the polarizer further includes:

[0015] An adhesive layer disposed on the side of the first protective layer away from the polarization layer;

[0016] A surface treatment layer disposed on the side of the second protective layer away from the polarization layer.

[0017] According to a second aspect of the present invention, a method for preparing a polarizer is also provided, comprising the following steps:

[0018] A polyvinyl alcohol-based resin film is provided, and the polyvinyl alcohol-based resin film is subjected to a sizing treatment.

[0019] The polyvinyl alcohol-based resin film material after Pengrun treatment is dyed and then cleaned;

[0020] The cleaned membrane material is then stretched in a solution.

[0021] The film obtained after stretching is dried, and a protective layer is applied to at least one side of the dried film to obtain a polarizer.

[0022] According to an embodiment of the present invention, the step of the Pengrun treatment includes: immersing the polyvinyl alcohol resin film in water to allow the polyvinyl alcohol resin film to absorb water;

[0023] The dyeing process includes: placing the polyvinyl alcohol resin film in an aqueous solution containing iodine and a direct yellow or orange dye for dyeing.

[0024] According to one embodiment of the present invention, the aqueous solution containing iodine and the direct yellow or orange dye also include potassium iodide.

[0025] According to an embodiment of the present invention, the stretching step further includes:

[0026] The membrane is stretched in an aqueous solution containing boric acid, and the membrane is uniaxially stretched by 300% to 650% in the solution.

[0027] The uniaxially stretched membrane material is immersed in an aqueous solution for color correction.

[0028] According to a second aspect of the present invention, a display device is also provided, including a display panel and polarizers disposed on both sides of the display panel, the polarizers comprising:

[0029] An adhesive layer is bonded to one side of the display panel;

[0030] A first protective layer is disposed on the adhesive layer;

[0031] A polarizing layer is disposed on the first protective layer;

[0032] A second protective layer is disposed on the polarization layer;

[0033] The ratio of the transmittance of the polarizer for light with a wavelength of 450 nm to the transmittance for light with a wavelength of 550 nm is set to be greater than 0.1 and less than 0.8.

[0034] The beneficial effects of this invention are as follows: Compared with the prior art, this application provides a polarizer, a method for preparing the polarizer, and a display device. The polarizer includes a first protective layer, a polarizing layer, and a second protective layer. The polarizing layer is disposed on the first protective layer, and the second protective layer is disposed on the polarizing layer. The ratio of the transmittance of the polarizer for light with a wavelength of 450 nm to the transmittance for light with a wavelength of 550 nm is set to be greater than 0.1 and less than 0.8. In this application, by controlling the transmittance of the polarizing layer for light of different wavelengths, the absorption spectrum of the polarizer in the short wavelengths of visible light is controlled, effectively avoiding display problems such as dark-state light leakage in the display device. Attached Figure Description

[0035] To more clearly illustrate the technical solutions in the embodiments or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0036] Figure 1 This is a schematic diagram of the film structure of the polarizer provided in the embodiments of this application;

[0037] Figure 2 The spectrum diagrams of the polarizer under backlight and dark conditions are shown.

[0038] Figure 3 This is a schematic diagram of a partial film layer structure of a display device provided in an embodiment of this application. Detailed Implementation

[0039] The following description, in conjunction with the accompanying drawings of the embodiments of the present invention, provides different implementation methods or examples to realize different structures of the present invention. To simplify the present invention, the components and arrangements of specific examples are described below. Furthermore, the various specific processes and materials provided in the present invention are examples that those skilled in the art will recognize for the application of other processes. All other embodiments obtained by those skilled in the art without inventive effort are within the scope of protection of the present invention.

[0040] In the description of this invention, it should be understood that the terms "center," "longitudinal," "lateral," "length," "width," "thickness," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," "outer," "clockwise," and "counterclockwise," etc., indicating orientations or positional relationships, are based on the orientations or positional relationships shown in the accompanying drawings and are only for the convenience of describing the invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of the invention. Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated.

[0041] This application provides a polarizer and a display device to effectively improve the problem that the polarizers prepared in the prior art have unsatisfactory polarization effect and are prone to light leakage.

[0042] like Figure 1 As shown, Figure 1 This is a schematic diagram of the film structure of the polarizer provided in this embodiment. The polarizer in this embodiment is formed by stacking multiple film layers. Specifically, the polarizer includes a release film 101, an adhesive layer 102, a first protective layer 103, a polarizing layer 104, a second protective layer 105, a surface treatment layer 106, and a protective film 107.

[0043] Specifically, when setting the above-mentioned film layers, the release film 101 is disposed at the bottom of the polarizer. When the polarizer needs to be bonded or assembled with the corresponding display panel, the release film 101 can be peeled off and then adhered to the other film layers. In this embodiment, the release film 101 has high strength, is not easily deformed, and has a high degree of surface flatness, thus providing better protection for the other film layers.

[0044] Optionally, in this embodiment, the material of the release film 101 can be polyethylene terephthalate or an organosilicon layer. Meanwhile, the film thickness of the release film 101 can be set between 10µm and 100µm, such as 50µm, to ensure the performance of the release film 101.

[0045] Furthermore, the adhesive layer 102 is disposed on the release film 101. In this embodiment, the adhesive layer 102 is mainly used for bonding with other film layers. Therefore, when setting it, ensuring the adhesive performance of the adhesive layer 102 can effectively prevent the problem of weak bonding.

[0046] In the following embodiments, the adhesive layer 102 is described using a pressure-sensitive adhesive material as an example. When this pressure-sensitive adhesive layer is applied, the adhesive exhibits high bonding performance and transparency. Furthermore, the adhesive residue is minimal during the coating process, thus ensuring good adhesion to other film layers after the adhesive layer 102 is applied, while also maintaining the smoothness of the bonded surface.

[0047] Specifically, when setting the adhesive layer 102, the film thickness of the adhesive layer 102 can be set to 10um-50um. Optionally, the film thickness of the adhesive layer 102 can be set to 20um, 30um or 40um, or set according to the product specifications.

[0048] Furthermore, in this embodiment, the first protective layer 103 is disposed on the adhesive layer 102, thereby further improving the overall performance of the polarizer. Specifically, the first protective layer 103 has excellent support properties, and at the same time, it has high transparency, acid and alkali resistance, ultraviolet resistance, and optical uniformity.

[0049] In this embodiment, the first protective layer 103 can be a resin film. For example, the material of the first protective layer 103 is a triacetate cellulose (TAC) layer. Optionally, the material of the first protective layer 103 can also be any one of triacetate cellulose, polymethyl methacrylate, and polyethylene terephthalate, which can be selected according to product requirements.

[0050] Specifically, when setting the first protective layer 103, the film thickness of the first protective layer 103 can be set to 10um-90um. Optionally, the thickness of the first protective layer 103 can be set to one of 25um, 40um, 60um, or 80um, or adjusted according to the usage requirements to ensure the overall performance of the polarizer.

[0051] Furthermore, a polarization layer 104 is disposed on the first protective layer 103. In this embodiment, the polarization layer 104 has a high unidirectional elongation. By disposing the polarization layer 104 on the first protective layer 103, the polarization layer 104 is fixed and ensured that the polarization layer 104 does not shrink back, thereby ensuring the overall performance of the film.

[0052] In this embodiment, the polarizing layer 104 can be made of a polyvinyl alcohol (PVA) film material that has undergone dyeing and extension alignment treatment. Specifically, a biaxially absorbing molecular material is also disposed within the polarizing layer 104. This biaxially absorbing molecular material is uniformly distributed within the polarizing layer 104. This material exhibits high biaxial absorption of light; when light passes through the polarizing layer 104, it absorbs different types of light and achieves a specific polarization effect.

[0053] In this embodiment, the dihedral absorbing molecular material can be selected from either iodine molecules or anthocyanin molecules. The following example uses iodine molecules. Iodine molecules have a high affinity for the polarization layer 104. During stretching, the iodine ions exhibit high orientation, replacing the -OH groups in the polarization layer and forming long iodine chains. Furthermore, during stretching, the randomly arranged coiled molecular chains within the polarization layer are roughly straightened and aligned parallel to the stretching direction.

[0054] Similarly, during the stretching process together with the polarizing layer, the aforementioned iodine molecular material will arrange itself in an orderly manner on the polarizing layer 104, thereby forming a film with uniform bidirectional absorption properties. When natural light passes through, the light component with the polarization direction aligned with the stretching direction will be strongly absorbed, while the light with the polarization direction perpendicular to the stretching direction will pass through the polarizing layer. This achieves the polarization of light and obtains the desired polarization effect.

[0055] Furthermore, in this embodiment of the application, within the visible light wavelength range, the ratio of the transmittance of the polarizer for light with a wavelength of 450nm to the transmittance for light with a wavelength of 550nm is set to be greater than 0.1 and less than 0.8.

[0056] like Figure 2 As shown, Figure 2The graphs show the spectrum of an existing polarizer under backlight and dark conditions. Graph a shows the spectrum under backlight conditions, and graph b shows the spectrum under dark conditions. The curves in both graphs show that the spectrum is not uniform within the visible light range of 380nm–780nm, which causes light leakage in the dark, especially in the 430nm–490nm visible light wavelength range, resulting in decreased contrast and affecting display performance.

[0057] In this embodiment, the polarization layer 104 is improved so that the ratio of the transmittance of the polarizer based on the polarization layer 104 for light with a wavelength of 450 nm to that for light with a wavelength of 550 nm is set to be greater than 0.1 and less than 0.8, i.e., 0.1 < Ts(450) / (550) < 0.8. Here, Ts(450) is the transmittance of the polarizer at a wavelength of 450 nm, and Ts(550) is the transmittance of the polarizer at a wavelength of 550 nm. In this way, the light within this range can be effectively controlled, thereby improving its polarization effect and controlling the absorption spectrum of the polarizer at short wavelengths of visible light, reducing dark-state light leakage, and effectively improving the contrast of the display panel.

[0058] Specifically, when setting it, Ts(450) and Ts(550) can be adjusted according to the above specific relationship. For example, when the polarizer sets Ts(450) for light with a wavelength of 450nm to 39%, the corresponding polarizer sets Ts(550) for light with a wavelength of 550nm to 54.17%. At this time, Ts(450) / Ts(550) = 0.72.

[0059] Furthermore, in this embodiment of the application, in order to ensure the stretching effect of the iodine molecules and the corresponding film layer, the unidirectional elongation of the polarization layer 104 is set to 300%-650%. Optionally, the unidirectional elongation of the polarization layer 104 is set to 400%, 550%, or 620%, thereby ensuring that after stretching, the polarization layer and the corresponding iodine molecules can be effectively stretched and have a high effect on light.

[0060] Specifically, to ensure the effectiveness of the polarizing layer 104 and achieve a thinner film, in this embodiment, the thickness of the polarizing layer 104 can be set to 10µm-150µm. Optionally, the polarizing layer 104 has a high stretchability; after stretching, its corresponding film thickness can be set to 10µm-30µm, thereby achieving a thinner film and improving its polarization effect. Alternatively, the setting can be adjusted according to the needs of different products to ensure the polarizing effect of the polarizer on light.

[0061] Furthermore, in this embodiment of the application, the second protective layer 105 is disposed on the polarization layer 104. When the second protective layer 105 is disposed, it can be disposed in accordance with the first protective layer 103. By disposing the first protective layer 103 and the second protective layer 105 on both sides of the polarization layer 104 film, the polarization layer 104 is effectively protected and its quality and performance are improved.

[0062] In this embodiment, the material of the second protective layer 105 includes any one of cellulose triacetate, amorphous cyclic olefin polymer, polymethyl methacrylate, and polyethylene terephthalate. Furthermore, the second protective layer 105 can be the same as that on the first protective layer 103, or it can be configured as two different film layers as needed.

[0063] Specifically, when setting the second protective layer 105, the thickness of the second protective layer 105 can be set to 10um-90um. Optionally, the thickness of the first protective layer 103 can be set to one of 25um, 40um, 60um, or 80um, or adjusted according to the usage requirements, so as to ensure the overall performance of the polarizer.

[0064] Furthermore, the surface treatment layer 106 of the polarizer is disposed on the second protective layer 105, and the surface treatment layer 106 is made of a material with a certain rigidity and hardness. When the surface of the surface treatment layer 106 is touched or slid, scratches will not appear on its surface due to its certain hardness. At the same time, because the surface treatment layer 106 has a certain hardness, it can also effectively support and protect other film layers, thereby achieving the purpose of improving the overall performance of the display panel.

[0065] In this embodiment, the hardness value of the surface treatment layer 106 can be greater than the hardness value of the second protective layer 105, thereby providing better protection for the underlying film layers. Specifically, the hardness of the surface treatment layer 106 can be set to 1H-5H, optionally, the hardness of the surface treatment layer 106 can be set to 2H, or other hardness values ​​can be set according to usage requirements.

[0066] Furthermore, in order to improve the film quality of the surface treatment layer 106, a hardening layer can be coated on the surface of the surface treatment layer 106 during the treatment process, thereby increasing its hardness.

[0067] Meanwhile, a protective layer 107 is also provided on the surface treatment layer 106. By providing the protective layer 107 on the surface treatment layer 106, external dust and other contaminants are effectively prevented from entering the interior of the film layer, and the film layer is protected.

[0068] Furthermore, this application embodiment also provides a method for preparing a polarizer. Specifically, the preparation method includes the following steps:

[0069] A polyvinyl alcohol-based resin film is provided, and the polyvinyl alcohol-based resin film is subjected to a sizing treatment.

[0070] The polyvinyl alcohol-based resin film material after Pengrun treatment is dyed and then cleaned;

[0071] The cleaned membrane material is then stretched in a solution.

[0072] The film obtained after stretching is dried, and a protective layer is applied to at least one side of the dried film to obtain a polarizer.

[0073] Specifically, in preparing the above-mentioned polarizer structure, the polarizing layer 104 can be prepared according to the following process. In this embodiment, the polarizing layer 104 is mainly prepared using a polyvinyl alcohol (PVA) resin film as the substrate. The substrate film is treated to obtain the polarizer structure described in this embodiment. In the following embodiments, the substrate is mainly polyvinyl alcohol (PVA) material.

[0074] First, the polyvinyl alcohol (PVA) film undergoes a humidification treatment. This humidification treatment removes excess residual impurities from the film layer, such as plasticizers and PVA film crystals, and allows the PVA film to absorb moisture during the process. During the humidification treatment, the PVA film is placed in a solution, such as immersing it in a pure aqueous solution for 30 to 90 minutes. Immersion removes residual impurities from the PVA film, thereby improving its performance and allowing the PVA film to absorb a certain amount of moisture.

[0075] After the sizing process, the polyvinyl alcohol film treated with the sizing process is immersed in a dyeing bath containing an aqueous solution of iodine molecules and a highly dichroic direct yellow or orange dye for dyeing. In preparing the dyeing bath solution, different materials are added to the aqueous solution to obtain solutions with different concentrations. Specifically, in this embodiment, iodine molecules, potassium iodide, and highly dichroic direct yellow or orange dye are dissolved in water to prepare the dyeing bath solution. The mass percentages of iodine molecules, potassium iodide, and highly dichroic direct yellow or orange dye in the dyeing bath solution are set as follows: (0.03%–0.1%):(0.5%–3%):(0.005%–0.04%). Optionally, the ratio of the above components is set to 0.1%:1%:0.02%, and the PVA film is immersed in the dyeing bath with this ratio for dyeing. Furthermore, the ratio of the materials in the dyeing bath can be adjusted according to the different polarizers, which will not be elaborated here.

[0076] After dyeing, the polyvinyl alcohol film is immersed in an aqueous solution containing boric acid for stretching. In this embodiment, the mass percentage of the aforementioned boric acid aqueous solution is set to 0.1% to 1%, optionally 0.5%. During the stretching treatment of the polyvinyl alcohol film, its unidirectional elongation in the solution is 300% to 650%, such as 600%. The stretched polyvinyl alcohol film is then immersed in an aqueous solution at approximately 25°C to 35°C for color correction.

[0077] After completing the above steps, the polyvinyl alcohol film is dried in an oven to obtain the polarizing layer 104 provided in this embodiment. The polarizing layer 104 has a strong absorption spectrum in the short wavelength range of visible light (430nm to 490nm). The ratio of the transmittance of the polarizer using the polarizing layer 104 to the transmittance of light at a wavelength of 550nm is set to be greater than 0.1 and less than 0.8. By limiting the transmittance for different wavelengths, the problem of light leakage and bluish tint in the dark state of the polarizer in the liquid crystal display is improved, and the display effect of the display panel is effectively enhanced.

[0078] After the polarization layer 104 is prepared, a protective layer is coated on at least one side of the surface of the polarization layer 104, such as the first protective layer and the second protective layer provided in the embodiments of this application, which are respectively coated on the upper and lower surfaces of the polarization layer 104, and the polarizer provided in the embodiments of this application is obtained.

[0079] In this embodiment, the polyvinyl alcohol film is dyed by adding an aqueous solution containing iodine molecules and a highly dichroic dye such as Direct Yellow or Orange to a dyeing bath. The absorption spectrum of the polarizer at short visible wavelengths (430nm–490nm) is controlled, and its transmittance at wavelengths of 450nm and 550nm satisfies the following relationship: 0.1 < Ts(450) / Ts(550) < 0.8, thus achieving high contrast even at short wavelengths. This reduces the blue leakage phenomenon in dark states of liquid crystal displays and achieves high contrast.

[0080] Furthermore, such as Figure 3 As shown, Figure 3 This is a schematic diagram of a partial film layer structure of a display device provided in an embodiment of this application. In this embodiment, a liquid crystal display device is used as an example for description.

[0081] Specifically, the display device includes a backlight module 300, a first polarizer 301, a first glass substrate 302, a TFT wiring layer 303, a liquid crystal layer 304, a color filter layer 305, a second glass substrate 306, and a second polarizer 307. The first glass substrate 302, TFT wiring layer 303, liquid crystal layer 304, color filter layer 305, and second glass substrate 306 together constitute a display panel. The first polarizer 301 and the second polarizer 307 are respectively disposed on the light-incident and light-exit sides of the display panel. The backlight module 300 is used to provide backlight.

[0082] Specifically, when setting the above-mentioned film layers, the first polarizer 301 is attached to the first glass substrate 302, the TFT wiring layer 303 is disposed on the first glass substrate 302, the color filter layer 305 is disposed on the second glass substrate 306, and the second polarizer 307 is disposed on the second glass substrate 306. In this embodiment, other film layers may also be disposed between the backlight module 300 and the first polarizer 301; here, only the main film layer structure is described as an example.

[0083] In this embodiment, when the first polarizer 301 and the second polarizer 307 are configured, the first polarizer 301 is the lower polarizer, and the second polarizer 307 is the upper polarizer layer. Both the first polarizer 301 and the second polarizer 307 are configured according to the film layer structure described in this embodiment. Specifically, the first polarizer 301 and the second polarizer 307 have the same structure, including an adhesive layer, a first protective layer, a polarizing layer, and a second protective layer. For example, the adhesive layer of the first polarizer 301 is bonded to the first glass substrate 302, and the adhesive layer of the second polarizer 307 is bonded to the second glass substrate 306. The transmittance of the first polarizer 301 and the second polarizer 307 for light with wavelengths between 450nm and 550nm is greater than 0.1 and less than 0.8. By controlling light of different wavelengths, the effect of the polarizer on light is effectively improved, and the problem of dark-state light leakage in the display panel is avoided.

[0084] In this embodiment, the polarizer and its corresponding display device can be any product or component that can be displayed or touched, such as a mobile phone, computer, electronic paper, monitor, laptop, or digital photo frame, and there are no specific limitations on its type.

[0085] In summary, the present invention has provided a detailed description of a polarizer, a method for preparing the polarizer, and a display device. Specific examples have been used to illustrate the principles and implementation methods of the present invention. The descriptions of the above embodiments are only for the purpose of helping to understand the technical solutions and core ideas of the present invention. Although the present invention has been disclosed above with preferred embodiments, the above preferred embodiments are not intended to limit the present invention. Those skilled in the art can make various modifications and refinements without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention is based on the scope defined by the claims.

Claims

1. A polarizer, characterized in that, include: First protective layer; A polarizing layer is disposed on the first protective layer; as well as, A second protective layer is disposed on the polarization layer; The polarizer has a transmittance ratio of 450nm light to 550nm light of greater than 0.1 and less than 0.8; the polarizing layer includes a polyvinyl alcohol film and iodine molecules dispersed in the polyvinyl alcohol film, as well as direct yellow or orange dye.

2. The polarizer according to claim 1, characterized in that, The unidirectional elongation of the polarization layer is set to 300%-650%.

3. The polarizer according to claim 1, characterized in that, The materials of the first protective layer and the second protective layer are any one of cellulose triacetate, amorphous cyclic olefin polymer, polymethyl methacrylate, and polyethylene terephthalate.

4. The polarizer according to claim 1, characterized in that, The polarizer also includes: An adhesive layer disposed on the side of the first protective layer away from the polarization layer; A surface treatment layer disposed on the side of the second protective layer away from the polarization layer.

5. A method for preparing a polarizer, characterized in that, Includes the following steps: A polyvinyl alcohol-based resin film is provided, and the polyvinyl alcohol-based resin film is subjected to a swelling treatment; The polyvinyl alcohol-based resin film material after swelling treatment is dyed and then cleaned. The cleaned membrane material is then stretched in a solution. as well as The film obtained after stretching is dried, and a protective layer is provided on at least one side of the dried film to obtain a polarizer. The ratio of the transmittance of the polarizer for light with a wavelength of 450 nm to the transmittance for light with a wavelength of 550 nm is greater than 0.1 and less than 0.

8. The dyeing process includes: placing the polyvinyl alcohol resin film in an aqueous solution containing iodine and a direct yellow or orange dye for dyeing.

6. The method for preparing a polarizer according to claim 5, characterized in that, The swelling treatment step includes: immersing the polyvinyl alcohol resin film in water to allow the polyvinyl alcohol resin film to absorb water.

7. The method for preparing a polarizer according to claim 5, characterized in that, The aqueous solution containing iodine and the direct yellow or orange dye also include potassium iodide.

8. The method for preparing a polarizer according to claim 5, characterized in that, The stretching step also includes: The membrane material is stretched in an aqueous solution containing boric acid, and the membrane material is uniaxially stretched by 300% to 650% in the solution. The uniaxially stretched membrane material is immersed in an aqueous solution for color correction.

9. A display device, comprising a display panel and polarizers disposed on both sides of the display panel, characterized in that, The polarizer includes: An adhesive layer is bonded to one side of the display panel; A first protective layer is disposed on the adhesive layer; A polarizing layer is disposed on the first protective layer; the polarizing layer includes a polyvinyl alcohol film and iodine molecules dispersed in the polyvinyl alcohol film, as well as direct yellow or orange dye; A second protective layer is disposed on the polarization layer; The ratio of the transmittance of the polarizer for light with a wavelength of 450 nm to the transmittance for light with a wavelength of 550 nm is set to be greater than 0.1 and less than 0.8.

Citation Information

Patent Citations

  • Adjustable polaroid and preparation method and application thereof

    CN115793127A

  • Polarizing plate and liquid crystal display device using the same

    JP2002258043A