Resistive touchscreen, its fabrication method, and touch device
By employing a single-layer transparent conductive layer structure in the resistive screen, and utilizing silver nanowire arrays and silver nanoparticles to form a conductive path, the problems of complex processes and material waste in traditional resistive screens are solved, achieving simpler fabrication and lower costs.
Patent Information
- Application Number
- CN202311414237.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-27
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-10-27
AI Technical Summary
Traditional resistive touchscreen structures require two layers of transparent conductive electrodes and a transparent particle layer, which leads to complex processes and material waste, hindering their commercial development.
It adopts a single-layer transparent conductive layer structure, and utilizes silver nanowire arrays and silver nanoparticles to form a conductive path by pressing, thereby realizing touch function and simplifying the overall structure and control logic.
This reduces material and process costs, simplifies the manufacturing process, and enhances the commercial potential of resistive touchscreens.
Smart Images

Figure CN117590969B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of touch technology, and in particular to resistive touchscreens, their manufacturing methods, and touch devices. Background Technology
[0002] The common structure of a traditional resistive touchscreen includes a rigid transparent substrate, a first layer of transparent conductive electrodes, a transparent particle layer, a second layer of transparent conductive electrodes, and a flexible film, stacked sequentially. In use, pressing the flexible film brings the first and second layers of transparent conductive electrodes into contact, and an algorithm determines the position coordinates, thus enabling touch functionality. However, the common structure of traditional resistive touchscreens requires two layers of transparent conductive electrodes and the insertion of transparent particles in between for barrier purposes, leading to complex manufacturing processes and wasted raw materials, hindering the commercialization of resistive touchscreens. Summary of the Invention
[0003] Therefore, it is necessary to provide a resistive touchscreen, its preparation method, and a touch device to address the above problems. The resistive touchscreen is a single-layer transparent conductive layer, which simplifies the overall structure and control logic, makes it easier to prepare, and helps reduce material and process costs.
[0004] A resistive touchscreen includes a transparent substrate, a transparent conductive layer, and a flexible film stacked sequentially. The transparent conductive layer includes multiple electrodes and silver nanowire arrays connecting adjacent electrodes. The width of the silver nanowire arrays increases sequentially. Each silver nanowire array includes multiple parallel silver nanowire bundles. The angle between the silver nanowire bundles and the electrodes is greater than 0° and less than 90°. Each silver nanowire bundle can form a conductive path under pressure.
[0005] In one embodiment, the angle between the silver nanowire bundle and the edge of the transparent substrate is 30°-60°.
[0006] In one embodiment, the transparent conductive layer satisfies at least one of the following conditions:
[0007] (1) The width of the silver nanowire array increases sequentially;
[0008] (2) The difference in width of the silver nanowire array is 0.01mm-0.012mm;
[0009] (3) The minimum width of the silver nanowire array is 0.2mm-0.4mm;
[0010] (4) In each of the silver nanowire arrays, the spacing between two adjacent silver nanowire bundles is 0.5 mm to 0.8 mm;
[0011] (5) The width of each electrode is 0.5mm-0.8mm;
[0012] (6) At least some of the silver nanowire bundles in two adjacent silver nanowire arrays are on the same straight line.
[0013] In one embodiment, the widths of the silver nanowire arrays are equal.
[0014] In one embodiment, in each of the silver nanowire arrays, the spacing between two adjacent silver nanowire bundles is equal.
[0015] In one embodiment, each of the electrodes has an equal width.
[0016] In one embodiment, the electrode is selected from silver nanowire electrodes.
[0017] In the resistive touchscreen described in this invention, on the one hand, the silver nanowire bundles have breakpoints and silver nanoparticles distributed near the breakpoints, allowing the single-layer transparent conductive layer of the resistive touchscreen to replace the double-layer transparent conductive electrodes and transparent particle layer in the traditional resistive touchscreen structure. By pressing, the silver nanoparticles enter the breakpoints, thereby forming a conductive path in the silver nanowire bundles, thus realizing the touch function. On the other hand, the design of a silver nanowire array structure with progressively increasing horizontal widths allows the silver nanowire bundles to have different resistance distributions in the horizontal direction. At the same time, since each silver nanowire bundle has different breakpoints, the conductivity of the silver nanoparticles allows the silver nanowire bundles to form different resistance distributions in the vertical direction due to the different lengths of the conductive silver nanowire bundles. Thus, the different output resistances at different positions when the circuit is activated after pressing can be used to determine the touch position point, thereby constructing a new logic network for resistance-touch position feedback, making the overall structure and control logic simpler.
[0018] A method for fabricating a resistive touchscreen as described above includes the following steps:
[0019] Multiple silver nanowire arrays with progressively increasing widths and spaced apart are prepared on the surface of a transparent substrate. Each silver nanowire array includes multiple parallel silver nanowire bundles. The angle between the silver nanowire bundles and the arrangement direction of the silver nanowire array is greater than 0° and less than 90°.
[0020] Electrode plates are placed at opposite ends of each silver nanowire array so that both ends of the silver nanowire bundle are in contact with the electrode plates. The silver nanowire bundle in each silver nanowire array is disconnected by energizing.
[0021] Remove the electrode sheet and prepare an electrode at the original position of the electrode sheet, so that both ends of the silver nanowire bundle in each silver nanowire array are in contact with the electrode;
[0022] A flexible film is deposited on the surface of the silver nanowire array, and the flexible film is parallel to the transparent substrate to obtain a resistive screen.
[0023] In one embodiment, prior to the power-on process, the minimum resistance of each of the silver nanowire bundles is 100Ω-120Ω;
[0024] And / or, the voltage of the power-on process is 36V-43V.
[0025] A touch device, including a resistive screen as described above.
[0026] The preparation method described in this invention, by designing inclined silver nanowire bundles, generates tensile stress perpendicular to the direction of the silver nanowire bundles during the electrification process, due to the electron wind force along the direction of the silver nanowire bundles and the electric field force along the horizontal direction. This drives the silver nanowire bundles to migrate, resulting in the formation of breakpoints in the silver nanowire bundles. Silver nanoparticles are generated at the breakpoints, forming a single-layer transparent conductive layer that can generate a resistance signal by pressing. This method is not only easy to prepare, but also helps to reduce material and process costs, promoting the further application of resistive touch screens in touch devices. Attached Figure Description
[0027] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0028] Figure 1 This is a schematic diagram of the transparent conductive layer in the resistive screen described in this invention;
[0029] Figure 2 This is a schematic diagram illustrating the principle of breaking the circuit of the silver nanowire bundle through energization in this invention.
[0030] Among them, 101 is the silver nanowire array; 1011 is the silver nanowire bundle; 1012 is the silver nanoparticle; 201 is the electrode; F1 is the electron wind; E is the electric field force; and F2 is the tensile stress. Detailed Implementation
[0031] To facilitate understanding of the present invention, it will be described in more detail below. However, it should be understood that the present invention can be implemented in many different forms and is not limited to the embodiments or examples described herein. Rather, these embodiments or examples are provided to make the disclosure of the present invention more thorough and complete.
[0032] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments or examples only and is not intended to be limiting of the invention.
[0033] Combination Figure 1 As shown, the present invention provides a resistive touch screen, comprising a transparent substrate, a transparent conductive layer, and a flexible film stacked sequentially. The transparent conductive layer includes a plurality of electrodes 201 and silver nanowire arrays 101 connecting adjacent electrodes 201. The width of the silver nanowire arrays 101 increases sequentially. Each silver nanowire array 101 includes a plurality of parallel silver nanowire bundles 1011. The angle between the silver nanowire bundles 1011 and the electrodes 201 is greater than 0° and less than 90°. Each silver nanowire bundle 1011 can form a conductive path under pressure.
[0034] In the resistive touchscreen of this invention, on the one hand, the silver nanowire bundle 1011 has a breakpoint and silver nanoparticles 1012 distributed near the breakpoint, allowing the single-layer transparent conductive layer of the resistive touchscreen to replace the double-layer transparent conductive electrode and transparent particle layer in the traditional resistive touchscreen structure. By pressing, the silver nanoparticles 1012 enter the breakpoint, thereby forming a conductive path in the silver nanowire bundle 1011, thus realizing the touch function. On the other hand, the design of the silver nanowire array 101 structure with progressively increasing horizontal width allows the silver nanowire bundle 1011 to have different resistance distributions in the horizontal direction. At the same time, since each silver nanowire bundle 1011 has different breakpoints, through the conductive effect of the silver nanoparticles 1012, the silver nanowire bundle 1011 forms different resistance distributions in the vertical direction due to the different lengths of the conductive silver nanowire bundle 1011. Thus, the different output resistances at different positions when the circuit is activated after pressing can be used to determine the touch position point, thereby constructing a new logic network for resistance-touch position feedback, making the overall structure and control logic simpler.
[0035] It should be noted that the present invention does not limit the number of silver nanowire arrays 101 and silver nanowire bundles 1011; depending on the needs of different touch products, silver nanowire bundles 1011 that can form conductive paths under different pressure conditions can also be provided.
[0036] Preferably, the angle between the silver nanowire bundle 1011 and the electrode is 30°-60°, which is more conducive to improving the accuracy of the resistance-touch position feedback in the resistive screen.
[0037] Preferably, the width difference of the silver nanowire array 101 is 0.01mm-0.012mm, which is beneficial for accurately controlling the different resistances of the laterally distributed silver nanowire bundles 1011, thereby further improving the accuracy of the resistance-touch position feedback in the resistive screen.
[0038] It should be noted that the difference in width of the silver nanowire array 101 can be the same or different, and the present invention does not impose any restrictions on this.
[0039] Further preferably, the silver nanowire array 101 has the same width difference, which is more conducive to improving the accuracy of the resistance-touch position feedback in the resistive screen.
[0040] Preferably, the minimum width of the silver nanowire array 101 is 0.2 mm to 0.4 mm.
[0041] Preferably, in each of the silver nanowire arrays 101, the spacing between two adjacent silver nanowire bundles 1011 is 0.5 mm to 0.8 mm.
[0042] It should be noted that in each of the silver nanowire arrays 101, the spacing between two adjacent silver nanowire bundles 1011 can be the same or different, and the present invention does not impose any restrictions on this.
[0043] Further preferably, in each of the silver nanowire arrays 101, the spacing between two adjacent silver nanowire bundles 1011 is equal, which is more conducive to improving the accuracy of the resistance-touch position feedback in the resistive screen.
[0044] In one embodiment, at least some silver nanowire bundles 1011 in two adjacent silver nanowire arrays 101 are on the same straight line. It should be noted that by ensuring that both ends of the silver nanowire bundles 1011 in each silver nanowire array 101 are in contact with the electrode 201 and have a certain included angle, a new logic network for resistance-touch position feedback can be constructed. The present invention does not limit the positional relationship of the silver nanowire bundles 1011 in adjacent silver nanowire arrays 101. Figure 1 This is only a preferred embodiment and does not imply that the silver nanowire bundles 1011 in two adjacent silver nanowire arrays 101 must be on the same straight line.
[0045] Preferably, the width of each electrode 201 is 0.5mm-0.8mm.
[0046] It should be noted that the width of each electrode 201 may be the same or different, and the present invention does not limit this.
[0047] Further preferably, the width of each of the electrodes 201 is equal.
[0048] Optionally, the electrode 201 includes, but is not limited to, a silver nanowire electrode, preferably a silver nanowire electrode.
[0049] Optionally, the transparent substrate includes, but is not limited to, a glass substrate, preferably a glass substrate.
[0050] Optionally, the flexible film includes, but is not limited to, polyethylene terephthalate (PET) film, preferably PET film. It should be noted that the flexible films described in this art all have excellent light transmittance.
[0051] Therefore, the resistive touchscreen of the present invention is a single-layer transparent conductive layer, which overcomes the drawbacks of traditional touch structures that require the construction of a double-layer transparent conductive electrode and a transparent particle layer. This makes the overall structure and control logic simpler, easier to manufacture, and also helps to reduce material and process costs, thus promoting the further application of resistive touchscreens.
[0052] It should be noted that the present invention does not limit the specific shape of the resistive screen, including but not limited to rectangles, circles or polygons, and those skilled in the art can design it according to the actual use scenario.
[0053] This invention also provides a method for preparing a resistive touchscreen, comprising the following steps:
[0054] S1, a plurality of silver nanowire arrays 101 with progressively increasing widths and spaced apart are prepared on the surface of a transparent substrate. Each of the silver nanowire arrays 101 includes a plurality of parallel silver nanowire bundles 1011. The angle between the silver nanowire bundles 1011 and the arrangement direction of the silver nanowire array 101 is greater than 0° and less than 90°.
[0055] S2, place electrode plates at opposite ends of each of the silver nanowire arrays 101, so that both ends of the silver nanowire bundles 1011 are in contact with the electrode plates, and then disconnect the silver nanowire bundles 1011 in each of the silver nanowire arrays 101 by applying an electric current.
[0056] S3, remove the electrode sheet and prepare an electrode 201 at the original position of the electrode sheet, so that both ends of the silver nanowire bundle 1011 in each silver nanowire array 101 are in contact with the electrode 201.
[0057] S4, a flexible film is disposed on the surface of the silver nanowire array 101, and the flexible film is parallel to the transparent substrate to obtain a resistive screen.
[0058] In step S1, the preparation method of the silver nanowire array 101 includes, but is not limited to, coating processes, preferably coating processes, wherein the coating process specifically includes electrohydraulic printing or inkjet printing.
[0059] It should be noted that the silver nanowire bundles 1011 in the silver nanowire array 101 are obtained by multiple silver nanowires arranged closely in the same direction. The method of preparing the silver nanowires is not limited in this invention.
[0060] By preparing and controlling the minimum resistance of each silver nanowire bundle 1011 to be 100Ω-120Ω, it is beneficial to coordinately adjust the input voltage during the power-on process, thereby enabling the silver nanowire bundle 1011 to achieve tensile stress failure during the power-on process.
[0061] Preferably, the angle between the silver nanowire bundle 1011 and the silver nanowire array 101 is 30°-60°, which is more conducive to improving the accuracy of the resistance-touch position feedback in the resistive screen.
[0062] Preferably, the difference in width of the silver nanowire array 101 is 0.01mm-0.012mm, which is beneficial for precisely controlling the different resistances of the laterally distributed silver nanowire bundles 1011, thereby further improving the accuracy of the resistance-touch position feedback in the resistive screen.
[0063] Further preferably, the widths of the silver nanowire array 101 are equal.
[0064] Preferably, the minimum width of the silver nanowire array 101 is 0.2 mm to 0.4 mm.
[0065] Preferably, in each of the silver nanowire arrays 101, the spacing between two adjacent silver nanowire bundles 1011 is 0.5mm-0.8mm. More preferably, the spacing between two adjacent silver nanowire bundles 1011 is equal, which is more conducive to improving the accuracy of the resistance-touch position feedback in the resistive screen.
[0066] Preferably, the spacing between two adjacent silver nanowire arrays 101 is 0.5 mm to 0.8 mm, and more preferably, the spacing between two adjacent silver nanowire arrays 101 is equal.
[0067] Preferably, at least a portion of the silver nanowire bundles 1011 in two adjacent silver nanowire arrays 101 are on the same straight line.
[0068] In one embodiment, the transparent substrate includes, but is not limited to, a glass substrate, preferably a glass substrate.
[0069] In step S2, combined Figure 2As shown, by designing an inclined silver nanowire bundle 1011, during the energization process, due to the electron wind force F1 along the direction of the silver nanowire bundle 1011 and the electric field force E along the horizontal direction, a tensile stress F2 perpendicular to the direction of the silver nanowire bundle 1011 is generated in the silver nanowire bundle 1011, driving the silver nanowire bundle 1011 to migrate, resulting in the formation of a break in the silver nanowire bundle 1011, and silver nanoparticles 1012 are generated at the break, forming a single-layer transparent conductive layer that can form a resistance signal by pressing. This is not only easy to prepare, but also helps to reduce material and process costs.
[0070] In one embodiment, the voltage of the power-on process is 36V-43V.
[0071] Preferably, the electrode sheet has a thickness of 0.5 mm to 0.8 mm, and the thickness of the electrode sheet is less than or equal to the spacing between two adjacent silver nanowire arrays 101.
[0072] Specifically, the electrode sheet is selected from silver electrode sheets or copper electrode sheets.
[0073] In step S3, by preparing electrode 201, both ends of the silver nanowire bundle 1011 are in contact with electrode 201, thereby constructing a complete single-layer transparent conductive layer.
[0074] Preferably, the width of each electrode 201 is 0.5mm-0.8mm. Since the width of the electrode 201 is equal to the spacing between two adjacent silver nanowire arrays 101, when the spacing between two adjacent silver nanowire arrays 101 is preferably equal, the width of each electrode 201 is also preferably equal.
[0075] In step S4, the flexible film can be bonded to the surface of the silver nanowire array 101 by insulating tape, or it can be disposed on the surface of the silver nanowire array 101 by other means. The present invention does not limit this.
[0076] The flexible film is made of materials including but not limited to polyethylene terephthalate (PET), and preferably PET film.
[0077] The present invention also provides a touch device, including the resistive screen. It will be understood that the touch device further includes electrical connectors and a control module.
[0078] The resistive screen, its manufacturing method, and the touch device will be further described below through specific embodiments.
[0079] Example 1
[0080] The glass substrate and two electrodes were cleaned with acetone and ethanol for 15 minutes under ultrasonic conditions, respectively, and then allowed to air dry. The selected electrode thickness was 0.5 mm. A silver nanowire array was fabricated on the cleaned glass substrate surface using inkjet printing. During coating, the width of the first silver nanowire array was controlled to be 0.2 mm, the angle between all parallel silver nanowire bundles in the first array and the edge of the glass substrate was 30°, the spacing between all adjacent parallel silver nanowire bundles was 0.5 mm, and the resistance of all silver nanowire bundles was controlled to be approximately 100 Ω. Following the arrangement direction of all silver nanowire bundles in the first array, subsequent silver nanowire arrays were designed with a width increase of 0.012 mm and a spacing of 0.5 mm between adjacent arrays until the silver nanowire array covered the entire glass substrate.
[0081] Electrodes were placed at both ends of the first silver nanowire array so that both ends of all silver nanowire bundles in the first silver nanowire array were in contact with the electrode plates. The array was then energized under a DC voltage of 36V until all silver nanowire bundles were completely disconnected. The same method was used to energize subsequent silver nanowire arrays.
[0082] The electrode sheet is removed, and electrodes are fabricated in the original positions of the electrode sheet using an inkjet printing process, so that both ends of all silver nanowire bundles are in contact with the electrodes.
[0083] A PET film is placed parallel to a glass substrate, and then bonded to the surface of a silver nanowire array using insulating tape to obtain a resistive screen.
[0084] Example 2
[0085] The glass substrate and two electrodes were cleaned with acetone and ethanol for 15 minutes under ultrasonic conditions, respectively, and then allowed to air dry. The selected electrode thickness was 0.6 mm. A silver nanowire array was fabricated on the cleaned glass substrate surface using inkjet printing. During coating, the width of the first silver nanowire array was controlled to be 0.3 mm, the angle between all parallel silver nanowire bundles in the first array and the edge of the glass substrate was 45°, the spacing between all adjacent parallel silver nanowire bundles was 0.6 mm, and the resistance of all silver nanowire bundles was controlled to be approximately 110 Ω. Following the arrangement direction of all silver nanowire bundles in the first array, subsequent silver nanowire arrays were designed with a width increase of 0.011 mm and a spacing of 0.6 mm between adjacent arrays until the silver nanowire array covered the entire glass substrate.
[0086] Electrodes were placed at both ends of the first silver nanowire array so that both ends of all silver nanowire bundles in the first silver nanowire array were in contact with the electrode plates. The array was then energized under a DC voltage of 40V until all silver nanowire bundles were completely disconnected. The same method was used to energize subsequent silver nanowire arrays.
[0087] The electrode sheet is removed, and electrodes are fabricated in the original positions of the electrode sheet using an inkjet printing process, so that both ends of all silver nanowire bundles are in contact with the electrodes.
[0088] A PET film is placed parallel to a glass substrate, and then bonded to the surface of a silver nanowire array using insulating tape to obtain a resistive screen.
[0089] Example 3
[0090] The glass substrate and two electrodes were cleaned with acetone and ethanol for 15 minutes under ultrasonic conditions, respectively, and then allowed to air dry. The selected copper electrode thickness was 0.8 mm. A silver nanowire array was fabricated on the cleaned glass substrate surface using inkjet printing. During coating, the width of the first silver nanowire array was controlled to be 0.4 mm, the angle between all parallel silver nanowire bundles in the first array and the edge of the glass substrate was 60°, the spacing between all adjacent parallel silver nanowire bundles was 0.8 mm, and the resistance of all silver nanowire bundles was controlled to be approximately 120 Ω. Following the arrangement direction of all silver nanowire bundles in the first array, subsequent silver nanowire arrays were designed with a width increase of 0.01 mm and a spacing of 0.8 mm between adjacent arrays until the silver nanowire array covered the entire glass substrate.
[0091] Electrodes were placed at both ends of the first silver nanowire array so that both ends of all silver nanowire bundles in the first silver nanowire array were in contact with the electrode plates. The array was then energized under a DC voltage of 43V until all silver nanowire bundles were completely disconnected. The same method was used to energize subsequent silver nanowire arrays.
[0092] The electrode sheet is removed, and electrodes are fabricated in the original positions of the electrode sheet using an inkjet printing process, so that both ends of all silver nanowire bundles are in contact with the electrodes.
[0093] A PET film is placed parallel to a glass substrate, and then bonded to the surface of a silver nanowire array using insulating tape to obtain a resistive screen.
[0094] Example 4
[0095] The glass substrate and two electrodes were cleaned with acetone and ethanol for 15 minutes under ultrasonic conditions, respectively, and then allowed to air dry. The thicknesses of the two electrodes were 0.5 mm and 0.6 mm, respectively. Silver nanowire arrays were fabricated on the cleaned glass substrate surface using inkjet printing. During coating, the width of the first silver nanowire array was controlled to be 0.2 mm, and the angle between all parallel silver nanowire bundles in the first array and the edge of the glass substrate was 30°. The spacing between adjacent parallel silver nanowire bundles was controlled to be 0.5 mm and 0.6 mm, and the resistance of all silver nanowire bundles was controlled to be approximately 100 Ω. A second silver nanowire array was fabricated along the arrangement direction of all silver nanowire bundles in the first array, with a 0.6 mm gap between the first and second arrays. The second array was 0.01 mm wider than the first array. Along the arrangement direction of all silver nanowire bundles in the second silver nanowire array, subsequent silver nanowire arrays are designed with a width increase of 0.012 mm and a spacing of 0.5 mm between adjacent silver nanowire arrays, until the silver nanowire arrays cover the entire glass substrate.
[0096] The subsequent preparation methods are the same as in Example 1.
[0097] Example 5
[0098] The difference between Example 5 and Example 1 is that the angle between all silver nanowire bundles and the edge of the glass substrate is 20°.
[0099] Example 6
[0100] The difference between Example 6 and Example 1 is that the angle between all silver nanowire bundles and the edge of the glass substrate is 75°.
[0101] Example 7
[0102] The difference between Example 7 and Example 1 is that the width of the silver nanowire array is increased by 0.015 mm.
[0103] Example 8
[0104] The difference between Example 8 and Example 1 is that the width of the first silver nanowire array is 0.5 mm.
[0105] Example 9
[0106] The difference between Example 9 and Example 1 is that the silver nanowire bundles in the subsequent silver nanowire array are not arranged along the direction of the silver nanowire bundles in the first silver nanowire array, that is, there are no silver nanowire bundles in two adjacent silver nanowire arrays that are on the same straight line.
[0107] Comparative Example 1
[0108] The difference between Comparative Example 1 and Example 1 is that all silver nanowire arrays have the same width.
[0109] Because all the silver nanowire arrays have the same width, the resistance of the transverse silver nanowire array structure is the same. This results in some of the output resistances being the same at different positions when the touch is activated, making it impossible to determine the touch position and leading to poor positioning accuracy.
[0110] Comparative Example 2
[0111] The difference between Comparative Example 2 and Example 1 is that all silver nanowire bundles are at a 90° angle to the electrode.
[0112] Since the electron wind force is along the direction of the silver nanowire bundle and the electric field force is along the horizontal direction, and the direction of the silver nanowire bundle is consistent with the horizontal direction, there is no tensile stress in the silver nanowire bundle. Therefore, the silver nanowire bundle will not form a break and cannot realize the touch function.
[0113] The resistive screens prepared in Examples 1 to 9 and Comparative Example 1 were assembled and their performance was tested. The test results are shown in Table 1.
[0114] Table 1
[0115]
[0116] As shown in Table 1, Examples 1 to 9 exhibit excellent overall sensing time and positioning accuracy. Comparing Examples 1 with Examples 5 and 6 reveals that a larger angle reduces the number of silver nanowire bundles in a single array, leading to decreased positioning accuracy; a smaller angle prevents some silver nanowire bundles from contacting the electrodes at both ends, thus avoiding tensile stress failure and resulting in decreased accuracy. Comparing Examples 1 with Examples 7 and 8 shows that a larger width increase leads to excessively large linewidths at the substrate tail, reducing positioning accuracy; a larger initial array width increases resistance, resulting in longer sensing time. Furthermore, inconsistent vertical and horizontal spacing within the array affects resistance collection, consequently reducing accuracy.
[0117] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0118] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.
Claims
1. A resistive touchscreen, characterized in that, The device includes a transparent substrate, a transparent conductive layer, and a flexible thin film stacked sequentially. The transparent conductive layer includes multiple electrodes and silver nanowire arrays connecting adjacent electrodes. The width of the silver nanowire arrays increases sequentially. Each silver nanowire array includes multiple parallel silver nanowire bundles. The angle between the silver nanowire bundles and the electrodes is greater than 0° and less than 90°. Each silver nanowire bundle can form a conductive path under pressure. The silver nanowire bundle has a breakpoint and silver nanoparticles distributed near the breakpoint. By pressing, the silver nanoparticles are forced into the breakpoint, thereby forming a conductive path in the silver nanowire bundle.
2. The resistive touchscreen according to claim 1, characterized in that, The angle between the silver nanowire bundle and the electrode is 30°-60°.
3. The resistive touchscreen according to claim 1 or claim 2, characterized in that, The transparent conductive layer satisfies at least one of the following conditions: (1) The difference in width of the silver nanowire array is 0.01 mm to 0.012 mm; (2) The minimum width of the silver nanowire array is 0.2 mm to 0.4 mm; (3) In each of the silver nanowire arrays, the spacing between two adjacent silver nanowire bundles is 0.5 mm to 0.8 mm; (4) The width of each electrode is 0.5 mm to 0.8 mm; (5) At least some of the silver nanowire bundles in two adjacent silver nanowire arrays are on the same straight line.
4. The resistive touchscreen according to claim 3, characterized in that, The widths of the silver nanowire arrays are all equal.
5. The resistive touchscreen according to claim 3, characterized in that, In each of the silver nanowire arrays, the spacing between two adjacent silver nanowire bundles is equal.
6. The resistive touchscreen according to claim 3, characterized in that, Each of the electrodes has the same width.
7. The resistive touchscreen according to claim 1, characterized in that, The electrode is selected from silver nanowire electrodes.
8. A method for preparing a resistive screen as described in any one of claims 1 to 7, characterized in that, Includes the following steps: Multiple silver nanowire arrays with progressively increasing widths and spaced apart are prepared on the surface of a transparent substrate. Each silver nanowire array includes multiple parallel silver nanowire bundles. The angle between the silver nanowire bundles and the arrangement direction of the silver nanowire array is greater than 0° and less than 90°. Electrode plates are placed at opposite ends of each silver nanowire array so that both ends of the silver nanowire bundle are in contact with the electrode plates. The silver nanowire bundle in each silver nanowire array is disconnected by energizing. Remove the electrode sheet and prepare an electrode at the original position of the electrode sheet, so that both ends of the silver nanowire bundle in each silver nanowire array are in contact with the electrode; A flexible film is deposited on the surface of the silver nanowire array, and the flexible film is parallel to the transparent substrate to obtain a resistive screen.
9. The method for preparing a resistive screen according to claim 8, characterized in that, Before the electro-energizing process, the minimum resistance of each silver nanowire bundle is 100Ω-120Ω; And / or, the voltage of the power-on process is 36V-43V.
10. A touch device, characterized in that, Including the resistive screen as described in any one of claims 1 to 7.
Citation Information
Patent Citations
Method for preparing silver nano sheet self-assembling material
CN101811193A
Low-temperature conductive silver paste and preparation method and application thereof
CN106024100A