A preparation method of black gold graphene thermal insulation fabric
By using the combined structure of outer polyester fiber, intermediate isolation layer spandex, inner graphene polyester fiber and copper-containing pyrrolidone-based black gold graphene treatment in graphene warm fabrics, the antibacterial and antibacterial properties of fabrics in the prior art are solved. The heavy problems caused by poor and thermal insulation are achieved, and the high-efficiency far-infrared function and excellent mechanical properties are achieved.
Patent Information
- Application Number
- CN202311528887.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-16
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-11-16
AI Technical Summary
The existing graphene warm-insulating fabrics have poor antibacterial and antibacterial properties and thermal insulation resistance lead to heavy fabrics, which cannot effectively maintain good far-infrared function in low temperature states.
The composition structure of outer polyester fiber, intermediate isolation layer spandex, inner graphene polyester fiber is prepared by dyeing, woven and finishing, combined with the treatment method of copper pyrrolidone-based black gold graphene, uniformly distributed graphene is prepared. Polyester fiber is made of composite non-woven fabric by needle puncture, which enhances the antibacterial and far-infrared functions of the fabric.
It has achieved high fracture strength, excellent mechanical properties, good antibacterial and antibacterial effects and significant far infrared functions. The fabric has good warmth and far infrared properties at low temperatures.
Abstract
Description
Technical Field
[0001] The invention relates to the field of textile materials, in particular to a method for preparing a graphene thermal insulation fabric. Background Art
[0002] Graphene has excellent properties such as high hardness, light weight, electrical conductivity and thermal conductivity. At present, my country's graphene industry has been listed as one of the key development areas. In the field of textile materials, graphene composite fibers have become a research hotspot in recent years. Graphene composite fibers are modified by adding graphene to polyester, viscose, acrylic and other fibers as the matrix, thereby giving the material antibacterial, antistatic, far-infrared heating and other properties, opening up the application market of conventional fibers in functional textiles. Chinese patent CN216466609U: discloses a graphene thermal insulation fabric, including a skin-friendly layer, a graphene layer and a thermal insulation layer, a moisture absorption layer is provided between the upper side of the skin-friendly layer and the lower side of the graphene layer, staggered heat-conducting wires are provided on the upper side of the graphene layer and the lower side of the thermal insulation layer, and heat-conducting sheets are evenly arranged on the heat-conducting wires, a surface layer is provided on the upper side of the thermal insulation layer, a cavity is evenly provided between the thermal insulation layer and the surface layer, a filler is provided in the cavity, and a waterproof layer is coated on the upper side of the surface layer. The utility model improves the uniformity of heat conduction on the inner side of the fabric by placing heat-conducting wires and heat-conducting sheets in contact with the lining yarn graphene fibers. Chinese patent CN115613153A: Provides a method for preparing graphene thermal insulation fabrics. A method for preparing graphene thermal insulation fabrics, the preparation steps of the graphene thermal insulation fabrics are as follows: S1, prepare graphene oxide solution; S2, prepare polyvinyl alcohol-graphene oxide solution; S3, prepare spinning solution; S4, weave the spinning solution on viscose fiber through an electrostatic spinning device to prepare graphene composite fiber, and blend the graphene composite fiber with aerogel fiber to prepare fabric; S5, dye and shape the fabric to obtain graphene thermal insulation fabric. The thermal insulation fabric prepared by the present invention is light and skin-friendly. Graphene oxide is made into fiber material for weaving thermal insulation fabrics, so that the prepared graphene thermal insulation underwear has anti-inflammatory and antibacterial functions, and has a good thermal insulation effect. Chinese patent CN109537270A: It relates to the field of clothing fabric preparation, and specifically to a method for preparing a graphene sanded inner warm microcirculation fabric, which includes the following steps: weaving → making finishing liquid → soaking → drying → dyeing → post-treatment. The graphene sanded inner warm microcirculation fabric prepared according to the above steps is soaked in finishing liquid, which enhances the inherent hygroscopicity and breathability of the fiber, and the fabric is smooth and soft, and feels smooth; at the same time, it perfectly reflects the efficacy of black gold graphene, the most obvious of which is the enhancement of body temperature far infrared effect. The manual states that at a low temperature of 20-35℃, the absorption rate of 6-14μm wavelength far infrared light is more than 88%, and the powerful body temperature far infrared function improves the body microcirculation. Most of the thermal insulation fabrics prepared by the above patents and prior art adopt heat-resistant warmth, that is, they are kept warm by wearing heavy down jackets, cotton-padded jackets, etc., and the antibacterial and antibacterial properties of the fabrics are poor. Summary of the invention
[0003] A main purpose of the present invention is to provide a method for preparing a graphene thermal insulation fabric, which is composed of an outer layer of polyester fiber, a middle isolation layer of spandex, and an inner layer of graphene polyester fiber, and is subjected to dyeing, napping, and post-finishing.
[0004] Process, to obtain graphene thermal fabric.
[0005] One embodiment of the present invention also provides a graphene polyester fiber, and the preparation method thereof is as follows: 80-95 parts of polyester chips are weighed by weight, and the polyester chips are ground into powder using a plastic grinder; S2: 0.5-1 parts of a dispersant and 5-15 parts of copper-containing pyrrolidone-based black gold graphene are added, and stirred and mixed.
[0006] After being uniformed, it is sent to a twin-screw extruder for extrusion and pelletization to obtain black gold graphene polyester masterbatch; S3: the black gold graphene polyester masterbatch is spun by a spinning machine, formed by side blowing, stretched, and sizing to obtain graphene polyester fiber.
[0007] Further, the dispersant is a polycarboxylate, a poly(meth)acrylic acid derivative, or a maleic anhydride copolymer. Further, the extrusion temperature in the screw extruder is 180-220°C. Further, the spinning temperature is 250-270°C. Further, the spinning speed is 2400-2800 m / min. Further, the side blowing temperature is 15-25°C. Further, the stretching multiple is 1.3-1.7.
[0008] One embodiment of the present invention also provides a method for processing copper-pyrrolidone-based black gold graphene, which is as follows:
[0009] B1: Place black gold graphene in a plasma surface treatment instrument, introduce ammonia into the plasma surface treatment instrument, set the power to 150-250W, and treat for 10-20min to obtain amino biomass graphene; B2: Add 33-45 parts by weight of a 10-16% zinc pyrrolidone carboxylate aqueous solution,
[0010] 500-700 parts of ethanol, 20-40 parts of copper acrylate, 5-10 parts of sodium ethoxide, stir at 50-60℃ for 100-150 minutes, then add 100-150 parts of amino black gold graphene, stir at 50-60℃ for 30-60 minutes, then filter, wash with water, and dry to obtain copper-containing pyrrolidone-based black gold graphene.
[0011] Furthermore, the ammonia flow rate is 1-100 mL / min.
[0012] The outer layer of the graphene thermal insulation fabric is 100D polyester fiber, the inner layer is 75D graphene plus 75D polyester fiber, and the middle isolation layer is 100% spandex. The composite non-woven fabric is woven by a large circular machine, and the graphene thermal insulation fabric is compounded by a needle punching method; the outer layer of the graphene thermal insulation fabric is plain, the middle isolation layer is spandex, and the inner layer is checkered, and then it is processed into black gold graphene velvet through dyeing and napping. The needle density of the needle punching machine used in the needle punching method is 220 times / cm2, the needle depth is 8mm, 6mm, 4mm, 2mm, 0mm, and the vehicle speed is 2.5m / min; the warp shrinkage of the graphene thermal insulation fabric is 14%, the weft shrinkage is 19%, and the graphene thermal insulation fabric has a warp shrinkage of 14%, a weft shrinkage of 19%, and a thickness of 100mm.
[0013] The graphene thermal fabric shrinks consistently without curling.
[0014] Reaction mechanism:
[0015] Zinc pyrrolidone carboxylate reacts with one double bond of copper acrylate to undergo an amino-acrylic acid addition reaction, and the other double bond of copper acrylate reacts with amino black gold graphene to undergo an amino-acrylic acid addition reaction to obtain copper-containing pyrrolidone carboxylate.
[0016] Pyrrolidone-based black gold graphene.
[0017] Technical effect:
[0018] The preparation method of a graphene thermal insulation fabric of the present invention has the following remarkable effects compared with the prior art: 1. The black gold graphene of the present invention is evenly distributed in the polyester fiber, and the black gold graphene has no agglomeration phenomenon, and the fiber surface is smooth; 2. The graphene polyester fiber prepared by the present invention has high breaking strength, indicating that the fiber has excellent mechanical properties and can meet the requirements of fiber mechanical properties; 3. The copper-based, zinc pyrrolidonecarboxylate graphene hybrid of the present invention has high temperature resistance, can be subjected to high temperature extrusion and high temperature spinning, and still has good UV resistance, lubrication, dustproof, breathable and sterilization effects; 4. The graphene thermal insulation fabric prepared by the present invention has the advantages of warmth preservation, antibacterial, far infrared and temperature increase; the antibacterial rate to Escherichia coli, Staphylococcus aureus and Candida albicans is high, and has good antibacterial and antibacterial effects; the far infrared radiation temperature rise value of the fabric is 2.5°C. The far infrared emissivity is 0.95, indicating that the fabric has good far infrared function. DETAILED DESCRIPTION
[0019] Typical embodiments that embody the features and advantages of the present invention will be described in detail in the following description. It should be understood that the present invention can have various changes in different embodiments without departing from the scope of the present invention, and the descriptions therein are essentially used as illustrations rather than to limit the present invention.
[0020] Evaluation method:
[0021] 1. Breaking strength: refer to GB / T14464-2008 "Polyester staple fiber" test; 2. Antibacterial performance: refer to GB / T20944.3-2008 "Evaluation of antibacterial properties of textiles Part 3: Oscillation method" test; 3. Far infrared performance: according to GB / T30127-2013 "Testing and evaluation of far infrared properties of textiles"
[0022] test.
[0023] Example 1
[0024] A method for preparing a graphene thermal insulation fabric comprises an outer layer of polyester fiber, a middle isolation layer of spandex, and an inner layer of graphene polyester fiber, and the graphene thermal insulation fabric is obtained through dyeing, napping, and post-finishing.
[0025] The graphene polyester fiber is prepared by:
[0026] S1: Weigh 80g of polyester chips and grind them into powder using a plastic grinder; S2: Add 0.5g of dispersant and 5g of copper-pyrrolidone-based black gold graphene, stir and mix evenly, then send them into a twin-screw extruder for extrusion and pelletization to obtain black gold graphene polyester masterbatch; S3: Spin the black gold graphene polyester masterbatch through a spinning machine, form it with side blowing, stretch it, and apply sizing.
[0027] Graphene polyester fiber is obtained.
[0028] The dispersant is polycarboxylate.
[0029] The extrusion temperature in the screw extruder is 180°C.
[0030] The spinning temperature is 250°C.
[0031] The spinning speed is 2400 m / min.
[0032] The side blowing temperature is 15°C.
[0033] The stretching ratio is 1.3.
[0034] The processing conditions of the copper-containing pyrrolidone-based black gold graphene are:
[0035] B1: Place the black gold graphene into a plasma surface treatment instrument, introduce ammonia into the plasma surface treatment instrument, set the power to 150W, and treat for 10 minutes to obtain amino black gold graphene; B2: Add 33g of 10% by mass zinc pyrrolidonecarboxylate aqueous solution, 500g of ethanol, 20g of copper acrylate, and 5g of sodium ethoxide, stir at 50°C for 100 minutes, then add 100g of amino black gold graphene, stir at 50°C for 30 minutes, then filter, wash with water, and dry to obtain copper-containing pyrrolidone-based black gold graphene.
[0036] The ammonia flow rate is 1 mL / min.
[0037] The outer layer of the graphene thermal insulation fabric is 100D polyester fiber, the inner layer is 75D graphene plus 75D polyester fiber, and the middle isolation layer is 100% spandex. The composite non-woven fabric is made by large circular knitting machine, and the graphene thermal insulation fabric is compounded by needle punching method; the outer layer of the graphene thermal insulation fabric is plain weave, the middle isolation layer is spandex, and the inner layer is checkered, and then processed into black gold graphene velvet by dyeing and napping. The needle density of the needle punching machine used in the needle punching method is 220 times / cm2, the needle depth is 8mm, 6mm, 4mm, 2mm, 0mm, and the speed is 2.5m / min; the warp shrinkage of the graphene thermal insulation fabric is 14%, the weft shrinkage is 19%, and the shrinkage of the graphene thermal insulation fabric is consistent without curling.
[0038] Example 2
[0039] A method for preparing a graphene thermal insulation fabric comprises an outer layer of polyester fiber, a middle isolation layer of spandex, and an inner layer of graphene polyester fiber, and the graphene thermal insulation fabric is obtained through dyeing, napping, and post-finishing.
[0040] The graphene polyester fiber is prepared by:
[0041] S1: Weigh 85g of polyester chips and grind them into powder using a plastic grinder; S2: Add 0.6g of dispersant and 8g of copper-pyrrolidone-based black gold graphene, stir and mix evenly, then send them into a twin-screw extruder for extrusion and pelletization to obtain black gold graphene polyester masterbatch; S3: The black gold graphene polyester masterbatch is spun by a spinning machine, formed by side blowing, stretched, and sized to obtain graphene polyester fiber.
[0042] The dispersant is a poly(meth)acrylic acid derivative.
[0043] The extrusion temperature in the screw extruder is 190°C.
[0044] The spinning temperature is 255°C.
[0045] The spinning speed is 2500m / min.
[0046] The side blowing temperature is 18°C.
[0047] The stretching ratio is 1.4.
[0048] The processing conditions of the copper-containing pyrrolidone-based black gold graphene are:
[0049] B1: Place the black gold graphene into a plasma surface treatment instrument, introduce ammonia into the plasma surface treatment instrument, set the power to 200W, and treat for 15 minutes to obtain amino black gold graphene; B2: Add 38g of 12% by mass zinc pyrrolidonecarboxylate aqueous solution, 550g of ethanol, 25g of copper acrylate, and 6g of sodium ethoxide, stir at 55°C for 110 minutes, then add 110g of amino black gold graphene, stir at 55°C for 40 minutes, then filter, wash with water, and dry to obtain copper-containing pyrrolidone-based black gold graphene.
[0050] The ammonia flow rate is 30 mL / min.
[0051] The outer layer of the graphene thermal insulation fabric is 100D polyester fiber, the inner layer is 75D graphene plus 75D polyester fiber, and the middle isolation layer is 100% spandex. The composite non-woven fabric is made by large circular knitting machine, and the graphene thermal insulation fabric is compounded by needle punching method; the outer layer of the graphene thermal insulation fabric is plain weave, the middle isolation layer is spandex, and the inner layer is checkered, and then processed into black gold graphene velvet by dyeing and napping. The needle density of the needle punching machine used in the needle punching method is 220 times / cm2, the needle depth is 8mm, 6mm, 4mm, 2mm, 0mm, and the speed is 2.5m / min; the warp shrinkage of the graphene thermal insulation fabric is 14%, the weft shrinkage is 19%, and the shrinkage of the graphene thermal insulation fabric is consistent without curling.
[0052] Example 3
[0053] A method for preparing a graphene thermal insulation fabric comprises an outer layer of polyester fiber, a middle isolation layer of spandex, and an inner layer of graphene polyester fiber, and the graphene thermal insulation fabric is obtained through dyeing, napping, and post-finishing.
[0054] The graphene polyester fiber is prepared by:
[0055] S1: Weigh 90g of polyester chips and grind them into powder using a plastic grinder; S2: Add 0.8g of dispersant and 13g of copper-pyrrolidone-based black gold graphene, stir and mix evenly, then send them into a twin-screw extruder for extrusion and pelletization to obtain black gold graphene polyester masterbatch; S3: The black gold graphene polyester masterbatch is spun by a spinning machine, formed by side blowing, stretched, and sized to obtain graphene polyester fiber.
[0056] The dispersant is a poly(meth)acrylic acid derivative.
[0057] The extrusion temperature in the screw extruder is 210°C.
[0058] The spinning temperature is 265°C.
[0059] The spinning speed is 2700 m / min.
[0060] The side blowing air temperature is 23°C.
[0061] The stretching ratio is 1.6.
[0062] The processing conditions of the copper-containing pyrrolidone-based black gold graphene are:
[0063] B1: Place the black gold graphene into a plasma surface treatment instrument, introduce ammonia into the plasma surface treatment instrument, set the power to 200W, and treat for 15 minutes to obtain amino black gold graphene; B2: Add 42g of 14% by mass zinc pyrrolidonecarboxylate aqueous solution, 650g of ethanol, 35g of copper acrylate, and 8g of sodium ethoxide, stir at 55°C for 140 minutes, then add 140g of amino black gold graphene, stir at 55°C for 50 minutes, then filter, wash with water, and dry to obtain copper-containing pyrrolidone-based black gold graphene.
[0064] The ammonia flow rate is 80 mL / min.
[0065] The outer layer of the graphene thermal insulation fabric is 100D polyester fiber, the inner layer is 75D graphene plus 75D polyester fiber, and the middle isolation layer is 100% spandex. The composite non-woven fabric is made by large circular knitting machine, and the graphene thermal insulation fabric is compounded by needle punching method; the outer layer of the graphene thermal insulation fabric is plain weave, the middle isolation layer is spandex, and the inner layer is checkered, and then processed into black gold graphene velvet by dyeing and napping. The needle density of the needle punching machine used in the needle punching method is 220 times / cm2, the needle depth is 8mm, 6mm, 4mm, 2mm, 0mm, and the speed is 2.5m / min; the warp shrinkage of the graphene thermal insulation fabric is 14%, the weft shrinkage is 19%, and the shrinkage of the graphene thermal insulation fabric is consistent without curling.
[0066] Example 4
[0067] A method for preparing a graphene thermal insulation fabric comprises an outer layer of polyester fiber, a middle isolation layer of spandex, and an inner layer of graphene polyester fiber, and the graphene thermal insulation fabric is obtained through dyeing, napping, and post-finishing.
[0068] The graphene polyester fiber is prepared as follows: S1: weigh 95g of polyester chips, and grind the polyester chips into powder using a plastic grinder; S2: add 1g of dispersant and 15g of copper-containing pyrrolidone-based black gold graphene, stir and mix evenly, and then send them into a twin-screw extruder for extrusion and pelletization to obtain black gold graphene polyester masterbatch; S3: spin the black gold graphene polyester masterbatch through a spinning machine, form it with side blowing, stretch it, and sizing it to obtain graphene polyester fiber.
[0069] S3: Black gold graphene polyester masterbatch is spun by a spinning machine, formed by side blowing, stretched, and sizing to obtain graphene polyester fiber.
[0070] The extrusion temperature in the screw extruder is 220°C.
[0071] The spinning temperature is 270°C.
[0072] The spinning speed is 2800 m / min.
[0073] The side blowing air temperature is 25°C.
[0074] The stretching ratio is 1.7.
[0075] The processing conditions of the copper-containing pyrrolidone-based black gold graphene are:
[0076] B1: Place the black gold graphene into a plasma surface treatment instrument, introduce ammonia into the plasma surface treatment instrument, set the power to 250W, and treat for 20 minutes to obtain amino black gold graphene; B2: Add 45g of 16% by mass zinc pyrrolidonecarboxylate aqueous solution, 700g of ethanol, 40g of copper acrylate, and 10g of sodium ethoxide, stir at 60°C for 150 minutes, then add 150g of amino black gold graphene, stir at 60°C for 60 minutes, then filter, wash with water, and dry to obtain copper-containing pyrrolidone-based black gold graphene.
[0077] The ammonia flow rate is 100 mL / min.
[0078] The outer layer of the graphene thermal insulation fabric is 100D polyester fiber, the inner layer is 75D graphene plus 75D polyester fiber, and the middle isolation layer is 100% spandex. The composite non-woven fabric is made by large circular knitting machine, and the graphene thermal insulation fabric is compounded by needle punching method; the outer layer of the graphene thermal insulation fabric is plain weave, the middle isolation layer is spandex, and the inner layer is checkered, and then it is processed into black gold graphene velvet by dyeing and napping. The needle density of the needle punching machine used in the needle punching method is 220 times / cm2, the needle depth is 8mm, 6mm, 4mm, 2mm, 0mm, and the speed is 2.5m / min; the warp shrinkage of the graphene thermal insulation fabric is 14%, the weft shrinkage is 19%, and the shrinkage of the graphene thermal insulation fabric is consistent without curling.
[0079] Comparative Example 1
[0080] No copper-pyrrolidone-based black gold graphene is added, and ordinary graphene is added. Others are the same as in Example 1.
[0081] Comparative Example 2
[0082] The zinc pyrrolidonecarboxylate aqueous solution was not added, and the other conditions were the same as in Example 1.
[0083] Comparative Example 3
[0084] No copper acrylate was added, and the rest was the same as in Example 1.
[0085] Breaking strength cN / dtex Escherichia coli inhibition rate% Staphylococcus aureus inhibition rate% Candida albicans inhibition rate% Far infrared emissivity / % Far infrared radiation temperature rise / ℃ Example 1 5.3 99.52 98.27 99.19 0.88 1.9 Example 2 5.4 99.63 98.43 99.32 0.91 2.2 Example 3 5.6 99.75 98.51 99.46 0.94 2.4 Example 4 5.7 99.87 98.63 99.56 0.95 2.5 Comparative Example 1 3.4 88.44 85.24 87.87 0.51 0.6 Comparative Example 2 4.0 91.95 91.61 91.91 0.67 1.1 Comparative Example 3 4.2 92.16 92.33 93.53 0.71 1.2
[0086] Through the data analysis of the above embodiments and comparative examples, the graphene polyester fiber prepared by the present invention has high breaking strength, which indicates that the fiber has excellent mechanical properties.
[0087] The graphene thermal insulation fabric prepared by the present invention has a high antibacterial rate against Escherichia coli, Staphylococcus aureus and Candida albicans, and has good antibacterial and antibacterial effects; the far-infrared radiation temperature rise value of the fabric is 2.5°C and the far-infrared emissivity is 0.95, indicating that the fabric has good far-infrared function.
[0088] Unless otherwise defined, the terms used in the present invention have the meanings commonly understood by those skilled in the art.
[0089] The embodiments described in the present invention are for illustrative purposes only and are not intended to limit the scope of protection of the present invention. Those skilled in the art may make various other substitutions, changes and improvements within the scope of the present invention. Therefore, the present invention is not limited to the above embodiments, but is only limited by the claims.
Claims
1. A method for preparing a graphene thermal insulation fabric, which comprises an outer layer of polyester fiber, a middle isolation layer of spandex, and an inner layer of graphene polyester fiber, and is processed by dyeing, napping, and post-finishing to obtain the graphene thermal insulation fabric; The graphene polyester fiber is prepared by: S1: Weigh 80-95 parts of polyester chips by weight, and grind the polyester chips into powder using a plastic grinder; S2: adding 0.5-1 parts of dispersant and 5-15 parts of copper-containing pyrrolidone-based black gold graphene, stirring and mixing evenly, and then feeding into a twin-screw extruder for extrusion and pelletization to obtain black gold graphene polyester masterbatch; S3: Black gold graphene polyester masterbatch, spun by a spinning machine, formed by side blowing, stretched, and sized to obtain graphene polyester fiber; The processing conditions of the copper-pyrrolidone-based black gold graphene are as follows: B1: Place the black gold graphene into a plasma surface treatment instrument, introduce ammonia into the plasma surface treatment instrument, set the power to 150-250W, and the treatment time to 10-20min to obtain amino biomass graphene; B2: By weight, 33-45 parts of 10-16% zinc pyrrolidonecarboxylate aqueous solution, 500-700 parts of ethanol, 20-40 parts of copper acrylate, 5-10 parts of sodium ethoxide, stir at 50-60°C for 100-150 minutes, add 100-150 parts of amino black gold graphene, stir at 50-60°C for 30-60 minutes, then filter, wash with water, and dry to obtain copper-containing pyrrolidone-based black gold graphene.
2. A method for preparing a graphene thermal insulation fabric according to claim 1, Features: The dispersant is polycarboxylate, poly(methyl)acrylic acid derivative, maleic anhydride copolymer.
3. A method for preparing a graphene thermal insulation fabric according to claim 1, Features: The extrusion temperature in the screw extruder is 180-220° C.; the spinning temperature is 250-270° C.; and the spinning speed is 2400-2800 m / min.
4. A method for preparing a graphene thermal insulation fabric according to claim 1, Features: The outer layer of the graphene thermal insulation fabric is 100D polyester fiber, the inner layer is 75D graphene plus 75D polyester fiber, and the middle isolation layer is 100% spandex. The composite non-woven fabric is made by knitting with a large circular machine.
5. A method for preparing a graphene thermal insulation fabric according to claim 1, Features: The graphene thermal insulation fabric is compounded by needle punching; the outer layer of the graphene thermal insulation fabric is plain weave, the middle isolation layer is spandex, the inner layer is checkered, and then it is processed into black gold graphene velvet by dyeing and napping; The needle density of the needle punching machine used in the acupuncture method is 220 times / cm 2 The needle depths are 8mm, 6mm, 4mm, 2mm, and 0mm respectively, and the vehicle speed is 2.5m / min; the warp shrinkage of the graphene thermal insulation fabric is 14%, and the weft shrinkage is 19%. The shrinkage of the graphene thermal insulation fabric is consistent without curling.
6. A method for preparing a graphene thermal insulation fabric according to claim 1, Features: The side blowing air temperature is 15-25°C.
7. A method for preparing a graphene thermal insulation fabric according to claim 1, Features: The stretching ratio is 1.3-1.
7.
8. The method for preparing a graphene thermal insulation fabric according to claim 1, Features: The ammonia flow rate is 30-50 mL / min.