A high-value conversion method for depolymerization of waste PET by coupling levulinic acid

By coupling waste PET depolymerization by levulinic acid, the PET depolymerization product ethylene glycol as a hydrogen source, combined with noble metal-supported molecular sieve catalyst, γ-valerolactone and terephthalic acid are directly prepared, and acetylepropylene in the prior art was solved The high cost of separation and purification of the exohydrogen source and PET hydrolysate is required to prepare γ-valerolide, which has achieved the upgrading and utilization of biomass resources and the high value of waste plastics.

CN117567399BActive Publication Date: 2024-11-19ZHEJIANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311592776.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-27
Publication Date
2024-11-19
Estimated Expiration
2043-11-27

AI Technical Summary

Technical Problem

In the prior art, the preparation of γ-valerolide of levulinic acid requires an exohydrogen source, and the separation and purification cost of the PET hydrolysate ethylene glycol is high, which hinders the high value recycling of waste PET.

Method used

By coupling waste PET depolymerization by levulinic acid, the PET depolymerization product ethylene glycol is used as the hydrogen source to perform a one-pot depolymerization-hydrogenation reaction, combined with noble metal-supported molecular sieve catalyst, γ-valerolactone and terebenzene are directly prepared Dicarboxylic acid.

Benefits of technology

The upgrade and utilization of biomass resources and the high value of waste plastics have been achieved, exohydrogen sources have been avoided, the yields of γ-valerolide and terephthalic acid have been improved, and the consumption of fossil resources has been reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117567399B_ABST
    Figure CN117567399B_ABST
Patent Text Reader

Abstract

The present invention provides a high-value conversion method for coupling levulinic acid with waste PET depolymerization. The method uses biomass derivative levulinic acid and waste plastic polyethylene terephthalate (PET) as raw materials, noble metal-loaded molecular sieves as catalysts, and reacts in an initial atmospheric nitrogen atmosphere, a reaction temperature of 210°C to 240°C, and different depolymerization aids in water for 6 to 24 hours to obtain γ-valerolactone and terephthalic acid. Compared with the existing γ-valerolactone production and PET depolymerization technology, the present invention cleverly utilizes the hydrogen energy contained in the ethylene glycol unit of the difficult-to-separate PET depolymerization product, and simultaneously solves the problems of high-value recycling of waste plastics and utilization of biomass resources faced by the world. This reaction coupling method can not only reduce the pollution of waste plastics and agricultural biomass waste, slow down the consumption of fossil resources, but also achieve the synchronous production of high-value products γ-valerolactone and terephthalic acid.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of chemical industry and polyester waste recycling, and specifically relates to a method for waste treatment and high-value chemical value-added recovery of preparing gamma-valerolactone and terephthalic acid by depolymerization of levulinic acid coupled waste PET. Background Art

[0002] Today, the reserves of easily accessible fossil resources are decreasing, while the market demand for chemicals and fuels is increasing. Biomass energy, as the fourth largest energy source in the world after coal, oil and natural gas, has great potential to gradually replace fossil resources. Therefore, it is urgent to develop an effective catalytic route from renewable biomass to fuels and chemicals. Levulinic acid, as an important biomass-derived platform compound, is easily hydrogenated and reduced to obtain γ-valerolactone. γ-Valerolactone is known as one of the most important green bio-based platform compounds in the 21st century. It has a wide range of uses. It can be used as an excellent green solvent and as a precursor of high-value platform chemicals such as butene, valeric acid, 2-methyltetrahydrofuran, 1,4-pentanediol and 5-nonanone. It can also produce "second-generation biofuels". At present, hydrogen is mainly used as the hydrogen source for the preparation of γ-valerolactone using levulinic acid, but the application of hydrogen is limited to a certain extent due to its safety issues and difficulties in transportation and storage.

[0003] Ethylene glycol is considered to be a potential liquid hydrogen source. It is also the main product of the hydrolysis of waste PET. As the main source of disposable plastic packaging, PET has the characteristics of being quickly discarded after use, and its annual output is as high as 70 million tons, making it one of the main sources of waste plastic pollution. Exploring high-value waste PET treatment methods is one of the most promising solutions to eliminate PET plastic pollution and develop a circular economy. Chemical recycling has attracted widespread attention because it can recycle PET at the molecular level, and the products can be directly used as industrial raw materials and reduce the consumption of petroleum energy. Among them, hydrolysis is the most widely studied chemical recycling strategy. PET can be hydrolyzed to obtain terephthalic acid and ethylene glycol, but due to the high cost of separating and purifying ethylene glycol in the aqueous phase, it is usually directly discarded as waste liquid, which hinders the high-value recycling of hidden hydrogen sources in waste PET. Summary of the invention

[0004] In view of the defects in the prior art, the purpose of the present invention is to provide a high-value conversion method of levulinic acid coupled with waste PET depolymerization. The present invention couples the preparation of γ-valerolactone by hydrogenation and cyclization of levulinic acid with the depolymerization of waste PET, and the two react synergistically. The PET depolymerization product ethylene glycol is directly used as a green hydrogen source to supply hydrogen to levulinic acid through a one-pot method, and finally γ-valerolactone and terephthalic acid are obtained by simple purification. This new green technology can simultaneously solve the problems of the greenness of the hydrogen source of levulinic acid hydrogenation and the further high-value utilization of the PET depolymerization product ethylene glycol, open up a new path for the utilization of biomass resources and the management of waste plastics, and reduce the consumption of fossil resources.

[0005] The present invention is achieved through the following technical solutions:

[0006] A high-value conversion method for levulinic acid-coupled waste PET depolymerization, comprising: placing polyethylene terephthalate (PET), a catalyst, levulinic acid, a depolymerization aid and water in a closed reactor in an inert atmosphere, performing a depolymerization-hydrogenation reaction at 210° C. to 240° C., separating the reaction product into solid and liquid after the reaction is completed, collecting and purifying the liquid product to obtain γ-valerolactone and terephthalic acid;

[0007] The depolymerization aid is one of sodium hydroxide and terephthalic acid;

[0008] The catalyst is a noble metal-loaded molecular sieve catalyst formed by loading noble metal Pt on MCM-41 molecular sieve.

[0009] The technical route of the above reaction in the present invention is as follows:

[0010]

[0011] Preferably, the inert atmosphere is a nitrogen atmosphere with an initial pressure of normal pressure. However, this is only the initial pressure. When the reaction proceeds, the pressure in the sealed reactor can gradually rise to 3-6 MPa, which is sufficient to meet the reaction conditions.

[0012] Preferably, the noble metal-loaded molecular sieve is obtained by sequentially drying and reductive calcining an impregnation solution formed by ultrasonically mixing MCM-41 molecular sieve and PtCl4 solution.

[0013] Preferably, the depolymerization aid is terephthalic acid, because terephthalic acid is both a depolymerization aid and a product, and the system is more environmentally friendly.

[0014] Preferably, the mass ratio of levulinic acid to PET, catalyst, depolymerization aid and water is 2:1 to 2:0.3 to 1:0.4 to 1:20 to 30.

[0015] Furthermore, when preparing the noble metal-loaded molecular sieve, in the impregnation solution, the ratio of Pt in PtCl4 to the total mass of Pt and MCM-41 molecular sieve is 0.01 to 0.1.

[0016] Furthermore, when preparing the noble metal-loaded molecular sieve, the ratio of Pt in PtCl4 to the total mass of Pt and MCM-41 molecular sieve in the impregnation solution is preferably 0.05.

[0017] Furthermore, when preparing the noble metal-loaded molecular sieve, the drying temperature is 20-70°C.

[0018] Furthermore, when preparing the noble metal loaded molecular sieve, the ultrasonic mixing adopts an ultrasonic frequency of 10 to 90 kHz, preferably 40 kHz. Too high a frequency will result in high energy and damage to the molecular sieve structure, while too low a frequency will result in uneven loading.

[0019] Furthermore, when preparing the noble metal-loaded molecular sieve, the atmosphere used in the reducing roasting is a hydrogen-argon mixed gas with a hydrogen volume percentage of 2% to 20%.

[0020] Furthermore, when preparing the noble metal-loaded molecular sieve, the reduction calcination temperature is 50 to 500° C. and the time is 4 to 8 hours.

[0021] Furthermore, the reaction time of the depolymerization-hydrogenation reaction is 6 to 24 hours.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1. The present invention couples the preparation of γ-valerolactone from levulinic acid with the hydrolysis of PET, and utilizes ethylene glycol, a depolymerization product of PET, as a hydrogen source for hydrogenation of levulinic acid, thereby avoiding the need for an external hydrogen source and solving the problem of separation and purification of ethylene glycol, thereby achieving the upgraded utilization of biomass derivatives and the high value of waste plastics;

[0024] 2. The unique mesoporous structure of the noble metal-supported molecular sieve catalyst used in the present invention is conducive to the uniform dispersion of the noble metal and further catalysis of the reaction process of ethylene glycol dehydrogenation and levulinic acid hydrogenation cyclization. The high surface area is conducive to the contact and depolymerization of PET with the active sites. At the same time, as a solid heterogeneous catalyst, it is easy to recycle;

[0025] 3. The yield of γ-valerolactone in the present invention can reach up to 87.0% at the highest, and the effect is excellent under the condition of alcohol hydrogen source. In addition, the yield of terephthalic acid can reach up to 99.1%. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is the hydrogen nuclear magnetic spectrum of disodium terephthalate of Example 2 of the present invention

[0027] Figure 2 This is the hydrogen nuclear magnetic spectrum of γ-valerolactone and by-products of Example 2 of the present invention. DETAILED DESCRIPTION

[0028] In order to make the above-mentioned purpose, features and advantages of the present invention more obvious and easy to understand, a detailed description is given below through specific embodiments. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below. The technical features in each embodiment of the present invention can be combined accordingly without conflicting with each other.

[0029] The invention provides a high-value conversion method for depolymerization of levulinic acid coupled with waste PET. The specific method comprises the following steps: placing polyethylene terephthalate (PET), a catalyst, levulinic acid, a depolymerization aid and water in a closed reactor in an inert atmosphere, performing a depolymerization-hydrogenation reaction at 210° C. to 240° C. for 6 to 24 hours, separating the reaction product into solid and liquid after the reaction is completed, collecting and purifying the liquid product to obtain gamma-valerolactone and terephthalic acid.

[0030] The present invention ingeniously utilizes the hidden hydrogen of the ethylene glycol unit of the PET depolymerization product which is difficult to separate, and simultaneously solves the problems of high-value recycling of waste plastics and utilization of biomass resources faced by the world. Through this reaction coupling mode, not only can the pollution of waste plastics and agricultural biomass waste be reduced and the consumption of fossil resources be slowed down, but also the simultaneous production of high-value products γ-valerolactone and terephthalic acid can be achieved.

[0031] In the subsequent examples, the raw materials in the above reaction system are as follows: the depolymerization aid is one of sodium hydroxide and terephthalic acid; the catalyst is a noble metal-loaded molecular sieve catalyst formed by loading the noble metal Pt on the MCM-41 molecular sieve. The noble metal-loaded molecular sieve can be obtained by ultrasonically mixing the MCM-41 molecular sieve and the PtCl4 solution to form an impregnation solution, and then drying and reducing roasting the impregnation solution in sequence.

[0032] In the subsequent examples, two noble metal supported molecular sieve catalysts were mainly used, namely 5% Pt / MCM-41 and 10% Pt / MCM-41, and the preparation methods of the two catalysts were as follows:

[0033] Preparation of 5% Pt / MCM-41 (the proportion of Pt in PtCl4 to the total mass of Pt and MCM-41 molecular sieve is 5%): Use an electronic balance to weigh 1.0000g MCM-41 molecular sieve and 0.0908g PtCl4 respectively, add them into a 75mm watch glass, then add 10ml distilled water to mix, put the mixture into an XM-400UVF ultrasonic cleaning machine, ultrasonicate at a frequency of 40kHz for 5min, then let it stand for 1min, repeat ultrasonication-standing three times to obtain a uniform light yellow suspension. After the suspension was dried in an oven at 50°C for 24 hours, the solid was ground into powder using an agate mortar and transferred to a porcelain boat. The powder was then placed in an OTF-1200X tube furnace and calcined in a 5% H2-Ar (i.e., a mixture of H2 and Ar with a H2 volume percentage of 5%) atmosphere. The reduction procedure was to increase the temperature from room temperature to 400°C at 10°C / min, maintain a constant temperature of 400°C for 5 hours, and then cool to room temperature. The resulting catalyst was 5% P / MCM-41.

[0034] Preparation of 10% Pt / MCM-41 (the proportion of Pt in PtCl4 to the total mass of Pt and MCM-41 molecular sieve is 10%): 1.0000g MCM-41 molecular sieve and 0.1920g PtCl4 were weighed separately using an electronic balance, added to a 75mm watch glass, and then 10ml of distilled water was added to mix. The mixture was placed in an XM-400UVF ultrasonic cleaning machine, ultrasonicated at a frequency of 40kHz for 5min and then allowed to stand for 1min. The ultrasonic-standing process was repeated three times to obtain a uniform light yellow suspension. After the suspension was dried in an oven at 50°C for 24 hours, the solid was ground into powder using an agate mortar and transferred to a porcelain boat. The powder was then placed in an OTF-1200X tube furnace and calcined in a 5% H2-Ar (i.e., a mixture of H2 and Ar with a H2 volume percentage of 5%) atmosphere. The reduction procedure was to increase the temperature from room temperature to 400°C at 10°C / min, maintain a constant temperature of 400°C for 5 hours, and then cool to room temperature. The resulting catalyst was 10% Pt / MCM-41.

[0035] The following examples are used to demonstrate the reaction results under different raw materials and parameters. The noble metal supported molecular sieve catalysts 5% Pt / MCM-41 and 10% Pt / MCM-41 were prepared by the above method, which will not be described in detail later.

[0036] Example 1

[0037] A high-value conversion method for depolymerization of waste PET coupled with levulinic acid provided in this embodiment comprises the following steps:

[0038] 0.1900g of levulinic acid, 0.0960g of PET, 0.0500g of 5% Pt / MCM-41, 1ml of 1mol / LNaOH solution and 1ml of water were added to a 10ml polytetrafluoroethylene liner in sequence and placed in a high-pressure reactor. Nitrogen was charged and discharged into the reactor several times. After the air was removed, the reactor was deflated and sealed. The reactor was placed on a heating plate and stirred and heated to 230°C. The reaction was carried out for 18 hours. After the reaction was completed, it was cooled to room temperature to complete the high-value conversion process of levulinic acid coupling depolymerization of waste PET, and subsequent product purification and analysis and identification were carried out.

[0039] During the product purification and analysis and identification process, 0.5mmol sodium fumarate was added to the liner as a calibration substance, and all the substances in the liner were transferred to a 15ml centrifuge tube with a dropper, and the inner and outer walls of the liner and the inner wall of the kettle were repeatedly rinsed with 5ml distilled water 5 times, and the rinse liquid was collected and transferred to the centrifuge tube. The substances in the centrifuge tube were mixed and divided into two centrifuge tubes A and B. Tube A was directly filtered, and 200μl of clear liquid and 400μl of heavy water were taken with a pipette and transferred to the nuclear magnetic tube. After adding sufficient NaOH to tube B, it was filtered, and 200μl of clear liquid and 400μl of heavy water were taken with a pipette and transferred to the nuclear magnetic tube. The products in the nuclear magnetic tube were analyzed by hydrogen nuclear magnetic spectrum. The hydrogen nuclear magnetic spectrum analysis showed that γ-valerolactone and terephthalic acid (salt) were the main products, with yields of 85.8% and 99.1%, respectively.

[0040] Example 2

[0041] A high-value conversion method for levulinic acid coupled with waste PET depolymerization provided in this embodiment comprises the following steps:

[0042] 0.1900g of levulinic acid, 0.0960g of PET, 0.0500g of 5% Pt / MCM-41, 0.1000g of terephthalic acid and 2ml of water were added to a 10ml polytetrafluoroethylene liner in sequence and placed in a high-pressure reactor. Nitrogen was charged and discharged into the reactor several times. After the air was removed, the reactor was vented and sealed. The reactor was placed on a heating plate with stirring and heated to 230°C. The reaction was carried out for 18h. After the reaction was completed, it was cooled to room temperature to complete the high-value conversion process of levulinic acid coupling depolymerization of waste PET, and subsequent product purification and analysis and identification were carried out.

[0043] During the product purification and analysis and identification process, add 0.5mmol sodium fumarate to the liner as a calibrant, use a dropper to transfer all the substances in the liner to a 15ml centrifuge tube, and rinse the inner and outer walls of the liner and the inner wall of the kettle repeatedly with 5ml of distilled water 5 times, and transfer the liquid to the centrifuge tube. Mix the substances in the centrifuge tube and divide them into two centrifuge tubes A and B. Filter tube A directly, and use a pipette to draw 200μl of clarified liquid and 400μl of heavy water, and transfer them to the NMR tube. Add enough NaOH to tube B and filter it, and use a pipette to draw 200μl of clarified liquid and 400μl of heavy water, and transfer them to the NMR tube. Perform NMR hydrogen spectrum analysis on the product in the NMR tube, such as Figure 1 and Figure 2 As shown, H NMR spectrum analysis showed that γ-valerolactone and terephthalic acid (salt) were the main products, with yields of 86.2% and 98.0%, respectively.

[0044] Example 3

[0045] A high-value conversion method for depolymerization of waste PET coupled with levulinic acid provided in this embodiment comprises the following steps:

[0046] 0.2900g of levulinic acid, 0.0960g of PET, 0.0500g of 5% Pt / MCM-41, 1ml of 1mol / LNaOH solution and 1ml of water were added to a 10ml polytetrafluoroethylene liner in sequence and placed in a high-pressure reactor. Nitrogen was charged and discharged into the reactor several times. After the air was removed, the reactor was deflated and sealed. The reactor was placed on a heating plate with stirring and heated to 230°C. The reaction was carried out for 18 hours. After the reaction was completed, it was cooled to room temperature to complete the high-value conversion process of levulinic acid coupling depolymerization of waste PET, and subsequent product purification and analysis and identification were carried out.

[0047] During the product purification and analysis and identification process, 0.5mmol sodium fumarate was added to the liner as a standard, and all the substances in the liner were transferred to a 15ml centrifuge tube with a dropper, and the inner and outer walls of the liner and the inner wall of the kettle were repeatedly rinsed with 5ml distilled water 5 times, and the rinse liquid was collected and transferred to the centrifuge tube. The substances in the centrifuge tube were mixed and divided into two centrifuge tubes A and B. Tube A was directly filtered, and 200μl of clear liquid and 400μl of heavy water were taken with a pipette and transferred to the nuclear magnetic tube. After adding sufficient NaOH to tube B, it was filtered, and 200μl of clear liquid and 400μl of heavy water were taken with a pipette and transferred to the nuclear magnetic tube. The products in the nuclear magnetic tube were analyzed by nuclear magnetic hydrogen spectrum. The hydrogen nuclear magnetic spectrum analysis showed that γ-valerolactone and terephthalic acid (salt) were the main products, with yields of 75.3 and 98.7%, respectively, and there was a large amount of by-product valeric acid, with a yield of 10.0%.

[0048] Example 4

[0049] A high-value conversion method for depolymerization of waste PET coupled with levulinic acid provided in this embodiment comprises the following steps:

[0050] 0.1900g of levulinic acid, 0.0960g of PET, 0.0500g of 5% Pt / MCM-41, 1ml of 1mol / LNaOH solution and 1ml of water were added to a 10ml polytetrafluoroethylene liner in sequence and placed in a high-pressure reactor. Nitrogen was charged and discharged into the reactor several times. After the air was removed, the reactor was deflated and sealed. The reactor was placed on a heating plate with stirring and heated to 230°C. The reaction was carried out for 24 hours. After the reaction was completed, it was cooled to room temperature to complete the high-value conversion process of levulinic acid coupling depolymerization of waste PET, and subsequent product purification and analysis and identification were carried out.

[0051] During the product purification and analysis and identification process, 0.5mmol sodium fumarate was added to the liner as a calibration substance, and all the substances in the liner were transferred to a 15ml centrifuge tube with a dropper, and the inner and outer walls of the liner and the inner wall of the kettle were repeatedly rinsed 5 times with 5ml distilled water, and the rinse liquid was collected and transferred to the centrifuge tube. The substances in the centrifuge tube were mixed and divided into two centrifuge tubes A and B. Tube A was directly filtered, and 200μl of clear liquid and 400μl of heavy water were drawn with a pipette and transferred to the nuclear magnetic tube. After adding enough NaOH to tube B, it was filtered, and 200μl of clear liquid and 400μl of heavy water were drawn with a pipette and transferred to the nuclear magnetic tube. The products in the nuclear magnetic tube were analyzed by hydrogen nuclear magnetic spectrum. The hydrogen nuclear magnetic spectrum analysis showed that γ-valerolactone and terephthalic acid (salt) were the main products, with yields of 87.0% and 99.0%, respectively, which was not much improved compared with the example yield.

[0052] Example 5

[0053] A high-value conversion method for depolymerization of waste PET coupled with levulinic acid provided in this embodiment comprises the following steps:

[0054] 0.1900g of levulinic acid, 0.0960g of PET, 0.0500g of 5% Pt / MCM-41, 1ml of 1mol / LNaOH solution and 1ml of water were added to a 10ml polytetrafluoroethylene liner in sequence and placed in a high-pressure reactor. Nitrogen was charged and discharged into the reactor several times. After the air was removed, the reactor was vented and sealed. The reactor was placed on a heating plate with stirring and heated to 230°C. The reaction was carried out for 6h. After the reaction was completed, it was cooled to room temperature to complete the high-value conversion process of levulinic acid coupling depolymerization of waste PET, and subsequent product purification and analysis and identification were carried out.

[0055] During the product purification and analysis and identification process, 0.5mmol sodium fumarate was added to the liner as a standard, and all the substances in the liner were transferred to a 15ml centrifuge tube with a dropper, and the inner and outer walls of the liner and the inner wall of the kettle were repeatedly rinsed with 5ml distilled water 5 times, and the rinse liquid was collected and transferred to the centrifuge tube. The substances in the centrifuge tube were mixed and divided into two centrifuge tubes A and B. Tube A was directly filtered, and 200μl of clear liquid and 400μl of heavy water were taken with a pipette and transferred to the nuclear magnetic tube. After adding sufficient NaOH to tube B, it was filtered, and 200μl of clear liquid and 400μl of heavy water were taken with a pipette and transferred to the nuclear magnetic tube. The products in the nuclear magnetic tube were analyzed by hydrogen nuclear magnetic spectrum. The hydrogen nuclear magnetic spectrum analysis showed that γ-valerolactone and terephthalic acid (salt) were the main products, with yields of 40.8% and 70.3%, respectively.

[0056] Example 6

[0057] A high-value conversion method for levulinic acid coupled with waste PET depolymerization provided in this embodiment comprises the following steps:

[0058] 0.1900g of levulinic acid, 0.0960g of PET, 0.0500g of 5% Pt / MCM-41, 1ml of 1mol / LNaOH solution and 1ml of water were added to a 10ml polytetrafluoroethylene liner in sequence and placed in a high-pressure reactor. Nitrogen was charged and discharged into the reactor several times. After the air was removed, the reactor was deflated and sealed. The reactor was placed on a heating plate with stirring and heated to 210°C. The reaction was carried out for 18 hours. After the reaction was completed, it was cooled to room temperature to complete the high-value conversion process of levulinic acid coupling depolymerization of waste PET, and subsequent product purification and analysis and identification were carried out.

[0059] During the product purification and analysis and identification process, 0.5mmol sodium fumarate was added to the liner as a calibration substance, and all the substances in the liner were transferred to a 15ml centrifuge tube with a dropper, and the inner and outer walls of the liner and the inner wall of the kettle were repeatedly rinsed with 5ml distilled water 5 times, and the rinse liquid was collected and transferred to the centrifuge tube. The substances in the centrifuge tube were mixed and divided into two centrifuge tubes A and B. Tube A was directly filtered, and 200μl of clear liquid and 400μl of heavy water were taken with a pipette and transferred to the nuclear magnetic tube. After adding enough NaOH to tube B, it was filtered, and 200μl of clear liquid and 400μl of heavy water were taken with a pipette and transferred to the nuclear magnetic tube. The products in the nuclear magnetic tube were analyzed by nuclear magnetic hydrogen spectrum. The hydrogen nuclear magnetic spectrum analysis showed that γ-valerolactone and terephthalic acid (salt) were the main products, with yields of 71.0% and 95.6%, respectively, indicating that the depolymerization of waste PET occurred faster than the hydrogenation of levulinic acid.

[0060] Example 7

[0061] A high-value conversion method for levulinic acid coupled with waste PET depolymerization provided in this embodiment comprises the following steps:

[0062] 0.1900g of levulinic acid, 0.0960g of PET, 0.0500g of 10% Pt / MCM-41, 1ml of 1mol / LNaOH solution and 1ml of water were added to a 10ml polytetrafluoroethylene liner in sequence and placed in a high-pressure reactor. Nitrogen was charged and discharged into the reactor several times. After the air was removed, the reactor was deflated and sealed. The reactor was placed on a heating plate and stirred and heated to 230°C. The reaction was carried out for 24 hours. After the reaction was completed, it was cooled to room temperature to complete the high-value conversion process of levulinic acid coupling depolymerization of waste PET, and subsequent product purification and analysis and identification were carried out.

[0063] During the product purification and analysis and identification process, 0.5mmol sodium fumarate was added to the liner as a calibration substance, and all the substances in the liner were transferred to a 15ml centrifuge tube with a dropper, and the inner and outer walls of the liner and the inner wall of the kettle were repeatedly rinsed with 5ml distilled water 5 times, and the rinse liquid was collected and transferred to the centrifuge tube. The substances in the centrifuge tube were mixed and divided into two centrifuge tubes A and B. Tube A was directly filtered, and 200μl of clear liquid and 400μl of heavy water were taken with a pipette and transferred to the nuclear magnetic tube. After adding sufficient NaOH to tube B, it was filtered, and 200μl of clear liquid and 400μl of heavy water were taken with a pipette and transferred to the nuclear magnetic tube. The products in the nuclear magnetic tube were analyzed by hydrogen nuclear magnetic spectrum. The hydrogen nuclear magnetic spectrum analysis showed that γ-valerolactone and terephthalic acid (salt) were the main products, with yields of 79.2% and 98.8%, respectively.

[0064] Ordinary technicians in the relevant technical field can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, all technical solutions obtained by equivalent replacement or equivalent transformation fall within the protection scope of the present invention.

Claims

1. A high-value conversion method for depolymerization of waste PET coupled with levulinic acid, characterized in that: Put polyethylene terephthalate, a catalyst, levulinic acid, a depolymerization aid and water in a closed reactor in an inert atmosphere, and carry out a depolymerization-hydrogenation reaction at 210° C. to 240° C. After the reaction is completed, separate the reaction product into solid and liquid, collect the liquid product and purify it to obtain γ-valerolactone and terephthalic acid; The depolymerization aid is one of sodium hydroxide and terephthalic acid; The catalyst is a noble metal-loaded molecular sieve catalyst formed by loading noble metal Pt on MCM-41 molecular sieve.

2. The high-value conversion method of levulinic acid coupled with waste PET depolymerization as claimed in claim 1, characterized in that: The inert atmosphere is a nitrogen atmosphere with an initial pressure of normal pressure.

3. The high-value conversion method of levulinic acid coupled with waste PET depolymerization as claimed in claim 1, characterized in that: The noble metal-loaded molecular sieve is obtained by sequentially drying and reducing calcining an impregnation solution formed by ultrasonically mixing MCM-41 molecular sieve and PtCl4 solution.

4. The high-value conversion method of levulinic acid coupled with waste PET depolymerization as claimed in claim 3, characterized in that: When preparing the noble metal-loaded molecular sieve, in the impregnation solution, the ratio of Pt in PtCl4 to the total mass of Pt and MCM-41 molecular sieve is 0.01 to 0.

1.

5. The high-value conversion method of levulinic acid coupled with waste PET depolymerization as claimed in claim 4, characterized in that: When preparing the noble metal-loaded molecular sieve, the ratio of Pt in PtCl4 to the total mass of Pt and MCM-41 molecular sieve in the impregnation solution is preferably 0.

05.

6. The high-value conversion method of levulinic acid coupled with waste PET depolymerization as claimed in claim 3, characterized in that: When preparing the noble metal-loaded molecular sieve, the drying temperature is 20-70°C.

7. The high-value conversion method of levulinic acid coupled with waste PET depolymerization as claimed in claim 3, characterized in that: When preparing the noble metal-loaded molecular sieve, the ultrasonic frequency used in the ultrasonic mixing is 10 to 90 kHz.

8. The high-value conversion method of levulinic acid coupled with waste PET depolymerization as claimed in claim 3, characterized in that: When preparing the noble metal-loaded molecular sieve, the atmosphere used in the reducing roasting is a hydrogen-argon mixed gas with a hydrogen volume percentage of 2% to 20%.

9. The high-value conversion method of levulinic acid coupled with waste PET depolymerization as claimed in claim 3, characterized in that: When preparing the noble metal-loaded molecular sieve, the reduction calcination temperature is 50 to 500° C. and the time is 4 to 8 hours.

10. The high-value conversion method of levulinic acid coupled with waste PET depolymerization as claimed in claim 3, characterized in that: The reaction time of the depolymerization-hydrogenation reaction is 6 to 24 hours.