Barium titanate-based energy storage ceramics and preparation method and application thereof
Through the high entropy design and ion doping of barium titanate-based energy storage ceramic materials, the problem of low energy storage density of dielectric capacitors is solved, high energy storage density and high efficiency are achieved, and it is suitable for fields such as avionics and automobile industries.
Patent Information
- Application Number
- CN202311595028.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2023-11-21
- Filing Date
- 2023-11-27
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-11-27
AI Technical Summary
The existing dielectric capacitors have low energy storage density, making it difficult to achieve high energy storage density and high energy storage efficiency at the same time, limiting their application in the avionics, automobile industry and other fields.
Barium titanate-based energy storage ceramic material is used, and its chemical composition is (Ba0.47-2xBi0.32Ca0.11SmxNaxSr0.1)(Ti0.68-yFe0.32Zry)O3. Through high entropy design and ion doping, electron scattering is enhanced. and lattice distortion, reduce conduction loss, improve breakdown strength and energy storage density, while inhibiting nanodomain growth and maintaining high energy storage efficiency.
It has achieved high energy storage density (8J/cm3~10J/cm3) and high energy storage efficiency (85%~93.5%) of barium titanate-based energy storage ceramics, meeting a wider range of application needs, and the preparation process is simple and suitable for scale. Chemical production.
Smart Images

Figure CN117602933B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of dielectric energy storage ceramic materials, and specifically relates to a barium titanate-based energy storage ceramic and a preparation method and application thereof. Background Art
[0002] With the rapid development of microwave communications, automotive industry, and aerospace technology, the demand for high-performance energy storage capacitors in the power industry continues to grow. Compared with various types of batteries and electrochemical capacitors, dielectric capacitors have become core components in avionics, automotive industry, military applications, etc. due to their ultra-high charge and discharge rates and extremely high power density. However, the energy storage density of dielectric capacitors is relatively low, which limits their further application. How to improve the energy storage properties of dielectric capacitors has become a research hotspot in this field.
[0003] The energy storage density of a dielectric capacitor is determined by the applied electric field and the dielectric polarization, effectively increasing the polarization intensity difference (P m -P r ), and enhanced breakdown field strength (E b ) are two important ways to improve the energy storage properties of dielectric materials. BaTiO3 is the earliest discovered ABO3 perovskite ferroelectric material. Since its discovery, researchers have carried out a lot of work on it. However, it is often difficult to obtain high energy storage density and energy storage efficiency at the same time. This is mainly because a significant increase in energy storage density is usually achieved under high electric fields, but the energy storage efficiency is reduced due to increased conduction losses and the growth of nanodomains. Therefore, the preparation of a ceramic with both high energy storage density and high energy storage efficiency has very important application value. Summary of the invention
[0004] The present invention aims to solve one of the technical problems in the related art to at least a certain extent. To this end, one object of the present invention is to provide a barium titanate-based energy storage ceramic and a preparation method and application thereof. The barium titanate-based energy storage ceramic not only has a high energy storage density, but also maintains a high energy storage efficiency, which can meet the use needs to a greater extent. Specifically, at room temperature and 100Hz, the energy storage density of the barium titanate-based energy storage ceramic is 8J / cm 3 ~10J / cm 3 , the energy storage efficiency is 85% to 93.5%.
[0005] In one aspect of the present invention, the present invention provides a barium titanate-based energy storage ceramic. According to an embodiment of the present invention, the chemical composition of the barium titanate-based energy storage ceramic includes (Ba 0.47-2x Bi 0.32 Ca 0.11 Sm x Na x Sr 0.1 )(Ti 0.68-y Fe 0.32 Zr y )O3, where 0<x≤0.14, 0≤y≤0.10.
[0006] According to the above-mentioned embodiment of the present invention, the chemical composition of the barium titanate-based energy storage ceramic includes (Ba 0.47- 2x Bi 0.32 Ca 0.11 Sm x Na x Sr 0.1 )(Ti 0.68-y Fe 0.32 Zr y )O3, where 0<x≤0.14, 0≤y≤0.10. The calculation formula of the configuration entropy of barium titanate-based energy storage ceramics is: Where R is the ideal gas constant, x i is the percentage of elements occupying the cation sites, x j It is the percentage of elements occupying anionic sites. High entropy requires that the configuration entropy S is greater than 1.5R. High entropy design is achieved by adjusting the doping content of Sm, Na and / or Zr ions. High entropy design helps to enhance electron scattering, cause large lattice distortion and smaller grain size, thereby reducing conduction losses and improving resistivity, which helps to greatly improve the breakdown strength, thereby improving the energy storage density of ceramic materials. At the same time, the introduced Sm, Na and / or Zr ions with different ionic radii, valence states and electronegativity transform micron domains into nano domains, and inhibit the further growth of nano domains under high electric fields, ensuring the high energy storage efficiency of ceramic materials under high electric fields. As a result, the barium titanate-based energy storage ceramic not only has a high energy storage density, but also maintains a high energy storage efficiency, which can meet the needs of use to a greater extent.
[0007] In addition, the barium titanate-based energy storage ceramic according to the above embodiment of the present invention may also have the following additional technical features:
[0008] In some embodiments of the present invention, 0.04≤x≤0.10, 0.02≤y≤0.08. Thus, the energy storage density and energy storage efficiency of the barium titanate-based energy storage ceramic can be improved.
[0009] In some embodiments of the present invention, at 1050° C. to 1100° C., the breakdown field strength of the barium titanate-based energy storage ceramic is 540 kV / cm to 550 kV / cm.
[0010] In some embodiments of the present invention, at room temperature and 100 Hz, the energy storage density of the barium titanate-based energy storage ceramic is 8 J / cm 3 ~10J / cm 3 , the energy storage efficiency is 85% to 93.5%.
[0011] In a second aspect of the present invention, the present invention provides a method for preparing the above-mentioned barium titanate-based energy storage ceramic. According to an embodiment of the present invention, the method comprises:
[0012] (1) According to the chemical composition (Ba 0.47-2x Bi 0.32 Ca 0.11 Sm x Na x Sr 0.1 )(Ti 0.68-y Fe 0.32 Zr y )O3 stoichiometric ratio of Ba source, Bi source, Ca source, Sm source, Na source, Sr source, Ti source, Fe source and / or Zr source, mixed, ground and then dried to obtain a mixed material powder;
[0013] (2) calcining the mixed material powder to obtain barium titanate-based energy storage ceramic precursor powder;
[0014] (3) mixing the barium titanate-based energy storage ceramic precursor powder and the binder, pressing the mixture into sheets, and removing the binder to obtain a barium titanate-based energy storage ceramic green body;
[0015] (4) Sintering the barium titanate-based energy storage ceramic green body to obtain the barium titanate-based energy storage ceramic.
[0016] According to the method for preparing barium titanate-based energy storage ceramics according to the above embodiment of the present invention, first, according to the chemical composition (Ba 0.47-2x Bi 0.32 Ca 0.11 Sm x Na x Sr 0.1 )(Ti 0.68-y Fe 0.32 Zr y)O3 stoichiometric ratio of Ba source, Bi source, Ca source, Sm source, Na source, Sr source, Ti source, Fe source and / or Zr source are weighed, mixed, ground and dried to obtain a mixed powder. Grinding ensures that all raw materials are evenly mixed and the particles become smaller, which is conducive to the subsequent calcination reaction. The mixed powder is then calcined. Calcination promotes the solid-phase chemical reaction of each raw material to be more sufficient and uniform, to obtain a solid solution with a fixed composition, to form a main crystalline phase, and at the same time reduces carbon dioxide and moisture in the raw materials, reduces the shrinkage and deformation of the green body during the sintering process, avoids the cracking of the product and better controls the external dimensions. The barium titanate-based energy storage ceramic precursor powder obtained by calcination is mixed with a binder and pressed into sheets and debonded to obtain a barium titanate-based energy storage ceramic green body. Finally, the barium titanate-based energy storage ceramic green body is sintered to obtain a barium titanate-based energy storage ceramic with excellent density and good strength. Therefore, this method can be used to prepare barium titanate-based energy storage ceramics with high energy storage density and energy storage efficiency. At the same time, the preparation process is simple, has good repeatability, and has low requirements for production equipment and sites, which is conducive to large-scale and industrial production, and the prepared ceramics have stable performance.
[0017] In addition, the method for preparing barium titanate-based energy storage ceramics according to the above embodiment of the present invention may also have the following additional technical features:
[0018] In some embodiments of the present invention, the Ba source includes at least one of BaCO3 and BaO.
[0019] In some embodiments of the present invention, the Bi source includes Bi2O3.
[0020] In some embodiments of the present invention, the Ca source includes CaCO3.
[0021] In some embodiments of the present invention, the Sm source includes Sm2O3.
[0022] In some embodiments of the present invention, the Na source includes Na2CO3.
[0023] In some embodiments of the present invention, the Sr source includes SrCO3.
[0024] In some embodiments of the present invention, the Ti source includes TiO2.
[0025] In some embodiments of the present invention, the Fe source includes Fe2O3.
[0026] In some embodiments of the present invention, the Zr source includes ZrO2.
[0027] In some embodiments of the present invention, in step (1), the grinding speed is 260 r / min to 300 r / min, and the grinding time is 12 h to 24 h, thereby ensuring that the mixed material is mixed evenly and the appropriate particle size of the particles is controlled.
[0028] In some embodiments of the present invention, in step (1), the drying temperature is 68° C. to 72° C., and the drying time is 6 h to 12 h.
[0029] In some embodiments of the present invention, in step (2), the calcination temperature is 600° C. to 800° C. and the calcination time is 2 h to 3 h. This can promote the solid-phase chemical reaction of each raw material to obtain a semi-phase precursor powder.
[0030] In some embodiments of the present invention, the pressure for pressing into tablets is 2 MPa to 8 MPa, and the holding time is 1 min to 2 min.
[0031] In some embodiments of the present invention, the debinding temperature is 500° C. to 600° C., and the debinding time is 2 h to 4 h.
[0032] In some embodiments of the present invention, the adhesive comprises at least one of a 5wt% to 8wt% polyvinyl alcohol aqueous solution and a 5wt% to 8wt% polyvinyl butyral ethanol solution.
[0033] In some embodiments of the present invention, in step (4), the sintering temperature is 1000° C. to 1200° C., and the sintering time is 2 h to 3 h. Thus, the density and strength of the barium titanate-based energy storage ceramic can be improved.
[0034] In a third aspect of the present invention, the present invention proposes the use of the above-mentioned barium titanate-based energy storage ceramics or the barium titanate-based energy storage ceramics prepared by the above-mentioned method in the fields of communications, aviation or automobile manufacturing.
[0035] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0037] Figure 1 is the XRD diagram of the barium titanate-based energy storage ceramics of Examples 1-3 of the present invention and Comparative Example 1;
[0038] Figure 2 is a STEM image of the barium titanate-based energy storage ceramic of Example 1 of the present invention;
[0039] Figure 3 is a PE curve measured at the maximum breakdown strength of the barium titanate-based energy storage ceramic of Example 1 of the present invention;
[0040] Figure 4 is a PE curve measured at the maximum breakdown strength of the barium titanate-based energy storage ceramic of Example 2 of the present invention;
[0041] Figure 5 is a PE curve measured at the maximum breakdown strength of the barium titanate-based energy storage ceramic of Example 3 of the present invention;
[0042] Figure 6 It is the PE curve measured at the maximum breakdown strength of the barium titanate-based energy storage ceramic of Comparative Example 1 of the present invention;
[0043] Figure 7 It is the PE curve measured at the maximum breakdown strength of the barium titanate-based energy storage ceramic of Comparative Example 2 of the present invention. DETAILED DESCRIPTION
[0044] The embodiments of the present invention are described in detail below, which are intended to explain the present invention but are not to be construed as limiting the present invention.
[0045] In one aspect of the present invention, the present invention provides a barium titanate-based energy storage ceramic. According to an embodiment of the present invention, the chemical composition of the barium titanate-based energy storage ceramic includes (Ba 0.47-2x Bi 0.32 Ca 0.11 Sm x Na x Sr 0.1 )(Ti 0.68-y Fe 0.32 Zr y )O3, where 0<x≤0.14, 0≤y≤0.10.
[0046] According to the above-mentioned embodiment of the present invention, the chemical composition of the barium titanate-based energy storage ceramic includes (Ba 0.47- 2x Bi 0.32 Ca 0.11 Sm x Na x Sr 0.1 )(Ti 0.68-y Fe 0.32 Zr y )O3, where 0<x≤0.14, 0≤y≤0.10. The calculation formula of the configuration entropy of barium titanate-based energy storage ceramics is: Where R is the ideal gas constant, x i is the percentage of elements occupying the cation sites, x jIt is the percentage of elements occupying anionic sites. High entropy requires that the configuration entropy S is greater than 1.5R. High entropy design is achieved by adjusting the doping content of Sm, Na and / or Zr ions. High entropy design helps to enhance electron scattering, cause large lattice distortion and smaller grain size, thereby reducing conduction losses and improving resistivity, which helps to greatly improve the breakdown strength, thereby improving the energy storage density of ceramic materials. At the same time, the introduced Sm, Na and / or Zr ions with different ionic radii, valence states and electronegativity transform micron domains into nano domains, and inhibit the further growth of nano domains under high electric fields, ensuring the high energy storage efficiency of ceramic materials under high electric fields. As a result, the barium titanate-based energy storage ceramic not only has a high energy storage density, but also maintains a high energy storage efficiency, which can meet the needs of use to a greater extent.
[0047] According to an embodiment of the present invention, at 1050° C. to 1100° C., the breakdown field strength of the barium titanate-based energy storage ceramic is 540 kV / cm to 550 kV / cm.
[0048] According to an embodiment of the present invention, 0.04≤x≤0.10, 0.02≤y≤0.08. By controlling the values of x and y within the above range, the energy storage density and energy storage efficiency of the barium titanate-based energy storage ceramic can be significantly improved.
[0049] In a second aspect of the present invention, the present invention provides a method for preparing the above-mentioned barium titanate-based energy storage ceramic. According to an embodiment of the present invention, the method comprises:
[0050] S100: Preparation of mixed powder
[0051] In this step, according to the chemical composition (Ba 0.47-2x Bi 0.32 Ca 0.11 Sm x Na x Sr 0.1 )(Ti 0.68-y Fe 0.32 Zr y)O3 stoichiometric ratio, weigh Ba source, Bi source, Ca source, Sm source, Na source, Sr source, Ti source, Fe source and / or Zr source, mix, grind and dry, grind to ensure that all raw materials are evenly mixed, the particles become smaller, which is conducive to the subsequent calcination reaction, so as to obtain a mixed material powder. It should be noted that the Ba source, Bi source, Ca source, Sm source, Na source, Sr source, Ti source, Fe source and Zr source are conventional compounds in the field, and those skilled in the art can select them according to actual conditions. For example, the Ba source includes at least one of BaCO3 and BaO, the Bi source includes Bi2O3, the Ca source includes CaCO3, the Sm source includes Sm2O3, the Na source includes Na2CO3, the Sr source includes SrCO3, the Ti source includes TiO2, the Fe source includes Fe2O3, and the Zr source includes ZrO2.
[0052] According to an embodiment of the present invention, the grinding speed is 260r / min to 300r / min, and the grinding time is 12h to 24h. By controlling the grinding speed and time within the above range, the materials can be mixed more evenly, ensuring the particle size of the particles, thereby improving the curing reaction efficiency of calcination. It can be understood by those skilled in the art that grinding is a conventional operation in the art, and conventional equipment is also used, such as a ball mill, and the ball milling medium is a molten iron ball. Furthermore, the drying temperature is 68°C to 72°C, and the drying time is 6h to 12h, so that the moisture in the mixture can be removed as much as possible.
[0053] S200: Calcination of mixed powder
[0054] In this step, the mixed material powder is calcined. Calcination promotes a more complete and uniform solid-phase chemical reaction of each raw material to obtain a solid solution with a fixed composition and form a main crystal phase. At the same time, it reduces carbon dioxide and moisture in the raw materials, reduces shrinkage and deformation of the green body during sintering, avoids cracking of the product and better controls the external dimensions.
[0055] According to an embodiment of the present invention, the calcination temperature is 600℃~800℃, and the time is 2h~3h. The inventors found that if the calcination temperature is too high and the time is too long, the grains will be too large after calcination, the sintering driving force will decrease, and it will be not conducive to sintering; if the calcination temperature is too low and the time is too short, the main crystal phase will not be obvious and many impurities will be generated. Therefore, the calcination temperature of the present application is 600℃~800℃, and the time is 2h~3h, which can remove the volatiles in the raw materials to prevent excessive shrinkage and cracks during the sintering process, and at the same time, the desired crystal phase can be formed.
[0056] S300: Mix barium titanate-based energy storage ceramic precursor powder and binder and press into tablets
[0057] In this step, the calcined barium titanate-based energy storage ceramic precursor powder and the binder are fully mixed and stirred in a mortar, aged for 2 hours, passed through a 150-mesh screen, and then pressed into tablets in an automatic tablet press. The pressure of the tablet press is 2MPa to 8MPa, and the holding time is 1min to 2min. Finally, the tablet is placed in a muffle furnace, and the binder is removed at a temperature of 500°C to 600°C for 2h to 4h to remove the binder, thereby obtaining a barium titanate-based energy storage ceramic green body. Furthermore, the binder includes at least one of a 5wt% to 8wt% polyvinyl alcohol aqueous solution and a 5wt% to 8wt% polyvinyl butyral ethanol solution. Specifically, 1g of barium titanate-based energy storage ceramic precursor powder is mixed with 2 to 3 drops of the above-mentioned binder.
[0058] S400: Sintering barium titanate-based energy storage ceramic green bodies
[0059] In this step, the barium titanate-based energy storage ceramic green body is placed in a muffle furnace for sintering, thereby obtaining a barium titanate-based energy storage ceramic with excellent density and certain strength, thereby achieving ceramic densification.
[0060] According to an embodiment of the present invention, the sintering temperature is 1000℃~1200℃, and the sintering time is 2h~3h. The inventors found that the selection of sintering temperature and time has an extremely important influence on the density and grain size of barium titanate-based energy storage ceramics, and thus affects the energy storage properties of barium titanate-based energy storage ceramics. Specifically, if the sintering temperature is too high and the time is too long, the sample is easy to melt, and grain abnormalities are prone to occur, a large number of impurities will be generated, and pores will appear, resulting in uneven grain size; if the sintering temperature is too low and the time is too short, the densification degree of the ceramic is not enough, the ceramic strength is insufficient, and impurities are prone to appear. Therefore, the present application adopts a sintering condition of a temperature of 1000℃~1200℃ and a time of 2h~3h, which can improve the density and strength of barium titanate-based energy storage ceramics, which is conducive to obtaining a pure phase structure, thereby improving the energy storage performance of barium titanate-based energy storage ceramics.
[0061] Thus, the method can be used to prepare barium titanate-based energy storage ceramics with high energy storage density and energy storage efficiency. At the same time, the preparation process is simple, has good repeatability, has low requirements for production equipment and sites, is conducive to large-scale and industrialized production, and the prepared ceramics have stable performance. It should be noted that the characteristics and advantages described above for barium titanate-based energy storage ceramics are also applicable to this method and will not be repeated here.
[0062] In a third aspect of the present invention, the present invention proposes the use of the above-mentioned barium titanate-based energy storage ceramics or the barium titanate-based energy storage ceramics prepared by the above-mentioned method in the fields of communications, aviation or automobile manufacturing.
[0063] The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present invention in any way.
[0064] Example 1
[0065] (1) BaCO3 powder, Bi2O3 powder, Fe2O3 powder, TiO2 powder, SrCO3 powder, Sm2O3 powder, Na2CO3 powder, CaCO3 powder, and ZrO2 powder are used as raw materials, and then (Ba 0.33 Bi 0.32 Ca 0.11 Sm 0.07 Na 0.07 Sr 0.1 )(Ti 0.63 Fe 0.32 Zr 0.05 )O3 stoichiometric ratio, weigh the raw materials, put the powder into a 250ml nylon ball mill, pour alcohol according to the mass ratio of raw material powder: anhydrous ethanol of 1:2, ball mill at a speed of 260r / min for 18 hours, separate the slurry, dry at 70°C for 10h, and then place the powder in a muffle furnace and heat it to 750°C at a heating rate of 5°C / min and calcine for 3 hours to obtain barium titanate-based energy storage ceramic precursor powder.
[0066] (2) The above-mentioned barium titanate-based energy storage ceramic precursor powder and a 5wt% polyvinyl alcohol aqueous solution (PVA solution adhesive) are fully mixed in an agate mortar. The ratio of precursor powder to adhesive is: 1g precursor powder: 2 drops of 5wt% polyvinyl alcohol aqueous solution. After aging for 2h, pass through a 150-mesh sieve, take 0.4g of powder and pour it into a tableting mold with a diameter of 10cm, and press it into shape in an automatic tablet press at a pressure of 4Mpa for 1 minute. Put the tablet into a muffle furnace and heat it to 600℃ at a heating rate of 2℃ / min. Keep it warm for 3h to remove the adhesive to obtain a barium titanate-based energy storage ceramic green body.
[0067] (3) The barium titanate-based energy storage ceramic green body is slowly transferred to a muffle furnace, and the temperature is raised to 1050° C. at a heating rate of 5° C. / min and kept for 3 h to obtain the barium titanate-based energy storage ceramic.
[0068] Example 2
[0069] (1) BaCO3 powder, Bi2O3 powder, Fe2O3 powder, TiO2 powder, SrCO3 powder, Sm2O3 powder, Na2CO3 powder, CaCO3 powder, and ZrO2 powder are used as raw materials, and then (Ba 0.39 Bi 0.32 Ca 0.11 Sm 0.04 Na 0.04 Sr 0.1 )(Ti0.58 Fe 0.32 Zr 0.1 )O3 stoichiometric ratio, weigh the raw materials, put the powder into a 250ml nylon ball mill, pour alcohol according to the mass ratio of raw material powder: anhydrous ethanol of 1:2, ball mill at a speed of 260r / min for 18 hours, separate the slurry, dry at 70°C for 10h, and then place the powder in a muffle furnace and heat it to 750°C at a heating rate of 5°C / min and calcine for 3 hours to obtain barium titanate-based energy storage ceramic precursor powder.
[0070] (2) The above-mentioned barium titanate-based energy storage ceramic precursor powder and a 5wt% polyvinyl alcohol aqueous solution (PVA solution adhesive) are fully mixed in an agate mortar. The ratio of precursor powder to adhesive is: 1g precursor powder: 2 drops of 5wt% polyvinyl alcohol aqueous solution. After aging for 2h, pass through a 150-mesh sieve, take 0.4g of powder and pour it into a tableting mold with a diameter of 10cm, and press it into shape in an automatic tablet press at a pressure of 4Mpa for 1 minute. Put the tablet into a muffle furnace and heat it to 600℃ at a heating rate of 2℃ / min. Keep it warm for 3h to remove the adhesive to obtain a barium titanate-based energy storage ceramic green body.
[0071] (3) The barium titanate-based energy storage ceramic green body is slowly transferred to a muffle furnace, and the temperature is increased to 1100° C. at a heating rate of 5° C. / min and kept at this temperature for 3 h to obtain the barium titanate-based energy storage ceramic.
[0072] Example 3
[0073] (1) BaCO3 powder, Bi2O3 powder, Fe2O3 powder, TiO2 powder, SrCO3 powder, Sm2O3 powder, Na2CO3 powder, and CaCO3 powder are used as raw materials, and then (Ba 0.27 Bi 0.32 Ca 0.11 Sm 0.1 Na 0.1 Sr 0.1 )(Ti 0.68 Fe 0.32 )O3 stoichiometric ratio, weigh the raw materials, put the powder into a 250ml nylon ball mill, pour alcohol according to the mass ratio of raw material powder: anhydrous ethanol of 1:2, ball mill at a speed of 260r / min for 18 hours, separate the slurry, dry at 70°C for 10h, and then place the powder in a muffle furnace and heat it to 750°C at a heating rate of 5°C / min and calcine for 3 hours to obtain barium titanate-based energy storage ceramic precursor powder.
[0074] (2) The above-mentioned barium titanate-based energy storage ceramic precursor powder and a 5wt% polyvinyl alcohol aqueous solution (PVA solution adhesive) are fully mixed in an agate mortar. The ratio of precursor powder to adhesive is: 1g precursor powder: 2 drops of 5wt% polyvinyl alcohol aqueous solution. After aging for 2h, pass through a 150-mesh sieve, take 0.4g of powder and pour it into a tableting mold with a diameter of 10cm, and press it into shape in an automatic tablet press at a pressure of 4Mpa for 1 minute. Put the tablet into a muffle furnace and heat it to 600℃ at a heating rate of 2℃ / min. Keep it warm for 3h to remove the adhesive to obtain a barium titanate-based energy storage ceramic green body.
[0075] (3) The barium titanate-based energy storage ceramic green body is slowly transferred to a muffle furnace, and the temperature is raised to 1075° C. at a heating rate of 5° C. / min and kept for 3 h to obtain the barium titanate-based energy storage ceramic.
[0076] Comparative Example 1
[0077] (1) BaCO3 powder, Bi2O3 powder, Fe2O3 powder, TiO2 powder, SrCO3 powder, and CaCO3 powder are used as raw materials, and then (Ba 0.47 Bi 0.32 Ca 0.11 Sr 0.1 )(Ti 0.68 Fe 0.32 )O3 stoichiometric ratio, weigh the raw materials, put the powder into a 250ml nylon ball mill, pour alcohol according to the mass ratio of raw material powder: anhydrous ethanol of 1:2, ball mill at a speed of 260r / min for 18 hours, separate the slurry, dry at 70°C for 10h, and then place the powder in a muffle furnace and heat it to 750°C at a heating rate of 5°C / min and calcine for 3 hours to obtain barium titanate-based energy storage ceramic precursor powder.
[0078] (2) The above-mentioned barium titanate-based energy storage ceramic precursor powder and a 5wt% polyvinyl alcohol aqueous solution (PVA solution adhesive) are fully mixed in an agate mortar. The ratio of precursor powder to adhesive is: 1g precursor powder: 2 drops of 5wt% polyvinyl alcohol aqueous solution. After aging for 2h, pass through a 150-mesh sieve, take 0.4g of powder and pour it into a tableting mold with a diameter of 10cm, and press it into shape in an automatic tablet press at a pressure of 4Mpa for 1 minute. Put the tablet into a muffle furnace and heat it to 600℃ at a heating rate of 2℃ / min. Keep it warm for 3h to remove the adhesive to obtain a barium titanate-based energy storage ceramic green body.
[0079] (3) The barium titanate-based energy storage ceramic green body is slowly transferred to a muffle furnace, and the temperature is raised to 1050° C. at a heating rate of 5° C. / min and kept for 3 h to obtain the barium titanate-based energy storage ceramic.
[0080] Comparative Example 2
[0081] (1) BaCO3 powder, Bi2O3 powder, Fe2O3 powder, TiO2 powder, SrCO3 powder, Sm2O3 powder, Na2CO3 powder, CaCO3 powder, and ZrO2 powder are used as raw materials, and then (Ba 0.15 Bi 0.32 Ca 0.11 Sm 0.16 Na 0.16 Sr 0.1 )(Ti 0.53 Fe 0.32 Zr 0.15 )O3 stoichiometric ratio, weigh the raw materials, put the powder into a 250ml nylon ball mill, pour alcohol according to the mass ratio of raw material powder: anhydrous ethanol of 1:2, ball mill at a speed of 260r / min for 18 hours, separate the slurry, dry at 70°C for 10h, and then place the powder in a muffle furnace and heat it to 750°C at a heating rate of 5°C / min and calcine for 3 hours to obtain barium titanate-based energy storage ceramic precursor powder.
[0082] (2) The above-mentioned barium titanate-based energy storage ceramic precursor powder and a 5wt% polyvinyl alcohol aqueous solution (PVA solution adhesive) are fully mixed in an agate mortar. The ratio of precursor powder to adhesive is: 1g precursor powder: 2 drops of 5wt% polyvinyl alcohol aqueous solution. After aging for 2h, pass through a 150-mesh sieve, take 0.4g of powder and pour it into a tableting mold with a diameter of 10cm, and press it into shape in an automatic tablet press at a pressure of 4Mpa for 1 minute. Put the tablet into a muffle furnace and heat it to 600℃ at a heating rate of 2℃ / min. Keep it warm for 3h to remove the adhesive to obtain a barium titanate-based energy storage ceramic green body.
[0083] (3) The barium titanate-based energy storage ceramic green body is slowly transferred to a muffle furnace, and the temperature is increased to 1100° C. at a heating rate of 5° C. / min and kept at this temperature for 3 h to obtain the barium titanate-based energy storage ceramic.
[0084] The performance of the barium titanate-based energy storage ceramics of Examples 1-3 and Comparative Examples 1-2 was measured as follows:
[0085] (1) XRD analysis was performed on the barium titanate-based energy storage ceramics of Examples 1-3 and Comparative Example 1. The results are as follows Figure 1 .from Figure 1 It can be seen that the high-entropy barium titanate-based energy storage ceramic samples of Examples 1-3 and Comparative Example 1 all have a single perovskite structure without obvious impurity phases.
[0086] (2) STEM analysis was performed on the barium titanate-based energy storage ceramics of Example 1. The results are as follows Figure 2 .from Figure 2 It can be seen that in the sample of Example 1, there are tetragonal domains ( Figure 2B) and rhombohedral domains ( Figure 2 C), and the transition region between tetragonal and rhombohedral domains was observed ( Figure 2 D), which is beneficial to reduce polarization anisotropy and domain switching barriers, thereby improving efficiency.
[0087] (3) The PE curve test was performed on the barium titanate-based energy storage ceramics of Examples 1-3 and Comparative Examples 1-2, respectively. Figure 3-7 As shown. Figure 3-5 It can be seen that the breakdown field strength of the barium titanate-based energy storage ceramics of Examples 1-3 can reach 540 kV / cm-550 kV / cm, and the energy storage density under the maximum electric field is 8.42 J / cm 3 ~10.00J / cm 3 , the efficiency is 87.3% to 93.5%, from Figure 6 and Figure 7 It can be seen that the breakdown field strength of the barium titanate-based energy storage ceramics of Comparative Examples 1 and 2 is significantly reduced to 320 kV / cm-390 kV / cm, so its energy storage density is reduced to 4.07 J / cm 3 ~5.16J / cm 3 The specific performance test results of the barium titanate-based energy storage ceramics of Examples 1-3 and Comparative Examples 1-2 are shown in Table 1.
[0088] Table 1
[0089]
[0090] As can be seen from Table 1, the barium titanate-based energy storage ceramics of Examples 1-3 have a high breakdown field strength (540 kV / cm-550 kV / cm), while maintaining an extremely high maximum polarization strength, and can meet the use requirements to a greater extent. Compared with Comparative Examples 1-2, the barium titanate-based energy storage ceramics of Examples 1-3 not only have a high energy storage density, but also have excellent energy storage efficiency.
[0091] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0092] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A barium titanate-based energy storage ceramic, characterized in that: The chemical composition of the barium titanate-based energy storage ceramic includes (Ba 0.47-2x Bi 0.32 Ca 0.11 Sm x Na x Sr 0.1 )(Ti 0.68-y Fe 0.32 Zr y )O3, where 0<x≤0.14, 0≤y≤0.10; At 1050° C. to 1100° C., the breakdown field strength of the barium titanate-based energy storage ceramic is 540 kV / cm to 550 kV / cm.
2. The barium titanate-based energy storage ceramic according to claim 1, characterized in that: 0.04≤x≤0.10, 0.02≤y≤0.
08.
3. The barium titanate-based energy storage ceramic according to claim 1, characterized in that: At room temperature and 100 Hz, the energy storage density of the barium titanate-based energy storage ceramic is 8 J / cm 3 ~10 J / cm 3 , the energy storage efficiency is 85%~93.5%.
4. A method for preparing the barium titanate-based energy storage ceramic according to any one of claims 1 to 3, characterized in that: include: (1) According to the chemical composition (Ba 0.47-2x Bi 0.32 Ca 0.11 Sm x Na x Sr 0.1 )(Ti 0.68-y Fe 0.32 Zr y )O3 stoichiometric ratio of Ba source, Bi source, Ca source, Sm source, Na source, Sr source, Ti source, Fe source and Zr source, mix and grind, and then dry to obtain a mixed material powder; (2) calcining the mixed material powder to obtain barium titanate-based energy storage ceramic precursor powder; (3) mixing the barium titanate-based energy storage ceramic precursor powder and the binder, pressing them into sheets, and removing the binder to obtain a barium titanate-based energy storage ceramic green body; (4) Sintering the barium titanate-based energy storage ceramic green body to obtain the barium titanate-based energy storage ceramic.
5. The method according to claim 4, characterized in that In step (1), the Ba source includes at least one of BaCO3 and BaO; Optionally, the Bi source comprises Bi2O3; Optionally, the Ca source comprises CaCO3; Optionally, the Sm source comprises Sm2O3; Optionally, the Na source comprises Na2CO3; Optionally, the Sr source comprises SrCO3; Optionally, the Ti source comprises TiO2; Optionally, the Fe source comprises Fe2O3; Optionally, the Zr source comprises ZrO2; Optionally, the grinding speed is 260 r / min~300 r / min, and the grinding time is 12h~24h; Optionally, the drying temperature is 68° C. to 72° C., and the drying time is 6 h to 12 h.
6. The method according to claim 4, characterized in that In step (2), the calcination temperature is 600°C to 800°C, and the calcination time is 2h to 3h.
7. The method according to claim 4, characterized in that In step (3), the pressure for pressing into tablets is 2MPa~8MPa, and the holding time is 1min~2min; Optionally, the debinding temperature is 500°C to 600°C, and the debinding time is 2h to 4h; Optionally, the adhesive comprises at least one of a 5wt% to 8wt% polyvinyl alcohol aqueous solution and a 5wt% to 8wt% polyvinyl butyral ethanol solution.
8. The method according to claim 4, characterized in that In step (4), the sintering temperature is 1000° C. to 1200° C., and the sintering time is 2 h to 3 h.
9. Use of the barium titanate-based energy storage ceramic according to any one of claims 1 to 3 or the barium titanate-based energy storage ceramic prepared by the method according to any one of claims 4 to 8 in the fields of communications, aviation or automobile manufacturing.