A tin-lead mixed perovskite solar cell and its preparation method
The tin-lead mixed perovskite was solved by adding (S)-2-(2,5-dioxoxazolidine-4-yl)acetate additive to the precursor of the tin-lead mixed perovskite solar cell. The problem of low photoelectric conversion efficiency and poor stability caused by the instability of the precursor liquid of solar cells has achieved the effect of improving the photoelectric conversion efficiency and stability.
Patent Information
- Application Number
- CN202311331157.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-13
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-10-13
AI Technical Summary
Tin-lead mixed perovskite solar cells have low photoelectric conversion efficiency and poor stability due to instability in the precursor liquid, which hinders their wide application.
To the precursor solution of the tin-lead mixed perovskite active layer, (S)-2-(2,5-dioxoxazolidin-4-yl)acetate additive was added, and the tin-lead mixed mixture was prepared by one-step spin coating method. Perovskite active layer inhibits the oxidation of Sn2+ and regulates crystallization kinetics.
The defect state density of the active layer is effectively reduced, the photoelectric conversion efficiency and stability are improved, and a high-quality active layer film is formed.
Smart Images

Figure CN117580421B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solar cells, and in particular relates to a tin-lead mixed perovskite solar cell and a preparation method thereof. Background Art
[0002] As a new type of green energy generation technology, metal halide perovskite solar cells have attracted widespread attention due to their high photoelectric conversion efficiency, large-area processing by solution method, and the ability to be combined with silicon solar cells to prepare stacked solar cells. As a research hotspot in the field of solar power generation, the photoelectric conversion efficiency of perovskite solar cells has increased from the initial 3.8% to 25.7% in just over a decade, and their application prospects are broad.
[0003] Tin-lead hybrid perovskite solar cells have attracted great attention due to their advantages in reducing toxic lead and adjusting the optical band gap. On the one hand, using tin instead of lead can reduce the toxicity of perovskite cells; on the other hand, narrow bandgap perovskites can only be achieved by partially or completely replacing lead with tin. Tin-lead hybrid perovskites with a bandgap range of 1.1 to 1.4 eV are ideal candidate materials for single-junction solar cells close to the Shockley-Queisser limit. At the same time, tin-lead hybrid perovskites are also ideal materials for bottom cells of high-efficiency tandem perovskite solar cells due to their narrow band gap and ability to absorb sunlight in the long wavelength part. However, due to the Sn in the tin-lead hybrid perovskite precursor solution, the 2+ Very easily oxidized to Sn 4+ , the precursor solution is unstable, resulting in p-type doping in the formed tin-lead mixed perovskite photoactive layer, increasing the defect state density and reducing the photovoltaic performance of the device. At the same time, using part of tin to replace lead will speed up the crystallization rate of the perovskite active layer film, and the crystallization process is less controllable, affecting the film quality, resulting in low photoelectric conversion efficiency and poor stability of the prepared tin-lead mixed perovskite solar cells, which hinders the widespread application of tin-lead mixed perovskite solar cells. Summary of the invention
[0004] Therefore, the technical problem to be solved by the present invention is to overcome the above-mentioned defects in the prior art, thereby providing a tin-lead mixed perovskite solar cell and a preparation method thereof.
[0005] To this end, the present invention provides the following technical solutions:
[0006] The invention provides a tin-lead mixed perovskite solar cell, comprising a tin-lead mixed perovskite active layer. When preparing the tin-lead mixed perovskite active layer, a (S)-2-(2,5-dioxooxazolidin-4-yl) benzyl acetate additive is added to a precursor solution of the tin-lead mixed perovskite active layer.
[0007] Optionally, the tin-lead mixed perovskite solar cell includes a transparent conductive substrate layer, a hole transport layer, a tin-lead mixed perovskite active layer, an electron transport layer and a metal back electrode arranged in sequence.
[0008] The present invention provides a method for preparing the above-mentioned tin-lead mixed perovskite solar cell, comprising the following steps: sequentially preparing a hole transport layer, a tin-lead mixed perovskite active layer, an electron transport layer and a metal back electrode on the surface of a transparent conductive substrate layer;
[0009] The tin-lead mixed perovskite active layer is prepared by a one-step spin coating method, and the preparation steps include:
[0010] A tin-lead mixed perovskite precursor solution with (S)-2-(2,5-dioxoxazolidin-4-yl) benzyl acetate additive is deposited on the substrate on which the hole transport layer is prepared, the substrate is rotated, an anti-solvent is added dropwise, and annealing is performed to obtain the tin-lead mixed perovskite active layer.
[0011] Optionally, in the tin-lead mixed perovskite precursor solution containing the (S)-2-(2,5-dioxooxazolidin-4-yl)benzyl acetate additive, the solvent is selected from at least one of N,N-dimethylformamide (DMF) and dimethyl sulfoxide (DMSO).
[0012] Optionally, in the tin-lead mixed perovskite precursor solution containing the (S)-2-(2,5-dioxoxazolidin-4-yl)benzyl acetate additive, the concentration of the (S)-2-(2,5-dioxoxazolidin-4-yl)benzyl acetate additive is 1 mg / mL to 20 mg / mL.
[0013] Optionally, the temperature of the annealing step is 80° C. to 150° C., and the annealing time is 1 min to 30 min.
[0014] Optionally, the thickness of the tin-lead mixed perovskite active layer is 100 nm to 1000 nm.
[0015] Typically, but not limiting, the method for preparing the above-mentioned tin-lead mixed perovskite solar cell provided by the present invention comprises the following specific steps:
[0016] Step 1: The ITO glass substrate is cleaned by ultrasonic cleaning with deionized water, acetone, and isopropanol in sequence, and the solvent remaining on the glass substrate is blown dry with a nitrogen stream to obtain a clean transparent conductive substrate;
[0017] Step 2: Place the conductive substrate cleaned in step 1 on a UVO treatment machine, use a pipette to absorb the PEDOT:PSS solution, and evenly apply it on the surface of the substrate. Start the high-speed rotation of the coating machine. After the rotation stops, place the substrate on a hot stage and anneal in air to obtain a hole transport layer.
[0018] Step 3: Place the substrate in step 2 on a coater in a glove box, use a pipette to absorb the prepared tin-lead mixed perovskite precursor solution, evenly apply it on the surface of the substrate, start the coater to rotate at high speed, drip the anti-solvent and infiltrate the additive solution into the semi-crystalline perovskite film, and after the rotation stops, place it on a hot stage in an air environment for annealing to obtain a tin-lead mixed perovskite active layer;
[0019] Step 4: Place the substrate in step 3 on a coating machine in the glove box, use a pipette to absorb the prepared electron transport layer solution, evenly apply it on the surface of the substrate, start the coating machine to rotate at high speed, and after the rotation stops, the electron transport layer is obtained;
[0020] Step 5: Prepare a metal back electrode on the electron transport layer by thermal evaporation on the substrate in step 4.
[0021] Furthermore, the ultrasonic cleaning time using each solvent in step 1 is 15 minutes to 30 minutes.
[0022] Furthermore, in step 2, the rotation speed of the coating machine is 3000 rpm to 5000 rpm, the rotation time is 20s to 40s, the hot stage annealing temperature is 140° C. to 160° C., and the annealing time is 5min to 15min.
[0023] Furthermore, in step 3, the volume of the precursor solution sucked by the pipette is 20 μL to 100 μL, the rotation speed of the gelator is 2000 rpm to 5000 rpm, the rotation time is 20s to 60s, the volume of the anti-solvent sucked by the pipette is 100 μL to 3000 μL, the anti-solvent is added at any moment between 10 and 50s after the start of rotation, the hot stage annealing temperature is 80°C to 150°C, and the annealing time is 5min to 30min.
[0024] Furthermore, in step 3, the anti-solvent is one or more of chlorobenzene, ethyl ether, anisole, acetone, toluene, ethyl acetate and chloroform.
[0025] Furthermore, in step 4, the volume of the electron transport layer solution sucked by the pipette is 30 μL to 80 μL, the rotation speed of the gelator is 1000 rpm to 6000 rpm, and the rotation time is 20 s to 60 s.
[0026] Furthermore, during the evaporation in step 5, the pressure in the evaporation chamber is 9×10 -5 Pa, the thickness of the metal Ag electrode is 80nm~120nm.
[0027] The technical solution of the present invention has the following advantages:
[0028] The tin-lead mixed perovskite solar cell provided by the present invention comprises a tin-lead mixed perovskite active layer, wherein when preparing the tin-lead mixed perovskite active layer, a (S)-2-(2,5-dioxoxazolidin-4-yl) benzyl acetate additive is added to the tin-lead mixed perovskite precursor solution, wherein the additive molecule contains a plurality of lactone functional groups with a strong reducing effect, and can effectively inhibit the reduction of Sn in the tin-lead mixed perovskite precursor solution. 2+ Oxidized to Sn 4+ , reducing the formation of Sn(Ⅳ) vacancies in the active layer and reducing the defect state density. At the same time, the interaction between the additive molecules and the perovskite molecules can also regulate the crystallization kinetics, slow down the crystallization rate, and ultimately form a high-quality active layer film, improving the photoelectric conversion efficiency and stability of the tin-lead mixed perovskite solar cell.
[0029] In addition, the preparation method provided by the present invention has simple process, mild conditions, easy control, and broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0031] Figure 1 It is a schematic diagram of the structure of the tin-lead mixed perovskite solar cell provided by the present invention;
[0032] Figure 2 is a JV curve diagram of the tin-lead mixed perovskite solar cell provided by the embodiments of the present invention and the comparative examples;
[0033] Figure 3 It is a graph showing the relationship between the normalized energy conversion efficiency of the tin-lead mixed perovskite solar cell provided in the embodiments of the present invention and the comparative examples and the change over time.
[0034] Reference numerals:
[0035] 1. Transparent conductive substrate layer; 2. Hole transport layer; 3. Tin-lead mixed perovskite active layer; 4. Electron transport layer; 5. Metal back electrode. DETAILED DESCRIPTION
[0036] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0037] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0038] The present invention provides a tin-lead mixed perovskite solar cell, the structural schematic diagram of which is as follows Figure 1 As shown, it includes a transparent conductive substrate layer 1, a hole transport layer 2, a tin-lead mixed perovskite active layer 3, an electron transport layer 4 and a metal back electrode 5 which are arranged in sequence.
[0039] In particular, when preparing the tin-lead mixed perovskite active layer, (S)-2-(2,5-dioxooxazolidin-4-yl)benzyl acetate additive is added to the tin-lead mixed perovskite precursor solution.
[0040] The method for preparing a tin-lead mixed perovskite solar cell provided by the present invention comprises the following steps:
[0041] A hole transport layer, a tin-lead mixed perovskite active layer, an electron transport layer and a metal back electrode are sequentially formed on the surface of a transparent conductive substrate to obtain a tin-lead mixed perovskite solar cell.
[0042] In the present invention, the transparent conductive substrate is preferably ITO glass, FTO glass, AZO glass or conductive PET, more preferably ITO glass. The present invention has no special restrictions on the source of the transparent conductive substrate, and commercially available products known to those skilled in the art can be used. In the present invention, the transparent conductive substrate is preferably washed with deionized water, acetone, and isopropanol for 15 to 30 minutes each before use, and blown dry with a nitrogen gun.
[0043] In the present invention, the hole transport layer is preferably PEDOT:PSS, PTAA, MnO x , WO x , 2PACz or 4PACz layer, more preferably a PEDOT:PSS layer; the thickness of the hole transport layer is preferably 10nm to 200nm, more preferably 20nm to 100nm. The present invention has no special restrictions on the method for forming the hole transport layer on the perovskite active layer, and a preparation method of the hole transport layer well known to those skilled in the art can be used.
[0044] In the present invention, the tin-lead mixed perovskite precursor solution film preferably has an ABX3 type crystal structure, wherein A is an organic cation and / or an inorganic cation, B is a positive divalent metal ion, and X is one or more of I, Br and Cl. In the present invention, the organic cation and / or inorganic cation is preferably one or more of Cs, FA, MA, and the positive divalent metal ion is preferably Pb 2+and Sn 2+ , X is preferably one or more of I and Br. More preferably, in the present invention, the perovskite precursor solution film crystal structure is Cs 0.25 FA 0.75 Pb 0.5 Sn 0.5 I3. The solvent of the perovskite precursor solution is preferably one or more of DMF and DMSO. More preferably, the solvent of the perovskite precursor solution is a mixed solvent of DMF and DMSO, and the volume ratio of DMF:DMSO=3:1. The concentration of the perovskite precursor solution is preferably 1 mg / mL to 2 mg / mL. More preferably, the concentration of the perovskite precursor solution is 1.8 mg / mL. On this basis, a perovskite precursor solution that is well known to those skilled in the art and capable of forming a thin film of the perovskite precursor solution can be used, and those skilled in the art have no special restrictions on the preparation method of the perovskite precursor solution.
[0045] In the present invention, in the tin-lead mixed perovskite precursor solution containing the (S)-2-(2,5-dioxoxazolidin-4-yl)benzyl acetate additive, the solvent is preferably at least one of N,N-dimethylformamide (DMF) and dimethyl sulfoxide (DMSO), and the concentration of the (S)-2-(2,5-dioxoxazolidin-4-yl)benzyl acetate additive is preferably 1 mg / mL to 20 mg / mL, and more preferably, the concentration of the additive is 5 mg / mL to 15 mg / mL.
[0046] In the present invention, the anti-solvent used in the preparation process of the perovskite active layer is preferably one or more selected from anisole, chlorobenzene, ethyl ether, acetone, toluene, ethyl acetate and chloroform, more preferably chlorobenzene or anisole.
[0047] In the present invention, the preparation method of the perovskite active layer is preferably a one-step spin coating method, and the preparation process is preferably as follows: placing a substrate (2cm×2cm) on a coater in a glove box, using a pipette to absorb 20μL~100μL of the prepared perovskite precursor solution, evenly coating it on the surface of the substrate, starting the coater to rotate at high speed, the rotation speed is 2000rpm~5000rpm, the rotation time is 20~60s, and 100μL~3000μL of anti-solvent is added at any moment between 10s and 50s after the start of rotation. After the rotation stops, it is placed on a hot stage in an air environment for annealing, the annealing temperature is 80℃~150℃, the annealing time is 5min~30min, and the air humidity is 20%~50%. After annealing, a tin-lead mixed perovskite active layer is obtained.
[0048] More preferably:
[0049] After UVO treatment of the substrate for 15 minutes, place it on a coater in a glove box, use a pipette to absorb 30μL~60μL of the prepared perovskite active layer precursor solution, evenly apply it on the surface of the substrate, start the coater to rotate at high speed, the rotation speed is 3000rpm~5000rpm, the rotation time is 30~60s, 100μL~500μL of anti-solvent is added 25~40s after the start of rotation, after the rotation stops, place it on a hot stage in an air environment for annealing, the annealing temperature is 100℃~150℃, the annealing time is 10min~30min, the air humidity is 30%~40%, and the perovskite active layer is obtained after annealing.
[0050] In the present invention, the thickness of the perovskite active layer is preferably 100 nm to 2000 nm, more preferably 300 nm to 1000 nm.
[0051] In the present invention, the electron transport layer is preferably SnO2, TiO x 、NiO x , CuO x , CuSCN, CuPc or C 60 and its derivatives (PC 61 BM, PC 71 BM, etc.), more preferably PC 61 BM. The thickness of the electron transport layer is preferably 10 nm to 200 nm, more preferably 20 nm to 100 nm. The present invention has no particular limitation on the method for forming the electron transport layer on the conductive substrate, and the preparation method of the electron transport layer well known to those skilled in the art can be used.
[0052] The present invention has no special restrictions on the type and formation method of the metal back electrode, and a technical solution for forming a metal back electrode on a hole transport layer well known to those skilled in the art can be used. In a preferred embodiment of the present invention, the substrate is transferred to a thermal evaporation device, and the vacuum degree reaches 1×10 -5 Pa, the electrode (Ag) is evaporated to a thickness of 100 nm; after the evaporation is completed, the perovskite solar cell is obtained.
[0053] The present invention provides a method for preparing a tin-lead mixed perovskite solar cell, comprising the following steps: forming a hole transport layer, a tin-lead mixed perovskite active layer, an electron transport layer and a metal back electrode in sequence on the surface of a transparent conductive substrate to obtain a tin-lead mixed perovskite solar cell. Compared with the prior art, the preparation method provided by the present invention adds (S)-2-(2,5-dioxoxazolidin-4-yl) benzyl acetate additive to the tin-lead mixed perovskite precursor solution during the preparation of the perovskite active layer. The present invention has the following beneficial technical effects: the additive molecule contains multiple lactone functional groups with strong reducing effects, which can effectively inhibit the Sn in the tin-lead mixed perovskite precursor solution.2+ Oxidized to Sn 4+ , reducing the formation of Sn(Ⅳ) vacancies in the active layer and reducing the defect state density. At the same time, the interaction between the additive molecules and the perovskite molecules can also regulate the crystallization dynamics, slow down the crystallization rate, and ultimately form a high-quality active layer film, improving the photoelectric conversion efficiency and stability of the tin-lead mixed perovskite solar cell.
[0054] In addition, the preparation method provided by the present invention has simple process, mild conditions, easy control, and broad application prospects.
[0055] In order to further illustrate the present invention, the following examples are provided for detailed description.
[0056] Example 1
[0057] This embodiment provides a tin-lead mixed perovskite solar cell, the composition and specific preparation method of which are as follows:
[0058] Step 1: Place ITO transparent conductive glass (2 cm×2 cm) in deionized water, acetone, and isopropanol and ultrasonically clean for 15 min each twice, blow dry with nitrogen, and store for later use.
[0059] Step 2: Place the ITO substrate in a UV ozone cleaner for 15 minutes and then place the substrate on a coater; take 100 μL of PEDOT:PSS solution and spread it evenly on the surface of the ITO conductive glass, start the coater to rotate at high speed, and set the coater parameters to 4000 rpm and 30 seconds; then place it on a 150°C hot plate in an air environment for annealing for 10 minutes to obtain a PEDOT:PSS film.
[0060] Step 3: Place the substrate on the coating machine in the glove box and use a pipette to draw 60 μL of the prepared tin-lead mixed perovskite precursor solution (the perovskite formula is: Cs 0.25 FA 0.75 Pb 0.5 Sn 0.5 I3, the concentration of the precursor solution is 1.8 mol / L, and the amount of (S)-2-(2,5-dioxooxazolidin-4-yl) benzyl acetate additive dissolved in each 1 mL of tin-lead mixed perovskite precursor solution is 10 mg), and it is evenly coated on the surface of the substrate. The high-speed rotation of the coating machine is started, the rotation speed is 4000 rpm, and the rotation time is 30 s. 200 μL of anisole anti-solvent is added at 25 s after the rotation starts. After the rotation stops, it is placed on a hot stage for annealing in an air environment. The annealing temperature is 100 ° C, the annealing time is 10 min, and the air humidity is 40%. After the annealing is completed, a tin-lead mixed perovskite active layer is obtained.
[0061] Step 4: Place the substrate on the gel coater in the glove box and use a pipette to draw 60 μL of the prepared PC61 BM solution (the solvent is chlorobenzene, the concentration is 20 mg / mL) is evenly applied on the surface of the substrate, and the high-speed rotation of the coating machine is started, the rotation speed is 1000 rpm, and the rotation time is 30 s. Then, 60 μL of the prepared BCP solution (the solvent is isopropanol, the concentration is 5 mg / mL) is taken with a pipette, and evenly applied on the surface of the substrate, and the high-speed rotation of the coating machine is started, the rotation speed is 5000 rpm, and the rotation time is 30 s to obtain the electron transport layer.
[0062] Step 5: Finally, use high vacuum evaporation equipment to evaporate, and the pressure in the evaporation chamber is 9×10 -5 Pa, evaporate a 100nm thick metal Ag electrode to obtain a perovskite solar cell device.
[0063] Example 2
[0064] This embodiment provides a tin-lead hybrid perovskite solar cell. Compared with Embodiment 1, the difference is that the concentration of the additive (S)-2-(2,5-dioxooxazolidin-4-yl)benzyl acetate in step 3 is 5 mg / mL.
[0065] Example 3
[0066] This embodiment provides a tin-lead hybrid perovskite solar cell. Compared with Embodiment 1, the difference is that the concentration of the additive (S)-2-(2,5-dioxooxazolidin-4-yl)benzyl acetate in step 3 is 15 mg / mL.
[0067] Comparative Example
[0068] This comparative example provides a tin-lead mixed perovskite solar cell, which is different from Examples 1-3 in that when preparing the perovskite active layer in step 3, the additive material is not added to the precursor solution.
[0069] Test Case
[0070] The performance of the perovskite solar cells provided in the embodiments of the present invention and the comparative examples was tested, and the specific testing method was as follows:
[0071] The current density voltage (JV) curves of the perovskite solar cells prepared in the PCE test examples and comparative examples were completed on a Kethley 2400 system under the following test conditions: the simulated light intensity was 100 mW cm -2 (AM 1.5G) scan rate 0.1V s -1 (step size is 0.02 V, time delay is 200 ms), the scanning interval is 1.2 V to -0.2 V, and the power output of the xenon lamp is calibrated by the KG5 standard Si battery of NERL (National Renewable Energy Laboratory) standard.
[0072] The stability test was carried out on unpackaged perovskite solar cell devices in a nitrogen glove box at room temperature.
[0073] The specific test results are shown in the table below:
[0074] Table 1
[0075]
[0076] From the examples and comparative examples Figure 2 , Figure 3 It can be seen from the data in Table 1 that when preparing the tin-lead mixed perovskite active layer, the present invention adds (S)-2-(2,5-dioxoxazolidin-4-yl) benzyl acetate additive to the tin-lead mixed perovskite active layer precursor solution (Example 1-3), and the prepared tin-lead mixed perovskite solar cell device is compared with the device (Comparative Example 1) to which the additive is not added during preparation, and the photoelectric characteristics such as open circuit voltage, short circuit current density, and fill factor are all improved. The perovskite solar cell device prepared by the method of the present invention has the advantages of high photoelectric conversion efficiency and strong stability.
[0077] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.
Claims
1. A tin-lead mixed perovskite solar cell, It is characterized in that The invention comprises a tin-lead mixed perovskite active layer. When preparing the tin-lead mixed perovskite active layer, a (S)-2-(2,5-dioxoxazolidin-4-yl) benzyl acetate additive is added to a precursor solution of the tin-lead mixed perovskite active layer.
2. The tin-lead hybrid perovskite solar cell according to claim 1, It is characterized in that It includes a transparent conductive substrate layer, a hole transport layer, a tin-lead mixed perovskite active layer, an electron transport layer and a metal back electrode which are arranged in sequence.
3. A method for preparing the tin-lead mixed perovskite solar cell according to claim 2, It is characterized in that The method comprises the following steps: sequentially preparing a hole transport layer, a tin-lead mixed perovskite active layer, an electron transport layer and a metal back electrode on the surface of a transparent conductive substrate layer; The tin-lead mixed perovskite active layer is prepared by a one-step spin coating method, and the preparation steps include: A tin-lead mixed perovskite precursor solution with (S)-2-(2,5-dioxoxazolidin-4-yl) benzyl acetate additive is deposited on the substrate on which the hole transport layer is prepared, the substrate is rotated, an anti-solvent is added dropwise, and annealing is performed to obtain the tin-lead mixed perovskite active layer.
4. The method for preparing a tin-lead mixed perovskite solar cell according to claim 3, It is characterized in that In the tin-lead mixed perovskite precursor solution containing (S)-2-(2,5-dioxoxazolidin-4-yl) benzyl acetate additive, the solvent is selected from at least one of N,N-dimethylformamide and dimethyl sulfoxide.
5. The method for preparing a tin-lead mixed perovskite solar cell according to claim 3, It is characterized in that In the tin-lead mixed perovskite precursor solution containing the (S)-2-(2,5-dioxoxazolidin-4-yl) benzyl acetate additive, the concentration of the (S)-2-(2,5-dioxoxazolidin-4-yl) benzyl acetate additive is 1 mg / mL to 20 mg / mL.
6. The method for preparing a tin-lead mixed perovskite solar cell according to claim 3, It is characterized in that The temperature of the annealing step is 80° C. to 150° C., and the annealing time is 1 min to 30 min.