A method for preparing a proton exchange membrane using a polyacrylate as a base membrane
By grafting sulfobetaine monomers onto the polyacrylate backbone, a proton exchange membrane with good conductivity and stability was prepared, solving the problem of insufficient performance of inorganic membranes and improving the performance of fuel cells.
Patent Information
- Application Number
- CN202311766816.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-21
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-12-21
AI Technical Summary
In existing proton exchange membrane fuel cells, inorganic membranes have poor mechanical and electrochemical properties, are prone to hydrolysis, and have poor membrane formation properties, which limits the performance and lifespan of fuel cells.
A proton exchange membrane material with good electrical conductivity, chemical stability, and thermal stability was prepared by grafting sulfobetaine functional monomers onto the polyacrylate backbone using solution polymerization.
The prepared proton exchange membrane has good conductivity, chemical stability and thermal stability, making it suitable for industrial production, and the synthesis process is simple.
Smart Images

Figure CN117525519B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of hydrogen fuel cell technology, specifically relating to a method for preparing a proton exchange membrane using polyacrylate as the matrix membrane. Background Technology
[0002] Climate change is a common challenge facing humanity. Widespread societal attention to climate issues has spurred the development of fuel cells. Proton exchange membrane fuel cells (PEMFCs), as one of the most promising fuel cells, have naturally attracted significant attention. The proton exchange membrane is the core component of a PEMFC, and its performance directly affects the fuel cell's performance and lifespan. Therefore, developing a high-performance, easy-to-manufacture, and low-cost proton exchange membrane material is of paramount importance.
[0003] There are many methods for preparing PEMFC membrane materials. Both inorganic compounds and organic polymers can be used as proton exchange membrane (PEM) matrix membranes, but inorganic membranes have poor mechanical properties, poor electrochemical properties, are easily hydrolyzed, and have poor film-forming properties. This has attracted more attention to organic membranes. Currently, polymers used in PEMFC membrane materials include: polyvinyl alcohol, bacterial cellulose, microcrystalline cellulose, polyetheretherketone, and polytetrafluoroethylene. Summary of the Invention
[0004] The purpose of this section is to outline some aspects of embodiments of the present invention and to briefly describe some preferred embodiments. Simplifications or omissions may be made in this section, as well as in the abstract and title of this application, to avoid obscuring the purpose of these documents; however, such simplifications or omissions should not be construed as limiting the scope of the invention.
[0005] The purpose of this invention is to provide a novel method for preparing a proton exchange membrane using polyacrylate as the matrix membrane. First, a sulfobetaine functional monomer is prepared, and then this functional monomer is grafted onto the polyacrylate backbone via solution polymerization to prepare a proton exchange membrane material with good electrical conductivity, good chemical stability, and good thermal stability. The reaction formulas are as follows: Formula 1 and Formula 2:
[0006]
[0007]
[0008] As one aspect of the present invention, the present invention provides a method for preparing a proton exchange membrane using polyacrylate as a matrix membrane, comprising,
[0009] (1) Preparation of sulfonate betaine: Dimethylaminoethyl acrylate was added to a solvent to obtain a dimethylaminoethyl acrylate solution; 1,3-propanesulfonyl lactone was added to a solvent to obtain a 1,3-propanesulfonyl lactone solution; under an inert atmosphere, the solution was heated and then slowly added to the dimethylaminoethyl acrylate solution to obtain the sulfonate betaine monomer.
[0010] (2) Add sulfonyl betaine monomer, methyl methacrylate, butyl acrylate and hydroxyethyl methacrylate to a solvent, heat under an inert atmosphere, add an initiator dropwise to carry out the reaction, and add the resulting liquid to a template to obtain a proton exchange membrane.
[0011] The mass ratio of methyl methacrylate to butyl acrylate is (1.5-2.5):3; the mass ratio of sulfonyl betaine monomer to methyl methacrylate is (0.6-1.9):1; and the mass ratio of methyl methacrylate to hydroxyethyl methacrylate is (3-5):1.
[0012] As a preferred embodiment of the method for preparing the proton exchange membrane with polyacrylate as the matrix membrane according to the present invention, the mass ratio of the sulfonate betaine monomer to methyl methacrylate is (6.13~9.53)∶5.2.
[0013] As a preferred embodiment of the method for preparing the proton exchange membrane with polyacrylate as the matrix membrane according to the present invention, the mass ratio of methyl methacrylate to butyl acrylate is 2:3.
[0014] As a preferred embodiment of the method for preparing the proton exchange membrane with polyacrylate as the matrix membrane according to the present invention, the mass ratio of methyl methacrylate to hydroxyethyl methacrylate is 4:1.
[0015] As a preferred embodiment of the method for preparing a proton exchange membrane with polyacrylate as the matrix membrane according to the present invention: in step (2), the solvent is a mixed solvent of N′N-dimethylformamide and water, wherein the mass ratio of N′N-dimethylformamide to water is 7:1.
[0016] As a preferred embodiment of the method for preparing a proton exchange membrane with polyacrylate as the matrix membrane according to the present invention: in step (2), the inert atmosphere includes a nitrogen atmosphere; the heating is to raise the temperature to 75°C.
[0017] As a preferred embodiment of the method for preparing a proton exchange membrane with polyacrylate as the matrix membrane according to the present invention: in step (2), the initiator includes azobisisobutyronitrile, the reaction temperature is 75°C, and the reaction time is 8h.
[0018] As a preferred embodiment of the method for preparing a proton exchange membrane with polyacrylate as the matrix membrane according to the present invention: in step (1), the molar ratio of dimethylaminoethyl acrylate to 1,3-propanesulfonyl lactone is 1:1.
[0019] As a preferred embodiment of the method for preparing the proton exchange membrane with polyacrylate as the matrix membrane according to the present invention, the heating temperature is 60°C.
[0020] As a preferred embodiment of the method for preparing the proton exchange membrane with polyacrylate as the matrix membrane according to the present invention, the solvents of the dimethylaminoethyl acrylate solution and the 1,3-propanesulfonyl lactone solution are both tetrahydrofuran.
[0021] The beneficial effects of this invention are as follows: This invention uses polyacrylate as the matrix membrane and grafts sulfobetaine onto the polyacrylate backbone via solution polymerization to prepare a sulfobetaine polyacrylate proton exchange membrane. The proton exchange membrane prepared by this invention exhibits good conductivity, chemical stability, and thermal stability. This invention employs mild reaction conditions, has a simple synthesis process, and uses readily available raw materials, making it suitable for industrial production and widespread application. Attached Figure Description
[0022] To more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort. Wherein:
[0023] Figure 1 Infrared spectra of sulfobetaine monomers, SBPA-0, and SBPA-40.
[0024] Figure 2 This is an NMR image of SBA.
[0025] Figure 3 The conductivity of SBPA-20, SBPA-30, and SBPA-40 varies with temperature.
[0026] Figure 4 It is TG and DTG of SBPA-0, SBPA-20, SBPA-30 and SBPA-40.
[0027] Figure 5 The percentage of residual mass and residual conductivity of SBPA-20, SBPA-30, and SBPA-40 membranes after immersion in 30% hydrogen peroxide solution for 300 hours.
[0028] Figure 6The mechanical properties of SBPA-20, SBPA-30, and SBPA-40 are described.
[0029] Figure 7 Arrhenius curves for SBPA-20, SBPA-30, and SBPA-40. Detailed Implementation
[0030] To make the above-mentioned objectives, features and advantages of the present invention more apparent and understandable, the specific embodiments of the present invention will be described in detail below with reference to specific examples.
[0031] Example 1:
[0032] (1) Preparation of sulfonyl betaine (SBA):
[0033] In a 250 mL three-necked flask, 14.32 g (0.1 mol) of dimethylaminoethyl acrylate and 50 g of tetrahydrofuran were added, and the mixture was heated to 60 °C under nitrogen protection. Then, 12.20 g (0.1 mol) of 1,3-propanesulfonyl lactone (C3H6O3S) was dissolved in 30 g of tetrahydrofuran and slowly added to the flask through a constant pressure drop funnel. The reaction was allowed to proceed for 4 h. Finally, the white solid crude product, sulfonyl betaine monomer labeled SBA, was extracted and filtered.
[0034] (2) Preparation of sulfonated betaine polyacrylate (SBPA):
[0035] In a 100 mL three-necked flask, 5.2 g of methyl methacrylate, 7.8 g of butyl acrylate, 1.3 g of hydroxyethyl methacrylate, different masses of sulfonated betaine (SBA), 35 g of N′N-dimethylformamide solvent, and 5 g of deionized water were added according to the amounts specified in Table 1. Under nitrogen protection, the temperature was raised to 75 °C, and an initiator (0.15 g of azobisisobutyronitrile added to 5 g of N′N-dimethylformamide solution as an initiator) was added dropwise over 1 hour. After the addition was complete, the reaction was continued at 75 °C for 8 hours. After the reaction was completed, the liquid was dropped into a polytetrafluoroethylene template to obtain SBPA polymer films with different SBA contents. The thickness of the SBPA polymer films was approximately 0.4 mm, and they were designated as SBPA-20, SBPA-30, and SBPA-40, respectively. The specific experimental formulations are shown in Table 1.
[0036] Table 1. Synthesis formulation of sulfonated betaine polyacrylate
[0037]
[0038] In Table 1, if the amount of sulfonate betaine monomer is further increased, it is found that the resulting polymer film is too rigid, and the polymer film is damaged during demolding, resulting in poor mechanical properties. Therefore, the plan to further increase the amount of sulfonate betaine monomer is abandoned.
[0039] The effect of the ratio of soft to hard monomers on the mechanical properties of polymer films:
[0040] The main chain structure of sulfonated betaine polyacrylate was optimized by changing the feed ratio of methyl methacrylate and butyl acrylate, as shown in Table 2. Experiments revealed that when the mass ratio of methyl methacrylate to butyl acrylate was 1:3, the resulting polymer had too high viscosity, making it difficult to demold from the PTFE plate and preventing the acquisition of a stable sulfonated betaine polyacrylate film. When the mass ratio of methyl methacrylate to butyl acrylate was 1:1, the resulting polymer was too rigid, breaking during demolding from the PTFE plate, also preventing the acquisition of a complete sulfonated betaine polyacrylate film. Therefore, optimization experiments showed that a mass ratio of methyl methacrylate to butyl acrylate of 2:3 yielded a sulfonated betaine polyacrylate film with good mechanical properties.
[0041] Table 2 Structural optimization of sulfonated betaine polyacrylate
[0042]
[0043] Effect of crosslinking agent dosage on the mechanical properties of polymer membranes:
[0044] 5.2 g of methyl methacrylate, 7.8 g of butyl acrylate, 1.3 g of hydroxyethyl methacrylate, 9.53 g of SBA, 35 g of N′N-dimethylformamide solvent, and 5 g of deionized water were added to a 100 mL three-necked flask. Under nitrogen protection, the temperature was raised to 75 °C, and a solution of 0.15 g of azobisisobutyronitrile in N′N-dimethylformamide was added dropwise over 1 hour. After the addition was complete, the reaction was continued at 75 °C for 8 hours. Subsequently, different amounts of the crosslinking agent pyromellitic anhydride (as shown in Table 3) were added, and the reaction was continued for 5 hours. After the reaction was completed, the liquid was dropped into a polytetrafluoroethylene (PTFE) template to obtain sulfonated betaine polyacrylate films with different degrees of crosslinking. Experiments showed that the addition of the crosslinking agent resulted in excessively rigid polymers, leading to breakage during demolding from the PTFE plate, making it impossible to obtain intact sulfonated betaine polyacrylate films. Therefore, optimization experiments show that sulfonate betaine polyacrylate membranes can achieve good mechanical properties without the addition of additional crosslinking agents.
[0045] Table 3 Optimization of crosslinking agent dosage
[0046] Sample number Crosslinking agent dosage (g) SBPA-40 O SBPA-40-5 0.42 SBPA-40-6 0.67
[0047] Figure 1 Infrared spectra of sulfobetaine monomers, SBPA-0, and SBPA-40.
[0048] exist Figure 1From this, we can see that SBA is 1202cm -1 With 1037cm -1 The vibration band at 1426 cm represents both asymmetric and symmetric stretching vibrations at S=O. -1 The stretching vibration characteristic spectrum at that location belongs to CN. + 1485cm -1 With 1647cm -1 The absorption peaks are for the stretching vibrations of -CH and C=C, respectively; the absorption peak of the C=O group appears at 1727 cm⁻¹. -1 The characteristic spectral band corresponding to the stretching vibration of -CH2- is at 2920 cm⁻¹. -1 and 3012cm -1 This indicates that the SBA monomer has been successfully synthesized. Furthermore, the infrared spectra of SBPA-0 and SBPA-40 show that the symmetric vibration peak of COC appears at 1168 cm⁻¹. -1 At this point, the bending vibration absorption peak of -CH2- appears at 1386 cm⁻¹. -1 and 1450cm -1 At this point, the tensile vibration peak of CH appears at 2954 cm⁻¹. -1 and 2873cm -1 At this point, the stretching vibration absorption peak of -OH appears at 3420 cm⁻¹. -1 The characteristic absorption peak at 1037 cm⁻¹ disappeared, indicating the successful synthesis of polyacrylate. Furthermore, the infrared spectrum of SBPA-40 showed a peak at 1037 cm⁻¹. -1 The presence of an S=O vibration peak indicates that SBA has been successfully grafted onto polyacrylate.
[0049] Figure 2 This is an NMR image of SBA.
[0050] The synthesized product SBA was subjected to 1 H NMR test, results as follows Figure 2 shown. δ=4.68 is the D2O solvent peak, δ=6.37 (m, 1H), δ=6.12 (m, 1H), δ=5.89 (m, 1H), δ=4.53 (s, 2H) , δ = 3.67 (s, 2H), δ = 3.44 (m, 2H), δ = 3.09 (d, 6H), δ = 2.88 (m, 2H), δ = 2.15 (m, 2H). 1 1H NMR testing further confirmed the successful synthesis of the SBA monomer.
[0051] Figure 3 The conductivity of SBPA-20, SBPA-30, and SBPA-40 varies with temperature.
[0052] Figure 3The graph shows the conductivity of SBPA-20, SBPA-30, and SBPA-40 as a function of temperature under 90% RH conditions. The conductivity of all membranes is positively correlated with temperature. SBPA-40 exhibits the highest conductivity, reaching 78 mS / cm at 80°C. Furthermore, the conductivity increases with increasing SBA content. This is because the large number of sulfonate groups in SBA are incorporated into the membrane, enhancing its water retention capacity and facilitating the formation of proton transport channels.
[0053] Figure 4 It is TG and DTG of SBPA-0, SBPA-20, SBPA-30 and SBPA-40.
[0054] The thermal stability of the proton exchange membrane is crucial for fuel cells, such as... Figure 4 The TG and DTG curves of SBPA-20, SBPA-30, and SBPA-40 are presented. We found two weight loss peaks at 300℃ and 400℃. The weight loss peak at 300℃ is due to the degradation of the sulfonate betaine groups on the side chain, while the weight loss peak at 400℃ is due to the degradation of the polymer backbone. We observed that the polymer membrane lost approximately 10% of its weight below 200℃, which may be due to the evaporation of residual solvent and some residual moisture within the membrane. Therefore, the main structure of the membrane did not degrade below 200℃, indicating that the SBPA series membranes can meet the thermal stability requirements of proton exchange membranes.
[0055] Figure 5 The percentage of residual mass and residual conductivity of SBPA-20, SBPA-30, and SBPA-40 membranes after immersion in 30% hydrogen peroxide solution for 300 hours.
[0056] Oxidation of proton exchange membranes is mainly due to the attack of peroxy (HOO-) and hydroxyl (-OH) free radicals generated by cross- or diffusion reactions between air and hydrogen. Therefore, the oxidation stability of SBPA series membranes was tested using a 30% H2O2 solution. After immersing the membranes in the 30% H2O2 solution for 300 h, it was found that SBPA-20 and SBPA-30 showed almost no mass loss, while SBPA-40 experienced a 10% mass loss. SBPA-20 showed almost no conductivity loss, SBPA-30 experienced a 7% conductivity loss, and SBPA-40 experienced a 35% conductivity loss. We found that the oxidation stability of the membrane decreased with increasing SBA content. This is because the relatively reduced polyacrylate content within the membrane leads to the inability of the carbon structure on the base membrane surface to effectively scavenge free radicals.
[0057] Figure 6 The mechanical properties of SBPA-20, SBPA-30, and SBPA-40 are described.
[0058] The mechanical properties of SBPA series membranes were studied at room temperature and 45% RH. We found that the membrane strength increased with the increase of SBA addition, with SBPA-40 reaching a strength of 3.7 MPa. This is because the introduction of zwitterionic groups increases the interaction force between molecular chains through electrostatic force, thereby improving the membrane strength. However, the elongation at break of the membrane decreased with the increase of SBA addition. This is because the addition of SBA increases the rigidity of the membrane, thus reducing its elongation at break.
[0059] Figure 7 Arrhenius curves for SBPA-20, SBPA-30, and SBPA-40.
[0060] Figure 7 The activation energy curves of the SBPA series membranes show that the activation energy is effectively reduced with increasing SBA dosage, with SBPA-40 exhibiting the lowest activation energy. A low activation energy indicates a lower energy barrier for proton conduction, which is more conducive to proton transport. Based on the calculated activation energy data, it is inferred that proton transport in the SBPA series membranes prepared in this invention is mainly dominated by the Grotthus mechanism. High levels of sulfonate ions and water molecules construct continuous proton conduction channels through hydrogen bonds, thereby reducing the barrier for proton hopping.
[0061] This invention utilizes polyacrylate as the matrix membrane and grafts sulfobetaine onto the polyacrylate backbone via solution polymerization to prepare a sulfobetaine-polyacrylate proton exchange membrane. The proton exchange membrane prepared by this invention exhibits good conductivity, chemical stability, and thermal stability. This invention employs mild reaction conditions, has a simple synthesis process, and uses readily available raw materials, making it suitable for industrial production and widespread application.
[0062] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.
Claims
1. A method for preparing a proton exchange membrane using polyacrylate as the matrix membrane, characterized in that: include, (1) Preparation of sulfonate betaine: Dimethylaminoethyl acrylate was added to a solvent to obtain a dimethylaminoethyl acrylate solution; 1,3-propanesulfonyl lactone was added to a solvent to obtain a 1,3-propanesulfonyl lactone solution; under an inert atmosphere, the mixture was heated, and the 1,3-propanesulfonyl lactone solution was slowly added to the dimethylaminoethyl acrylate solution to obtain the sulfonate betaine monomer; (2) Add sulfonyl betaine monomer, methyl methacrylate, butyl acrylate and hydroxyethyl methacrylate to a solvent, heat under an inert atmosphere, add an initiator dropwise to carry out the reaction, and add the resulting liquid to a template to obtain a proton exchange membrane. The mass ratio of methyl methacrylate to butyl acrylate is (1.5~2.5):3; the mass ratio of sulfonyl betaine monomer to methyl methacrylate is (0.6~1.9):1; and the mass ratio of methyl methacrylate to hydroxyethyl methacrylate is (3~5):
1.
2. The method for preparing a proton exchange membrane with polyacrylate as the matrix membrane according to claim 1, characterized in that: The mass ratio of the sulfonyl betaine monomer to methyl methacrylate is (6.13~9.53):5.
2.
3. The method for preparing a proton exchange membrane with polyacrylate as the matrix membrane according to claim 1 or 2, characterized in that: The mass ratio of methyl methacrylate to butyl acrylate is 2:
3.
4. The method for preparing a proton exchange membrane with polyacrylate as the matrix membrane according to claim 1 or 2, characterized in that: The mass ratio of methyl methacrylate to hydroxyethyl methacrylate is 4:
1.
5. The method for preparing a proton exchange membrane with polyacrylate as the matrix membrane according to claim 1 or 2, characterized in that: In step (2), the solvent is a mixture of N,N-dimethylformamide and water, wherein the mass ratio of N,N-dimethylformamide to water is 7:
1.
6. The method for preparing a proton exchange membrane with polyacrylate as the matrix membrane according to claim 1 or 2, characterized in that: In step (2), the inert atmosphere includes a nitrogen atmosphere; the heating is to raise the temperature to 75°C.
7. The method for preparing a proton exchange membrane with polyacrylate as the matrix membrane according to claim 1 or 2, characterized in that: In step (2), the initiator includes azobisisobutyronitrile, the reaction temperature is 75°C, and the reaction time is 8 h.
8. The method for preparing a proton exchange membrane with polyacrylate as the matrix membrane according to claim 1 or 2, characterized in that: In step (1), the molar ratio of dimethylaminoethyl acrylate to 1,3-propanesulfonyl lactone is 1:
1.
9. The method for preparing a proton exchange membrane with polyacrylate as the matrix membrane according to claim 1 or 2, characterized in that: In step (1), the heating temperature is 60°C.
10. The method for preparing a proton exchange membrane with polyacrylate as the matrix membrane according to claim 1 or 2, characterized in that: The solvents for both the dimethylaminoethyl acrylate solution and the 1,3-propanesulfonyl lactone solution are tetrahydrofuran.