Ceramic panel and heating device of heating device
By controlling the thermal expansion coefficient and water absorption rate of the ceramic panel, and combining the reinforcing layer and temperature measuring components, the problems of high cost of microcrystalline panels for induction cookers and uneven heating of slab tables have been solved, achieving low-cost, integrated high-power heating and high-precision temperature measurement.
Patent Information
- Application Number
- CN202210893977.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-27
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2042-07-27
AI Technical Summary
Existing microcrystalline panels for induction cookers are expensive, and existing slab tables suffer from uneven heating, poor aesthetics, and difficulty in cleaning, failing to meet the demand for integrated high-power heating.
Using ceramic panels with excellent resistance to thermal shock and mechanical impact, and by controlling the coefficient of thermal expansion and water absorption rate to reduce the Li2O content, combined with a reinforcing layer and temperature measuring components, uniform heat conduction and accurate temperature measurement are achieved, replacing microcrystalline panels and heat-insensitive rock panels.
It reduces raw material costs, improves the heat resistance and temperature measurement accuracy of the heating device, realizes integrated high-power heating, and enhances service life and overall performance.
Smart Images

Figure BDA0003768659060000081 
Figure BDA0003768659060000091
Abstract
Description
Technical Field
[0001] This invention belongs to the field of household appliances, and more specifically, relates to a ceramic panel for a heating device and a heating device. Background Technology
[0002] In recent years, increased demand and supply chain difficulties have led to a surge in lithium ore prices, with raw material costs rising exponentially, resulting in a sharp increase in the costs of downstream products. Aside from industries related to new energy, in the home appliance industry, microcrystalline panels used in induction cookers typically contain 3-4.5% Li₂O, which translates to 40-70% of the raw material in lithium ash. Faced with rising raw material prices, many microcrystalline panel manufacturers have had to raise prices multiple times, significantly increasing the cost of induction cookers and impacting the entire industry. Leaving aside supply chain difficulties, reducing the induction cooker industry's demand for lithium ore and replacing existing microcrystalline panels with other low-lithium or lithium-free panels is a viable option. In addition, in existing home settings, there are integrated slab stone tables with direct heating. These tables generally fall into two categories: one is a low-power heating type, with a low heating power and the slab temperature typically not exceeding 100℃, mainly used for keeping food or drinks warm; the other has a high heating power and can be used for direct cooking, but due to the heat resistance of the slab, it can only be used with a dedicated pot. The pot and slab do not directly contact each other to prevent the heat from the pot from being directly transferred to the slab, which could cause cracking. Besides these, there are also non-integrated slab stone tables in home settings. These products have grooves cut into the heating area of the slab, replacing the grooves with a microcrystalline panel to achieve heating on the tabletop. These products can be understood as an embedded induction cooker. The entire tabletop is not integrated, is less aesthetically pleasing, and has gaps, raising concerns about future cleaning. In summary, both integrated and non-integrated slab stone tables have certain shortcomings. Improving these shortcomings and perfecting new home settings is a new direction for companies to expand their market. Summary of the Invention
[0003] This invention aims to at least partially solve one of the technical problems in the related art. To this end, one object of this invention is to provide a ceramic panel for a heating device and a heating device in general. This ceramic panel possesses both good resistance to thermal shock and mechanical impact, and can replace existing microcrystalline panels and heat-sensitive slabs, thus enriching the selection of heating device panels and enabling integrated high-power heated slab tables.
[0004] This invention is primarily based on the following problems and findings:
[0005] Generally, the performance requirements for panels used in heating devices mainly focus on two aspects: resistance to thermal shock and resistance to mechanical impact. Similarly, the use of slab tables in home settings is primarily limited by these two performance requirements. Therefore, the demand is consistent: a panel capable of withstanding thermal shock at 550℃ and possessing mechanical impact resistance is required. The inventors discovered that the composition, crystal phase, porosity, elastic modulus, and microstructure of ceramics collectively influence the coefficient of thermal expansion and water absorption rate of ceramic materials. The magnitude of the coefficient of thermal expansion determines the volume change of the material due to temperature changes; the smaller the coefficient of thermal expansion, the smaller the volume change, and consequently, the smaller the temperature stress. After high-temperature sintering, ceramics have many small pores in their internal structure. These pores give ceramics a certain degree of water absorption, specifically reflected by the water absorption rate. The higher the water absorption rate, the more porous the ceramic, with higher porosity and lower elastic modulus. In fact, there is a certain relationship between the coefficient of thermal expansion and water absorption rate of ceramic panels and the resistance of ceramics to thermal shock. By controlling the coefficient of thermal expansion and water absorption rate of ceramic panels, heat-resistant ceramic panels that can withstand thermal shock and mechanical impact at 550℃ and above can be obtained.
[0006] In view of this, in one aspect of the present invention, a ceramic panel for a heating device is provided, particularly, the ceramic panel can be used in an electromagnetic heating device. According to an embodiment of the present invention, the coefficient of thermal expansion of the ceramic panel at 0–550°C is (0.5–3.5) × 10⁻⁶. -6 The ceramic panel has a water absorption rate of 2-30% and a Li₂O content not exceeding 3.5 wt%. Currently, to reduce the raw material cost of heating device panels or to obtain low-lithium or lithium-free panels, the Li content (calculated as Li₂O) in the panel is reduced, leading to an increase in the panel's coefficient of thermal expansion. A higher coefficient of thermal expansion results in greater thermal stress due to temperature changes. If this thermal stress cannot be effectively released, it will severely affect the panel's resistance to thermal shock. The inventors discovered that by adjusting the coefficient of thermal expansion and water absorption rate of the ceramic panel according to the aforementioned relationship, it is more conducive to the release of thermal stress during thermal shock and can improve the uniformity of thermal conductivity, reducing cracking caused by localized overheating. Furthermore, it can improve the accuracy of temperature measurement of the ceramic panel; on the other hand, by controlling the absorption rate of the ceramic panel to no more than 30%, it can also avoid the ceramic panel's structure being too loose, resulting in low overall strength. Thus, the ceramic panel can have good resistance to thermal shock and mechanical shock while having a low Li2O content, and can improve the uniformity of thermal conduction and the accuracy of temperature measurement. It can withstand thermal shock of 550℃ and above, which can not only reduce raw material costs, but also replace existing microcrystalline panels and heat-sensitive slabs, enrich the selection of heating device panels, and realize integrated high-power heating slab tables.
[0007] In addition, the ceramic panel of the heating device according to the above embodiments of the present invention may also have the following additional technical features:
[0008] In some embodiments of the present invention, one of the following conditions is met: the coefficient of thermal expansion of the ceramic panel at 0–550°C is (0.5–1) × 10⁻⁶. -6 / ℃, water absorption rate 2~30%; the coefficient of thermal expansion of the ceramic panel at 0~550℃ is (1~2)×10 -6 The water absorption rate is 5-30% at 0-550℃; the coefficient of thermal expansion of the ceramic panel at 0-550℃ is (2-3.5)×10⁻⁶. -6 / ℃, water absorption rate is 10-30%.
[0009] In some embodiments of the present invention, the coefficient of thermal expansion of the ceramic panel at 0–550°C is (0.5–1) × 10⁻⁶. -6 At ℃, the Li2O content in the ceramic panel is 3-3.5 wt%; the coefficient of thermal expansion of the ceramic panel at 0-550℃ is (1-2)×10⁻⁶. -6 At ℃, the Li2O content in the ceramic panel is 2.5–3 wt%; the coefficient of thermal expansion of the ceramic panel at 0–550℃ is (2–3.5) × 10⁻⁶. -6 / ℃, the Li2O content in the ceramic panel is no more than 2wt%.
[0010] In some embodiments of the present invention, the ceramic panel comprises Al2O3, SiO2, and Li2O, wherein the content of Al2O3 is 20-30 wt%, the content of SiO2 is 60-75 wt%, and the content of Li2O is 0.01-3.5 wt%.
[0011] In some embodiments of the present invention, the non-heated surface of the ceramic panel is provided with a reinforcing layer at least at its edge portion.
[0012] In some embodiments of the present invention, the reinforcing layer is disposed around the heating region.
[0013] In some embodiments of the present invention, the reinforcing layer is an inorganic material layer comprising glass fibers.
[0014] In some embodiments of the present invention, the reinforcing layer is a mesh structure layer.
[0015] In some embodiments of the present invention, a thinning zone and a temperature measuring component are also included, wherein the temperature measuring component is disposed in the thinning zone.
[0016] In another aspect, the present invention provides a heating device. According to an embodiment of the invention, the heating device includes the ceramic panel described above. This heating device possesses all the features and effects of the ceramic panel described above, which will not be repeated here. Further, in some embodiments of the invention, the heating device includes an electromagnetic heating element disposed below the ceramic panel. In summary, this heating device not only has low raw material costs but also a longer service life, achieving both heating function and integrated effect, resulting in superior overall performance.
[0017] Additional aspects and advantages of the invention will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of the invention. Detailed Implementation
[0018] The embodiments of the present invention are described in detail below. These embodiments are exemplary and intended to explain the present invention, and should not be construed as limiting the present invention.
[0019] In one aspect of the invention, a ceramic panel for a heating device is provided. According to an embodiment of the invention, the coefficient of thermal expansion of the ceramic panel at 0–550°C is (0.5–3.5) × 10⁻⁶. -6 The temperature is / ℃, the water absorption rate is 2-30%, and the Li2O content in the ceramic panel is no higher than 3.5wt%. Currently, in order to reduce the raw material cost of the heating device panel, or to obtain a low-lithium or lithium-free panel, the Li2O content in the panel is reduced, resulting in an increase in the thermal expansion coefficient of the panel. The higher the thermal expansion coefficient, the greater the thermal stress generated by temperature. If the generated thermal stress cannot be effectively released, it will seriously affect the panel's resistance to thermal shock. The inventors discovered that by adjusting the thermal expansion coefficient and water absorption rate of the ceramic panel in the above-mentioned correspondence, on the one hand, it is more conducive to the release of thermal stress during thermal shock, and on the other hand, it can improve the uniformity of thermal conduction of the ceramic panel, reduce the cracking phenomenon caused by local overheating of the ceramic panel, and further... This can improve the accuracy of temperature measurement of the ceramic panel; on the other hand, by controlling the absorption rate of the ceramic panel to no more than 30%, it can also avoid the ceramic panel's structure being too loose, resulting in low overall strength. Thus, the ceramic panel can have good resistance to thermal shock and mechanical shock while having a low Li2O content, and can improve the uniformity of thermal conduction and the accuracy of temperature measurement. It can withstand thermal shock of 550℃ and above, which can not only reduce raw material costs, but also replace existing microcrystalline panels and heat-sensitive slabs, enrich the selection of heating device panels, and realize an integrated high-power heating slab table.
[0020] The ceramic panel of the heating device according to the above embodiments of the present invention will be described in detail below.
[0021] The inventors discovered that by harmonizing the coefficient of thermal expansion and water absorption rate of the heating element panel, it is possible to produce a panel that can withstand thermal shock at 550°C. For example, taking the glass panel of an induction cooker as an example, the coefficient of thermal expansion of the microcrystalline panel at 550°C does not exceed 0.5 × 10⁻⁶. -6 At a temperature of 0℃ and a water absorption rate of 0, it can meet the performance requirements for thermal shock at 550℃; when the microcrystalline panel is changed to a high borosilicate panel, the coefficient of thermal expansion at 550℃ is not less than 3×10⁻⁶. -6 When the water absorption rate is 0 at ℃, it cannot meet the performance requirements for thermal shock at 550℃; when the microcrystalline panel is replaced with a ceramic panel, the coefficient of thermal expansion at 550℃ is 3.05×10. -6 The results are quite different when the water absorption rate is 19% at a given temperature, allowing it to withstand thermal shock at 550℃. This is because in microcrystalline panels, the coefficient of thermal expansion is small, resulting in low thermal stress. Even with zero water absorption, the panel structure is dense, and the elastic modulus is large, preventing the release of thermal stress. However, the thermal stress itself is very small and cannot exceed the material's thermal impact resistance, thus allowing it to withstand thermal shock at 550℃. Conversely, in high borosilicate panels, the coefficient of thermal expansion is large, resulting in high thermal stress. Since the water absorption rate is also zero, the thermal stress cannot be released. Therefore, under thermal shock at 550℃, the thermal stress would exceed the material's limits, making it unable to withstand the 550℃ thermal shock. In other words, when the panel's thermal stress is very low, even if it cannot be released, as long as the material's thermal impact resistance is not exceeded, it can withstand thermal shock at 550℃. Conversely, when the panel's thermal stress is high, if the thermal stress can be released in time, it can also withstand thermal shock at 550℃. Among the many components of a ceramic panel, the coefficient of thermal expansion can be effectively controlled by adjusting the Li₂O content. For panels with a high Li₂O content, such as microcrystalline panels, the Li₂O content is typically greater than 3.5 wt%, resulting in a lower coefficient of thermal expansion (e.g., not exceeding 0.5 × 10⁻⁶). -6 / ℃), typically capable of withstanding thermal shock up to 550℃, this invention primarily targets materials with a coefficient of thermal expansion higher than 0.5×10 -6 The ceramic panel has been improved to meet the requirements of thermal shock resistance up to 550℃ and mechanical shock resistance, replacing the existing microcrystalline panel and heat-sensitive slab. This enriches the selection of heating device panels and realizes an integrated high-power heated slab table.
[0022] According to embodiments of the present invention, the inventors discovered that for ceramic panels, the coefficient of thermal expansion of the panel tends to increase as the Li2O content decreases. To achieve both good thermal shock resistance and mechanical shock resistance in ceramic panels while reducing the Li2O content, the inventors conducted systematic research and extensive, meticulous experimental verification. They found that the ability of a panel to release thermal stress under thermal shock varies depending on its structure. Therefore, the optimal porosity requirement for different coefficients of thermal expansion is not the same, and the coefficient of thermal expansion is also affected by the Li2O content. Furthermore, when applying ceramic panels to heating devices such as slab tables, induction cookers, and ceramic cooktops, the panel's mechanical shock resistance must also be considered. Therefore, based on different Li2O content standards, how to coordinate the relationship between the panel's coefficient of thermal expansion, water absorption rate, thermal shock resistance, and mechanical shock resistance is of great significance for determining whether ceramic panels can replace microcrystalline panels for heating device panels.
[0023] According to embodiments of the present invention, the inventors discovered, and verified through numerous experiments, that the coefficient of thermal expansion of the ceramic panel at 0–550°C is (0.5–1) × 10⁻⁶. -6 At ℃, the water absorption rate of the ceramic panel can be controlled between 2% and 30%, for example, 3%, 5%, 7%, 9%, 11%, 13%, 15%, 17%, 19%, 21%, 23%, 25%, 27%, or 29%, etc. At this temperature, the Li₂O content in the ceramic panel is typically controlled between 3% and 3.5 wt%. When the coefficient of thermal expansion of the ceramic panel at 0–550℃ is (1–2) × 10⁻⁶, the water absorption rate can be controlled between 2% and 30%, for example, 3%, 5%, 7%, 9%, 11%, 13%, 15%, 17%, 19%, 21%, 23%, 25%, 27%, or 29%, etc., the Li₂O content in the ceramic panel is typically controlled between 3% and 3.5 wt%. -6 At a temperature of 0-550℃, the water absorption rate of the ceramic panel can be controlled between 5% and 30%, for example, it can be 6%, 8%, 10%, 12%, 14%, 16%, 18%, 20%, 22%, 24%, 26%, or 28%, etc. At this temperature, the Li₂O content in the ceramic panel is typically controlled between 2.5% and 3 wt%. When the coefficient of thermal expansion of the ceramic panel at 0-550℃ is (2-3.5) × 10⁻⁶, the water absorption rate can be controlled between 5% and 30%, for example, 6%, 8%, 10%, 12%, 14%, 16%, 18%, 20%, 22%, 24%, 26%, or 28%, etc. -6At a temperature of ℃, the water absorption rate of the ceramic panel can be controlled between 10% and 30%, for example, 11%, 13%, 15%, 17%, 19%, 21%, 23%, 25%, 27%, or 29%, etc. At this temperature, the Li₂O content in the ceramic panel is typically controlled to be no more than 2wt%. By adopting the above three methods, the ceramic panel can achieve both good resistance to thermal shock and mechanical shock while reducing the Li₂O content. It can also improve the uniformity of thermal conductivity and the accuracy of temperature measurement, and withstand thermal shock at 550℃ and above. This not only reduces raw material costs but also allows for the replacement of existing microcrystalline panels and heat-sensitive slabs, enriching the selection of heating device panels and enabling integrated high-power heated slab tables. It should be noted that in order to better meet the requirements of mechanical shock resistance in the application scenarios, the water absorption rate of the ceramic panel should not be too high. The higher the water absorption rate, the more porous the structure of the ceramic panel and the lower its strength. Therefore, for the above three specific solutions, it is preferable to choose a relatively low water absorption rate range on the premise that the water absorption rate of the ceramic panel does not exceed the upper limit (i.e., 30%) and the lower limit requirement. This can better balance the requirements of thermal shock resistance and mechanical shock resistance of the ceramic panel.
[0024] According to embodiments of the present invention, the specific composition of the ceramic panel is not particularly limited, and those skilled in the art can flexibly select it according to actual conditions. For example, the main components of the ceramic panel may include Al2O3, SiO2, and Li2O. In addition, small amounts of monovalent and divalent oxides such as Na2O and CaO, and other trace components may be added. The content of Al2O3 may be 20-30 wt% (e.g., 22 wt%, 24 wt%, 26 wt%, or 28%), and the content of SiO2 may be 60-75 wt% (e.g., 61 wt%, 63 wt%, or 65 wt%). The content of Al2O3, SiO2, and Li2O in the ceramic panel can range from 0.01% to 3.5% (e.g., 0.5% wt%, 1% wt%, 1.5% wt%, 2% wt%, 2.5% wt%, or 3%). Controlling the content of Al2O3, SiO2, and Li2O in the ceramic panel within these ranges not only facilitates processing and molding, resulting in ceramic panels with good chemical stability, thermal stability, and mechanical strength, but also further reduces the coefficient of thermal expansion of the ceramic panel by adjusting the Li2O content, thereby improving its chemical stability and resistance to thermal shock. Additionally, adding small amounts of oxides such as Na2O and CaO can provide a certain fluxing effect, lowering the sintering temperature in the preparation process. Furthermore, the water absorption rate of the ceramic panel can be adjusted by changing the sintering temperature and holding time. A higher sintering temperature and a longer holding time result in a relatively lower water absorption rate. This allows for flexible adjustment of the sintering conditions according to actual needs, thereby further improving the ceramic panel's resistance to thermal shock and mechanical impact, meeting the requirements of the heating device. According to a specific example of the present invention, for the ceramic panel with the above-mentioned specific composition, the sintering temperature can be controlled to be 1050–1300°C, for example, 1000°C, 1050°C, 1100°C, 1150°C, 1200°C, or 1250°C; the sintering time can be 80 min–3 h, for example, 1.5 h, 2 h, or 2.5 h. The inventors have found that by controlling the above sintering conditions, it is more advantageous to control the porosity of the ceramic panel with the above-mentioned raw material composition within the range of 2–30%, thus making it more advantageous to obtain a ceramic panel with both good resistance to thermal shock and mechanical impact.
[0025] According to embodiments of the present invention, the thickness of the ceramic panel is not particularly limited, and those skilled in the art can flexibly select it according to actual needs. For example, the thickness of the ceramic panel can be 4 to 8 mm, specifically 4.5 mm, 5 mm, 5.5 mm, 6 mm, 6.5 mm, 7 mm, or 7.5 mm, etc. If the ceramic panel is too thin, it is difficult to meet its strength requirements, while if the ceramic panel is too thick, it will reduce the temperature measurement accuracy and easily lead to uneven heat conduction and the risk of cracking. Setting the thickness of the ceramic panel within the aforementioned range can ensure that the water absorption rate of the ceramic panel is controlled at 2 to 30%, which can better take into account the requirements of the ceramic panel's resistance to thermal shock and mechanical impact.
[0026] According to embodiments of the present invention, a reinforcing layer may be provided at least at its edge portion on the non-heated surface of the ceramic panel. When the water absorption rate of the ceramic panel is high, its overall strength is reduced. In this invention, by providing a reinforcing layer at least at the edge portion of the non-heated surface of the ceramic panel, the strength can be improved without affecting the coefficient of thermal expansion of the heated area. It is understood that the reinforcing layer can be provided at the edge of the non-heated surface of the ceramic panel near the heated area and / or at the edge of the non-heated surface away from the heated area. Furthermore, the reinforcing layer can be provided on the entire non-heated surface of the ceramic panel.
[0027] According to an embodiment of the present invention, the reinforcing layer can be disposed around the heating area of the ceramic panel, thereby reducing the negative impact that heat from the heating area may have on the reinforcing layer and ensuring the structural and chemical stability of the reinforcing layer.
[0028] According to embodiments of the present invention, the material and structure of the reinforcing layer are not particularly limited. Those skilled in the art can flexibly choose according to actual conditions, as long as a good reinforcing effect can be achieved. For example, the reinforcing layer can be formed solely of inorganic materials or a composite of inorganic materials and reinforcing fibers. According to a specific example of the present invention, the reinforcing layer can be an inorganic material layer including reinforcing fibers, thereby achieving a good reinforcing effect without affecting the overall appearance of the ceramic panel. Preferably, the reinforcing layer can be integrally formed with the ceramic panel, thereby achieving good consistency between the reinforcing layer and the ceramic panel structure, while also improving strength. Furthermore, the reinforcing layer can be a mesh structure layer. By using a reinforcing layer with a mesh structure, the stress dispersion effect can be further achieved, which is more conducive to the release of thermal stress in the heated area and non-heated surface of the ceramic panel. This allows the ceramic panel to have better resistance to thermal shock and mechanical impact, enabling it to meet the usage requirements of the heating device.
[0029] According to embodiments of the present invention, the ceramic panel may further include a thinning zone and a temperature measuring component, wherein the temperature measuring component may be disposed in the thinning zone. The inventors have discovered that, due to the relatively thick ceramic panel and poor thermal conductivity, the accuracy of temperature measurement on its surface is not high. By setting a thinning zone to place the temperature measuring component for temperature measurement, the accuracy of temperature measurement can be significantly improved.
[0030] In another aspect, the present invention provides a heating device. According to an embodiment of the invention, the heating device includes a front ceramic panel. It should be noted that the features and effects described for the ceramic panel of the aforementioned heating device also apply to this heating device, and will not be repeated here. In some embodiments of the invention, the heating device may further include an electromagnetic heating element, which may be disposed below the ceramic panel, thereby enabling electromagnetic heating of the component to be heated. In general, this heating device not only has low raw material costs but also a longer service life, achieving both heating function and integrated effect, resulting in superior overall performance. It should be noted that the type of heating device is not particularly limited, and those skilled in the art can flexibly choose according to actual needs. For example, the heating device can be an induction cooker, an integrated high-power slab table with heating function, or a cooking set that further includes a matching component to be heated, etc.
[0031] The embodiments of the present invention are described in detail below. These embodiments are exemplary and are only used to explain the present invention, and should not be construed as limiting the invention. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in the art or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all commercially available conventional products.
[0032] Example 1
[0033] The ceramic panel 1 is provided, comprising: 26.58 wt% Al2O3, 68.28 wt% SiO2, 3.16 wt% Li2O, 0.3 wt% Na2O, 0.46 wt% K2O, 0.16 wt% CaO, 0.38 wt% MgO and other trace elements.
[0034] Example 2
[0035] Ceramic panel 2 is provided, comprising: 20.64 wt% Al2O3, 74.22 wt% SiO2, 2.98 wt% Li2O, 0.39 wt% Na2O, 0.35 wt% K2O, 0.24 wt% CaO, 0.16 wt% MgO, and other trace elements.
[0036] Example 3
[0037] The ceramic panel 3 is provided, comprising: 24.67 wt% Al2O3, 68.3 wt% SiO2, 2.54 wt% Li2O, 0.37 wt% Na2O, 0.85 wt% K2O, 0.42 wt% CaO, 0.31 wt% MgO, and other trace elements.
[0038] Example 4
[0039] The ceramic panel 4 is provided, comprising: 27.53 wt% Al2O3, 66.96 wt% SiO2, 1.47 wt% Li2O, 0.41 wt% Na2O, 0.76 wt% K2O, 0.62 wt% CaO, 0.41 wt% MgO, and other trace elements.
[0040] Comparative Example 1
[0041] The microcrystalline panel 1 comprises: 21.54 wt% Al2O3, 63.22 wt% SiO2, 4.05 wt% Li2O, and small amounts of other components such as CaO, MgO, K2O, Na2O, TiO2, etc.
[0042] Comparative Example 2
[0043] The microcrystalline panel 2 comprises: 21.21 wt% Al2O3, 63.53 wt% SiO2, 3.6 wt% Li2O, and small amounts of other components such as CaO, MgO, K2O, Na2O, and TiO2.
[0044] Comparative Example 3
[0045] We offer high borosilicate glass panels, specifically 3.3-series high borosilicate glass that is readily available on the market, comprising: 80.28 wt% SiO2, 12.66 wt% B2O3, and 3.5 wt% Na2O. , 2.7 wt% Al2O3 and other trace components.
[0046] Comparative Example 4
[0047] The ceramic panel 5 is provided, comprising: 28.06 wt% Al2O3, 65.30 wt% SiO2, 1.99 wt% Li2O, 0.29 wt% Na2O, 0.78 wt% K2O, 0.56 wt% CaO, 0.29 wt% MgO and other trace elements.
[0048] Comparative Example 5
[0049] The ceramic panel 6 is provided, comprising: 26.80 wt% Al2O3, 60.25 wt% SiO2, 1.91 wt% Li2O, 0.22 wt% Na2O, 0.73 wt% K2O, 0.27 wt% CaO, 0.18 wt% MgO and other trace elements.
[0050] In the above nine embodiments and comparative examples, for microcrystalline panels 1 and 2 and high borosilicate panels, the various raw materials constituting the glass were completely melted inside the furnace and then pressed into shape. Throughout the manufacturing process, the coefficient of thermal expansion was adjusted by controlling the Li content in the control panel, as shown in Table 1. Ceramic panels 1-6, on the other hand, involved controlling different compositions and sintering processes to create ceramic panels with inconsistent coefficients of thermal expansion, water absorption rates, and resistance to thermal shock at 550℃. Among the many components, adjusting the Li₂O content effectively controlled the coefficient of thermal expansion of the ceramic panel. The water absorption rate of the ceramic panel was mainly adjusted by changing the sintering temperature and holding time. Higher temperatures and longer holding times resulted in relatively lower water absorption rates. The Li content, sintering temperature and holding time, coefficient of thermal expansion, water absorption rate, and resistance to thermal shock for ceramic panels 1-6 are shown in Table 1.
[0051] Performance testing:
[0052] The absorption rate, coefficient of thermal expansion, and resistance to thermal shock of each panel in Examples 1-4 and Comparative Examples 1-5 were tested under the same conditions. The test results are shown in Table 1.
[0053] Table 1 shows the test results for each panel in Comparative Examples 1-5 and Examples 1-4.
[0054]
[0055]
[0056] Results and conclusions:
[0057] As shown in Table 1, reducing the Li₂O content generally leads to a higher coefficient of thermal expansion in the ceramic panel. However, when the coefficient of thermal expansion and water absorption rate of the ceramic panel meet a certain correlation, the requirement for resistance to thermal shock at 550℃ can still be met. For example, according to Comparative Examples 1 and 2, when the Li₂O content is greater than 3.5 wt%, the coefficient of thermal expansion of the panel is usually no higher than 0.5 × 10⁻⁶. -6 At a temperature of / ℃, the panel has no requirement for water absorption rate and can meet the thermal shock resistance of 550℃; however, according to Comparative Example 3 and Examples 1-4, when the Li2O content in the panel decreases, its coefficient of thermal expansion increases. When the coefficient of thermal expansion is (1-2)×10 -6When the temperature is between ℃, a water absorption rate of not less than 5% for the ceramic panel is sufficient to withstand thermal shock at 550℃; when the coefficient of thermal expansion is between (2~3.5)×10 -6 When the temperature is between ℃, further increasing the water absorption rate can also meet the thermal shock of 550℃; however, further combining with comparative examples 4 to 5, it can be seen that when the thermal expansion coefficient of the ceramic panel does not match the water absorption rate, it also cannot meet the thermal shock of 550℃.
[0058] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the present invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples.
[0059] Although embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of the present invention.
Claims
1. A ceramic panel for a heating device, characterized in that, The ceramic panel comprises: 26.58 wt% Al2O3, 68.28 wt% SiO2, 3.16 wt% Li2O, 0.3 wt% Na2O, 0.46 wt% K2O, 0.16 wt% CaO, 0.38 wt% MgO, and other trace elements. The ceramic panel was sintered at 1150℃ for 2 hours, and its coefficients of thermal expansion at 100℃, 200℃, 300℃, 400℃, 500℃, and 600℃ were 1.11×10⁻⁶. -6 / ℃, 0.37×10 -6 / ℃, 0.26×10 -6 / ℃, 0.38×10 -6 / ℃, 0.56×10 -6 / ℃, 0.75×10 -6 / ℃, water absorption rate is 5.1%.
2. A ceramic panel for a heating device, characterized in that, The ceramic panel comprises: 20.64 wt% Al2O3, 74.22 wt% SiO2, 2.98 wt% Li2O, 0.39 wt% Na2O, 0.35 wt% K2O, 0.24 wt% CaO, 0.16 wt% MgO, and other trace elements. The ceramic panel was sintered at 1150℃ for 90 minutes, and its coefficients of thermal expansion at 100℃, 200℃, 300℃, 400℃, 500℃, and 600℃ were 1.75×10⁻⁶. -6 / ℃, 0.88×10 -6 / ℃, 0.73×10 -6 / ℃, 0.83×10 -6 / ℃, 0.97×10 -6 / ℃, 1.14×10 -6 / ℃, water absorption rate is 8.1%.
3. A ceramic panel for a heating device, characterized in that, The ceramic panel comprises: 24.67 wt% Al2O3, 68.3 wt% SiO2, 2.54 wt% Li2O, 0.37 wt% Na2O, 0.85 wt% K2O, 0.42 wt% CaO, 0.31 wt% MgO, and other trace elements. The ceramic panel was sintered at 1200℃ for 90 minutes, and its coefficients of thermal expansion at 100℃, 200℃, 300℃, 400℃, 500℃, and 600℃ were 2.43 × 10⁻⁶. -6 / ℃, 1.73×10 -6 / ℃, 1.49×10 -6 / ℃, 1.5×10 -6 / ℃, 1.57×10 -6 / ℃, 1.73×10 -6 / ℃, water absorption rate is 6.9%.
4. A ceramic panel for a heating device, characterized in that, The ceramic panel comprises: 27.53 wt% Al2O3, 66.96 wt% SiO2, 1.47 wt% Li2O, 0.41 wt% Na2O, 0.76 wt% K2O, 0.62 wt% CaO, 0.41 wt% MgO, and other trace elements. The ceramic panel was sintered at 1100℃ for 60 minutes, and its coefficients of thermal expansion at 100℃, 200℃, 300℃, 400℃, 500℃, and 600℃ were 2.76 × 10⁻⁶. -6 / ℃, 2.43×10 -6 / ℃, 2.47×10 -6 / ℃, 2.62×10 -6 / ℃, 2.8×10 -6 / ℃, 3.25×10 -6 / ℃, water absorption rate is 19%.
5. The ceramic panel according to claim 1, characterized in that, The non-heated surface of the ceramic panel has a reinforcing layer at least at its edge.
6. The ceramic panel according to claim 5, characterized in that, The reinforcing layer is arranged around the heating area.
7. The ceramic panel according to claim 5, characterized in that, The reinforcing layer is an inorganic material layer including glass fiber.
8. The ceramic panel according to claim 5, characterized in that, The reinforcing layer is a mesh structure layer.
9. The ceramic panel according to claim 1 or 7, characterized in that, It also includes a thinning zone and a temperature measuring component, wherein the temperature measuring component is located in the thinning zone.
10. A heating device, characterized in that, The ceramic panel includes any one of claims 1 to 9.
11. The heating device according to claim 10, characterized in that, It includes an electromagnetic heating element, which is disposed below the ceramic panel.
Citation Information
Patent Citations
A ceramic composite gas stove panel
CN201606929U
Thermal shock resistant ceramics and its production
JP1998087365A
Ceramic heater
WO2001011919A1