Methods for forming semiconductor structures

By selectively forming titanium silicide and molybdenum silicide layers on nFET and pFET contacts, and combining them with barrier layer treatment, the problem of high contact resistance in the prior art is solved, achieving ohmic/pseudo-ohmic contacts with low contact resistance and improving transistor performance.

CN117616554BActive Publication Date: 2026-11-10APPLIED MATERIALS INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202280048889.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-07-15
Filing Date
2022-07-13
Publication Date
2026-11-10
Estimated Expiration
2042-07-13

AI Technical Summary

Technical Problem

Existing technologies make it difficult to selectively form ohmic and pseudo-ohmic contacts on nFET and pFET contacts, resulting in high contact resistance and affecting transistor performance.

Method used

An opening is formed by patterning a substrate, depositing a titanium silicide layer and selectively removing a barrier layer, then forming a molybdenum silicide layer on the n and p transistors, depositing a barrier layer on it, and finally forming an ohmic/pseudo-ohmic contact through an annealing process.

Benefits of technology

This achieves ohmic/pseudo-ohmic contacts with low contact resistance on nFET and pFET contacts, improving the electrical performance and integration of transistors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117616554B_ABST
    Figure CN117616554B_ABST
Patent Text Reader

Abstract

A method for forming a semiconductor structure and the semiconductor structure are described. The method includes patterning a substrate to form a first opening and a second opening, the substrate including an n-transistor and a p-transistor, the first opening being on the n-transistor and the second opening being on the p-transistor; pre-cleaning the substrate; depositing titanium silicide (TiSi) layers on the n-transistor and p-transistor by plasma-enhanced chemical vapor deposition (PECVD); depositing a first barrier layer on the TiSi layers as appropriate, and selectively removing the first barrier layer from the p-transistor; selectively forming a molybdenum silicide (MoSi) layer on the TiSi layers on the n-transistor and p-transistor; forming a second barrier layer on the MoSi layers; and annealing the semiconductor structure. The method can be performed in a processing chamber without disrupting the vacuum.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] Embodiments of this disclosure relate to the field of semiconductor devices and the manufacture of semiconductor devices. More specifically, embodiments of this disclosure relate to a method for selectively forming a silicide layer having ohmic and pseudo-ohmic contacts. Background Technology

[0002] Integrated circuits have evolved into complex devices that can include millions of transistors, capacitors, and resistors on a single chip. In the evolution of integrated circuits, functional density (i.e., the number of interconnected devices per chip area) has generally increased, while geometric dimensions (i.e., the smallest components (or lines) that can be produced using manufacturing processes) have decreased.

[0003] Transistors are critical components in most integrated circuits. Since the drive current and consequent speed of a transistor are proportional to its gate width, faster transistors typically require larger gate widths. Therefore, there is a trade-off between transistor size and speed, and "fin field-effect transistors" (finFETs) have been developed to resolve this conflicting goal of achieving the maximum drive current and the smallest size. FinFETs are characterized by a fin-shaped channel region, which significantly increases the transistor's size without substantially increasing its footprint, and are now used in many integrated circuits. However, finFETs also have their own drawbacks.

[0004] As transistor device feature sizes continue to shrink to achieve greater circuit density and higher performance, there is a need to improve transistor device structures to enhance electrostatic coupling and reduce negative impacts such as parasitic capacitance and off-state leakage. Examples of transistor device structures include planar structures, FinFET structures, and gate-all-around (GAA) structures. The performance of logic gates is related to the properties of the materials used, as well as the thickness and area of ​​the structural layers. However, challenges arise as some gate characteristics are adjusted to accommodate device scaling.

[0005] Ohmic or pseudo-ohmic contacts are a key element in achieving low contact resistance at the source / drain contacts in transistors. There is a need in the art for methods to selectively form ohmic and pseudo-ohmic contacts on both nFET and pFET contacts. Summary of the Invention

[0006] One or more embodiments of this disclosure relate to a method for forming a semiconductor structure. The method includes patterning a substrate to form a first opening and a second opening, the substrate including an n-transistor and a p-transistor, the first opening being on the n-transistor and the second opening being on the p-transistor; pre-cleaning the substrate; depositing a titanium silicide (TiSi) layer on the n-transistor and the p-transistor by plasma-enhanced chemical vapor deposition (PECVD); depositing a first barrier layer on the TiSi layer as appropriate, and selectively removing the first barrier layer from the p-transistor; selectively forming a molybdenum silicide (MoSi) layer on the TiSi layer on the n-transistor and the p-transistor; forming a second barrier layer on the MoSi layer; and annealing the semiconductor structure.

[0007] Another embodiment of this disclosure relates to a method for forming a semiconductor structure. The method includes patterning a substrate to form a first opening, the substrate including an n-transistor and a p-transistor, the first opening being above the n-transistor; pre-cleaning the substrate; depositing a titanium silicide (TiSi) layer on the n-transistor by plasma-enhanced chemical vapor deposition (PECVD); filling the first opening with a first interstitial material; forming a mask layer on the top surface of the n-transistor; patterning the substrate to form a second opening above the p-transistor; selectively forming a molybdenum silicide (MoSi) layer on the p-transistor; annealing the semiconductor structure; and filling the second opening with a second interstitial material.

[0008] Another embodiment of this disclosure relates to a semiconductor structure. The semiconductor structure includes an n-transistor and a p-transistor; a titanium silicide (TiSi) layer on one or more of the n-transistor and the p-transistor; a molybdenum silicide (MoSi) layer on one or more of the n-transistor and the p-transistor; a barrier layer, if applicable, on one or more of the titanium silicide (TiSi) layer and the molybdenum silicide (MoSi) layer; and an interstitial material. Attached Figure Description

[0009] To gain a more detailed understanding of the features described above, a more specific description of the present disclosure, which is briefly summarized above, can be obtained by referring to the embodiments, some of which are shown in the accompanying drawings. However, it should be noted that the drawings only illustrate typical embodiments of the present disclosure and should therefore not be considered as limiting its scope, as the present disclosure allows for other equivalent embodiments.

[0010] Figure 1A The present disclosure illustrates a semiconductor structure according to one or more embodiments;

[0011] Figure 1B The present disclosure illustrates a semiconductor structure according to one or more embodiments;

[0012] Figure 1C The present disclosure illustrates a semiconductor structure according to one or more embodiments;

[0013] Figure 1D The present disclosure illustrates a semiconductor structure according to one or more embodiments;

[0014] Figure 1E The present disclosure illustrates a semiconductor structure according to one or more embodiments;

[0015] Figure 1F The present disclosure illustrates a semiconductor structure according to one or more embodiments;

[0016] Figure 2A The present disclosure illustrates a semiconductor structure according to one or more embodiments;

[0017] Figure 2B The present disclosure illustrates a semiconductor structure according to one or more embodiments;

[0018] Figure 2C The present disclosure illustrates a semiconductor structure according to one or more embodiments;

[0019] Figure 2D The present disclosure illustrates a semiconductor structure according to one or more embodiments;

[0020] Figure 2E The present disclosure illustrates a semiconductor structure according to one or more embodiments;

[0021] Figure 2F The present disclosure illustrates a semiconductor structure according to one or more embodiments;

[0022] Figure 2G The present disclosure illustrates a semiconductor structure according to one or more embodiments;

[0023] Figure 3 A process flow diagram illustrating one or more embodiments of the method according to this disclosure is shown; and

[0024] Figure 4 A process flow diagram of a method according to one or more embodiments of this disclosure is shown.

[0025] In the accompanying drawings, similar parts and / or features may have the same reference numerals. Furthermore, various parts of the same type can be distinguished by adding a dash after the reference numerals and a second reference numeral to differentiate similar parts. If only the first reference numeral is used in the description, the description applies to any similar part having the same first reference numeral, and is unrelated to the second reference numeral. Detailed Implementation

[0026] Before describing several exemplary embodiments of the present invention, it should be understood that the invention is not limited to the details of the construction or process steps set forth in the following description. The invention can have other embodiments and can be practiced or performed in various ways.

[0027] As used herein, the term "substrate" refers to a surface or portion thereof on which a process is performed. Those skilled in the art will also understand that, unless the context clearly indicates otherwise, reference to substrate may also refer only to a portion of the substrate. Furthermore, reference to deposition on a substrate may refer to a bare substrate or a substrate on which one or more films or features are deposited or formed.

[0028] Furthermore, as used herein, the term "substrate" refers to any substrate or material surface formed on a substrate during a manufacturing process. For example, depending on the application, substrate surfaces that can be processed include materials such as silicon, silicon oxide, strained silicon, silicon on insulator (SOI), carbon-doped silicon oxide, amorphous silicon, doped silicon, germanium, gallium arsenide, glass, sapphire, and any other materials such as metals, metal nitrides, metal alloys, dielectric materials, other conductive materials, or combinations thereof. In some embodiments, the substrate comprises silicon (Si), ruthenium (Ru), cobalt (Co), tungsten (W), silicon phosphide (SiP), titanium silicon (TiSi), titanium nitride (TiN), titanium aluminide (TiAl), silicon germanium (SiGe), silicon germanium boron (SiGeB), hafnium oxide (HfO2), aluminum oxide (Al2O3), or combinations thereof. Substrates include, but are not limited to, semiconductor wafers. The substrate may be exposed to pretreatment processes such as polishing, etching, reduction, oxidation, hydroxylation, annealing, and / or baking of the substrate surface. In addition to performing film treatment directly on the surface of the substrate itself, any of the disclosed film treatment steps may also be performed on the underlayer formed on the substrate, as disclosed in more detail below, and the term "substrate surface" is intended to include such an underlayer as referred to in the context.

[0029] According to one or more embodiments, the term "on" regarding a film or film layer includes a film or layer directly on a surface (e.g., a substrate surface), and having one or more underlying layers between the film or layer and the surface (e.g., the substrate surface). Therefore, in one or more embodiments, the phrase "on a substrate surface" is intended to include one or more underlying layers. In other embodiments, the phrase "directly on" refers to a layer or film in contact with a surface (e.g., a substrate surface) without an intermediate layer. Therefore, the phrase "layer directly on a substrate surface" refers to a layer in direct contact with the substrate surface without any intermediate layers.

[0030] As used herein, the term "substrate surface" refers to any substrate surface on which layers may be formed. A substrate surface may have one or more features formed therein, one or more layers formed thereon, and combinations thereof. The shape of a feature may be any suitable shape, including but not limited to peaks, trenches, and cylindrical through-holes. As used herein, the term "feature" refers to any intentional surface irregularity. Suitable examples of features include, but are not limited to, trenches having a top, two sidewalls, and a bottom; peaks having a top and two sidewalls extending upwards from the surface; and through-holes having sidewalls extending downwards from the surface and an open bottom.

[0031] As used herein, the term "processing chamber" includes multiple portions of the processing chamber adjacent to the substrate surface, but does not encompass the entire internal volume of the processing chamber. For example, in a sector of a spatially partitioned processing chamber, a portion of the processing chamber adjacent to the substrate surface is cleared of one or more reactive compounds by any suitable technique, including but not limited to moving the substrate through an air curtain to a portion or sector of the processing chamber that does not contain or substantially does not contain reactive compounds.

[0032] As used herein, the terms "atomic layer deposition" or "cyclic deposition" refer to sequential exposure to two or more reactive compounds to deposit a material layer on a substrate surface. The substrate or portions of its surface are sequentially exposed to two or more reactive compounds introduced into a reaction zone within a processing chamber. The sequential exposure of the reactive gases prevents or minimizes gas-phase reactions between them. In time-domain ALD processes, exposure to each reactive compound is separated by a time delay to allow each compound to adhere to and / or react on the substrate surface. In spatial ALD processes, different portions of the substrate surface or material on the substrate surface are simultaneously exposed to two or more reactive compounds such that no given point on the substrate is substantially exposed to more than one reactive compound simultaneously. As used in this specification and the appended claims, the term "substantially" as understood by one of those skilled in the art means that there is a possibility that small portions of the substrate may be simultaneously exposed to multiple reactive gases due to diffusion, and that such simultaneous exposure is unintentional.

[0033] In one aspect of the time-domain ALD process, a first reactive gas (i.e., a first precursor or compound A) is pulsed into the reaction zone, followed by a first time delay. Next, a second precursor or compound B is pulsed into the reaction zone, followed by a second delay. During each time delay, a purge gas, such as argon, is introduced into the processing chamber to purge the reaction zone or otherwise remove any residual reactive compounds or byproducts from the reaction zone. Alternatively, the purge gas may flow continuously throughout the deposition process, such that only the purge gas flows during the time delay between reactive compound pulses. The reactive compounds are pulsed alternately until the desired film or film thickness is formed on the substrate surface. In either case, the ALD process of pulsed delivery of compound A, purge gas, compound B, and purge gas constitutes one cycle. The cycle may begin with compound A or compound B and continue in the respective sequence until a film with the desired thickness is obtained. In one or more embodiments, the time-domain ALD process may be performed in a predetermined sequence using more than two reactive compounds.

[0034] In one aspect of the spatial ALD process, a first reactant gas and a second reactant gas are simultaneously delivered to the reaction zone, but separated by an inert gas curtain and / or a vacuum curtain. The substrate moves relative to the gas delivery device such that any given point on the substrate is exposed to the first reactant gas and the second reactant gas. In one or more embodiments, the spatial ALD process can be performed using more than two reactive compounds in a predetermined sequence.

[0035] In some embodiments, the substrate surface is substantially sequentially exposed to the first reactive compound and the second reactive compound. As used throughout the specification, "substantially sequentially" means that the majority of the exposure time of the first reactive compound does not overlap with the exposure time of the second reactive compound, although some overlap may exist.

[0036] As used herein, the term "chemical vapor deposition" refers to exposure to at least one reactive compound to deposit a material layer on a substrate surface. In some embodiments, a chemical vapor deposition (CVD) process includes mixing two or more reactive compounds in a processing chamber to allow for vapor-phase reaction and deposition of the reactive compounds. In some embodiments, a CVD process includes simultaneously exposing a substrate surface to two or more reactive compounds. In some embodiments, a CVD process includes continuously exposing a substrate surface to a first reactive compound and intermittently exposing it to a second reactive compound. In some embodiments, the substrate surface undergoes a CVD reaction to deposit a film of a predetermined thickness. In a CVD process, the film may be deposited in a single exposure to a mixed reactive compound, or it may be exposed to a mixed reactive compound multiple times, with decontamination in between. In some embodiments, the substrate surface is substantially simultaneously exposed to both a first and a second reactive compound.

[0037] As used throughout this specification, “substantially simultaneous” means that the majority of the duration of exposure to the first reacting compound overlaps with the duration of exposure to the second reacting compound.

[0038] As used herein, the term "decontamination" includes any suitable decontamination process that removes unreacted precursors, reaction products, and byproducts from a process area. Suitable decontamination processes include moving a substrate through a gas curtain to a portion or sector of the processing area that does not contain or substantially does not contain reactants. In one or more embodiments, the decontamination chamber includes applying a vacuum. In some embodiments, the decontamination area includes a decontamination gas flowing over the substrate. In some embodiments, the decontamination process includes a flowing inert gas. In one or more embodiments, the decontamination gas is selected from one or more of nitrogen (N2), helium (He), and argon (Ar). In some embodiments, the first reaction compound is purged from the reaction chamber for a duration ranging from 0.2 to 30 seconds, 0.2 to 10 seconds, 0.2 to 5 seconds, 0.5 to 30 seconds, 0.5 to 10 seconds, 0.5 to 5 seconds, 1 to 30 seconds, 1 to 10 seconds, 1 to 5 seconds, 5 to 30 seconds, 5 to 10 seconds, or 10 to 30 seconds before the substrate is exposed to the second reaction compound.

[0039] Plasma-enhanced chemical vapor deposition (PECVD) is widely used for depositing thin films due to its cost-effectiveness and versatility in film properties. For example, in a PECVD process, a hydrocarbon source, such as vaporized gaseous hydrocarbons or liquid hydrocarbons already entrained in a carrier gas, is introduced into the PECVD chamber. A plasma-initiating gas, typically helium, is also introduced into the chamber. The plasma is then activated within the chamber to generate excited CH radicals. These excited CH radicals chemically bind to the substrate surface located within the chamber, forming the desired film thereon. The embodiments described herein with respect to the PECVD process can be performed using any suitable thin film deposition system. Any apparatus described herein is not and should not be construed as limiting the scope of the embodiments described herein.

[0040] As used herein, the terms "shim" or "barrier layer" refer to a layer conformally formed along at least a portion of the sidewall and / or lower surface of an opening, such that a substantial portion of the opening prior to layer deposition remains unfilled after layer deposition. The shim can be formed along the entire sidewall and lower surface of the opening. The shim can be formed by any process known to those skilled in the art. In some embodiments, the shim comprises a metal nitride, a PVD metal, or a combination thereof.

[0041] A transistor is a circuit component or element that is often formed on a semiconductor device. Depending on the circuit design, many transistors can be formed on a semiconductor device in addition to capacitors, inductors, resistors, diodes, wires, or other components. A metal-oxide-semiconductor field-effect transistor (MOSFET) is a type of field-effect transistor (FET). It has an insulated gate, the voltage of which determines the conductivity of the device. This ability to change conductivity with the amount of applied voltage is used to amplify or switch electronic signals.

[0042] Generally, a transistor includes a gate formed between a source region and a drain region. The source and drain regions may include doped regions of the substrate and may exhibit a doping profile suitable for a particular application. The gate is located above the channel region and may include a gate dielectric interposed between the gate electrode and the channel region in the substrate.

[0043] As used herein, the term "field-effect transistor" or "FET" refers to a transistor that uses an electric field to control the electrical behavior of the device. Field-effect transistors typically exhibit very high input impedance at low temperatures. The conductivity between the drain and source terminals is controlled by an electric field in the device, generated by the voltage difference between the body and the gate. The three terminals of an FET are the source (S), through which charge carriers enter the channel; the drain (D), through which charge carriers leave the channel; and the gate (G), which modulates the channel conductivity. Conventionally, the current entering the channel at the source (S) is designated as I0. S The current entering the channel at the drain (D) is designated as I. D Specify the drain-to-source voltage as V. DS By applying a voltage to the gate (G), the current (i.e., Id) entering the channel at the drain can be controlled. D ).

[0044] A metal-oxide-semiconductor field-effect transistor (MOSFET) is a type of field-effect transistor (FET). It has an insulated gate, the voltage of which determines the device's conductivity. This ability to change conductivity with the applied voltage is used to amplify or switch electronic signals. A MOSFET is based on the modulation of charge concentration by a metal-oxide-semiconductor (MOS) capacitor between a host electrode and a gate electrode, which is located above the host and insulated from all other device regions by a gate dielectric layer. Compared to a MOS capacitor, a MOSFET includes two additional terminals (source and drain), each connected to a separate, highly doped region separated from the host region. These regions can be p-type or n-type, but they belong to the same type and are the opposite of the host region. The source and drain (different from the host) are highly doped, as indicated by the "+" sign after the doping type.

[0045] If the MOSFET is an n-channel or nMOS FET, then the source and drain are in the n+ region, while the bulk is in the p region. If the MOSFET is a p-channel or pMOS FET, then the source and drain are in the p+ region, while the bulk is in the n region. The source is named as such because it is the origin of charge carriers flowing through the channel (electrons in the n-channel and holes in the p-channel); similarly, the drain is where charge carriers leave the channel.

[0046] Embodiments of this disclosure provide semiconductor structures and methods for forming semiconductor structures. Ohmic and / or pseudo-ohmic contacts are key elements for achieving low contact resistance of source / drain contacts. One or more embodiments advantageously provide integration schemes to generate dual silicides to create ohmic / pseudo-ohmic contacts on both nFET and pFET contacts.

[0047] Embodiments of this disclosure are described with the aid of accompanying drawings, which illustrate the process for forming double silicides on ohmic / pseudo-ohmic contacts on both nFET and pFET contacts. Reference Figures 1A-1E The image shows a semiconductor structure 100. The semiconductor structure 100 includes an n-transistor 102 and a p-transistor 104. In one or more embodiments, each of the n-transistor 102 and the p-transistor 104 includes a dielectric material 110, a source / drain material 120, and a substrate 130.

[0048] In one or more embodiments, the dielectric material 110 may comprise any suitable dielectric material known to those skilled in the art. In some embodiments, the dielectric material 110 comprises one or more of silicon, silicon oxide, silicon nitride, silicon carbide, and low-k dielectrics. As used herein, terms such as “silicon oxide” and “silicon nitride” refer to materials comprising silicon and oxygen or silicon and nitrogen. “Silicon oxide” and “silicon nitride” should not be construed as implying any stoichiometric ratio. In other words, dielectric materials comprising silicon oxide or silicon nitride may be stoichiometric or non-stoichiometric, silicon-rich or silicon-poor. In some embodiments, the dielectric material 110 comprises silicon oxide (SiO2).

[0049] In some embodiments, n-transistor 102 and p-transistor 104 include source and drain contacts. In one or more embodiments, the source / drain material 120 may have more than one layer. In some embodiments, the source / drain material 120 includes a silicon layer (e.g., SiGe, SiP, etc.) having a doped epitaxial layer, a second silicide layer that may contain nickel (Ni), titanium (Ti), aluminum (Al), etc., and a third or top layer that may be a metal such as, but not limited to, cobalt, tungsten, ruthenium, etc.

[0050] In one or more specific embodiments, the source / drain material 120 of the n-transistor 102 comprises phosphorus (P)-doped silicon (Si). In one or more embodiments, the source / drain material 120 of the n-transistor 102 has a band gap in the range of about 1.0 eV to about 1.2 eV.

[0051] In one or more embodiments, the source / drain material 120 of the p transistor 104 comprises boron (B)-doped silicon germanium (SiGe). In one or more embodiments, the source / drain material 120 of the p transistor 104 has a band gap in the range of about 0.5 eV to about 1.0 eV.

[0052] refer to Figures 1A-1D A first opening 106 is present above the n-transistor 102, and a second opening 108 is present above the p-transistor 104. The first and second openings may have any suitable aspect ratio (the ratio of the depth to the width of the opening). In one or more embodiments, the first and second openings may independently have an aspect ratio in the range of 3:1 to 15:1, 6:1 to 15:1, 9:1 to 15:1, 12:1 to 15:1, or greater than 10:1.

[0053] In one or more embodiments, structure (or surface of structure) 100 is cleaned. In some embodiments, cleaning structure 100 removes oxides from the surface. In some embodiments, the oxides are native oxides. In some embodiments, cleaning the surface forms a substantially oxide-free surface. As used in this way, the term "substantially oxide-free" means that the surface contains less than or equal to 5%, 2%, 1%, or 0.5% oxygen atoms. In one or more embodiments, anisotropic etching is used to remove oxides from the surface. In one or more embodiments, anisotropic etching removes more oxides from the surface of source / drain material 120 than from dielectric material 110. In one or more embodiments, cleaning the structure forms a substantially oxide-free source / drain material 120.

[0054] refer to Figure 1B A titanium silicide (TiSi) layer 140 is deposited on each of the n-transistor 102 and the p-transistor 104. The titanium silicide layer 140 may have any suitable thickness. In some embodiments, the thickness of the titanium silicide layer 140 is... To date Within the range, or about To date Within the range, or about To date Within the range, or about To date Within the range. In one or more embodiments, the titanium silicide (TiSi) layer 140 has approximately The thickness of the titanium silicide (TiSi) layer 140 on the n transistor 102 is approximately 0.4 eV to approximately 0.55 eV.

[0055] refer to Figure 1C An optional first barrier layer 150 is deposited on each of the n-transistor 102 and the p-transistor 104. In one or more embodiments, the optional first barrier layer 150 comprises a metal. In one or more embodiments, the optional first barrier layer 150 comprises a metal nitride. In one or more embodiments, the optional first barrier layer 150 comprises one or more of titanium nitride (TiN), tantalum nitride (TaN), tungsten nitride (WN), and molybdenum nitride (MoN). In one or more embodiments, the n-transistor 102 having the optional first barrier layer 150 has a lower Schottky barrier height than the n-transistor without the optional first barrier layer.

[0056] refer to Figure 1DWhen present, the first barrier layer 150 on the p transistor 104 is selectively removed from the p transistor 104 but not from the n transistor. The first barrier layer 150 can be removed by any suitable technique known to those skilled in the art. In one or more embodiments, the first barrier layer 150 is removed by one or more of etching, chemical mechanical polishing (CMP), planarization, etc.

[0057] refer to Figure 1E A molybdenum silicide (MoSi) layer 160 is formed on the titanium silicide (TiSi) layer 140 on each of the n-transistors 102 and p-transistors 104. In one or more embodiments, the molybdenum silicide (MoSi) layer 160 is formed on an optional first barrier layer 150 on the n-transistor 102. The molybdenum silicide (MoSi) layer 160 may have any suitable thickness. In some embodiments, the thickness of the molybdenum silicide (MoSi) layer 160 is... To date Within the range, or about To date Within the range, or about To date Within the range, or about To date Within the range. In one or more embodiments, the molybdenum silicide (MoSi) layer 160 has approximately The thickness.

[0058] The molybdenum silicide (MoSi) layer 160 can be formed using any suitable process known to those skilled in the art. In one or more embodiments, structure 100 is first cleaned to remove oxides from the surface. In some embodiments, the oxides are native oxides. In some embodiments, cleaning the surface forms a substantially oxide-free surface. As used in this way, the term "substantially oxide-free" means that the surface contains less than or equal to 5%, 2%, 1%, or 0.5% oxygen atoms. In one or more embodiments, anisotropic etching is used to remove oxides from the surface.

[0059] In one or more embodiments, a metal film is selectively formed on the titanium silicide (TiSi) layer 140 to form the molybdenum silicide (MoSi) layer 160. In some embodiments, structure 100 is exposed to the metal precursor and reactants. The metal film can be deposited by an ALD deposition process, a CVD deposition process, or a combination thereof. In some embodiments, the metal film comprises a molybdenum silicide (MoSi) film.

[0060] In one or more embodiments, the metal precursor comprises a molybdenum precursor. In some embodiments, the molybdenum precursor comprises molybdenum halide. In some embodiments, the molybdenum halide comprises molybdenum fluoride, molybdenum chloride, or a combination thereof. In a particular embodiment, the molybdenum precursor comprises molybdenum fluoride. In other particular embodiments, the molybdenum precursor comprises molybdenum chloride. In one or more embodiments, a carrier gas is used to flow the precursor through a surface. In some embodiments, the carrier gas flows through an ampoule containing the precursor. In some embodiments, the carrier gas is an inert gas. In some embodiments, the inert gas comprises one or more of N2, Ar, and He.

[0061] In one or more embodiments, the reactants comprise an oxidizing agent, a reducing agent, or a combination thereof. In some embodiments, the reactants comprise hydrogen (H2), ammonia (NH3), silane, polysilane, or a combination thereof. In some embodiments, the silane is selected from one or more of disilane, trisilane, tetrasilane, higher silanes, and substituted silanes. In a particular embodiment, the reactants comprise silane to form a molybdenum silicide (MoSi) layer 160. In one or more embodiments, a carrier gas is used to flow the reactants through the surface. In some embodiments, the carrier gas is an inert gas. In some embodiments, the inert gas comprises one or more of N2, Ar, and He. In other embodiments, the reactant gas can flow continuously and the flow of the molybdenum precursor into the chamber can be opened and closed.

[0062] refer to Figure 1E A second barrier layer 170 is formed on each of the n-transistor 102 and the p-transistor 104. The second barrier layer 170 may contain any suitable material known to those skilled in the art. In one or more embodiments, the second barrier layer 170 comprises a PVD metal film. In one or more embodiments, the second barrier layer 170 comprises molybdenum silicide (MoSiN). In one or more embodiments, the second barrier layer 170 prevents the formation of oxides on the molybdenum silicide (MoSi) layer 160. In one or more embodiments, the n-transistor 102 on which the second barrier layer 170 is formed has a lower Schottky barrier height than the n-transistor without the second barrier layer. In one or more embodiments, the p-transistor 104 on which the second barrier layer 170 is formed has a lower Schottky barrier height than the p-transistor without the second barrier layer.

[0063] The second barrier layer 170 can be formed by any process known to those skilled in the art. In some embodiments, the second barrier layer 170 is formed on a molybdenum silicide (MoSi) layer 160. In some embodiments, the molybdenum silicide (MoSi) layer 160 is treated to form the second barrier layer 170. In some embodiments, the second barrier layer 170 is formed by nitriding the molybdenum silicide (MoSi) layer 160 or a portion thereof. In some embodiments, the second barrier layer 170 is formed by nitriding the molybdenum silicide (MoSi) layer 160 using ammonia (NH3). In some embodiments, the second barrier layer 170 is formed by nitriding the molybdenum silicide (MoSi) layer 160 with plasma. In some embodiments, the plasma treatment includes nitrogen (N2) plasma treatment. In some embodiments, the second barrier layer 170 comprises a metal nitride, a PVD metal, or a combination thereof.

[0064] refer to Figure 1F The first opening 106 above the n-transistor 102 and the second opening 108 above the p-transistor 104 are each independently filled with interstitial materials 180 and 182, respectively. In one or more embodiments, the interstitial material 180 is substantially free of voids or seams. The interstitial materials 180 and 182 may independently comprise any suitable interstitial material known to those skilled in the art. In one or more embodiments, the interstitial materials 180 and 182 independently comprise one or more of tungsten (W), molybdenum (Mo), cobalt (Co), and ruthenium (Ru). In one or more embodiments, the interstitial material 180 in the first opening 106 above the n-transistor 102 is the same as the interstitial material 182 in the second opening 108 above the p-transistor 104. In one or more embodiments, the interstitial material 180 in the first opening 106 above the n-transistor 102 is different from the interstitial material 182 in the second opening 108 above the p-transistor 104.

[0065] The gap-filling process may include any suitable gap-filling process known to those skilled in the art. In one or more embodiments, the gap-filling process includes exposing the semiconductor structure 100 to a metal precursor and a reactant. In some embodiments, the metal precursor includes one or more of molybdenum precursors, tungsten precursors, cobalt precursors, and ruthenium precursors.

[0066] In some embodiments, the gap filling process is a bottom-up gap filling process. In other embodiments, the gap filling process includes a conformal gap filling process.

[0067] Figures 2A to 2GA semiconductor structure 200 is shown. The semiconductor structure 200 includes an n-transistor 202 and a p-transistor 204. Each of the n-transistor 202 and the p-transistor 204 includes a dielectric material 210, a source / drain material 220, and a substrate 230.

[0068] In one or more embodiments, the dielectric material 210 may comprise any suitable material known to those skilled in the art. In some embodiments, the dielectric material 210 comprises one or more of silicon, silicon oxide, silicon nitride, silicon carbide, and low-k dielectrics. In some embodiments, the dielectric material 210 comprises silicon oxide (SiO2).

[0069] In some embodiments, n-transistor 202 and p-transistor 204 include source and drain contacts. In one or more embodiments, the source / drain material 220 may have more than one layer. In some embodiments, the source / drain material 220 includes a silicon layer (e.g., SiGe, SiP, etc.) having a doped epitaxial layer, a second silicide layer that may contain nickel (Ni), titanium (Ti), aluminum (Al), etc., and a third or top layer that may be a metal such as, but not limited to, cobalt, tungsten, ruthenium, etc.

[0070] In one or more embodiments, the source / drain material 220 of the n-transistor 202 comprises silicon (Si) doped with phosphorus (P). In one or more embodiments, the source / drain material 220 of the n-transistor 202 has a band gap in the range of about 1.0 eV to about 1.2 eV.

[0071] In one or more embodiments, the source / drain material 220 of the p transistor 204 comprises boron (B)-doped silicon germanium (SiGe). In one or more embodiments, the source / drain material 220 of the p transistor 204 has a band gap in the range of about 0.5 eV to about 1.0 eV.

[0072] refer to Figures 2A-2B A first opening 206 is present above the n-transistor 202, and a second opening 208 is present above the p-transistor 204. The first opening 206 and the second opening 208 may have any suitable aspect ratio (the ratio of the depth of the opening to the width of the opening). In one or more embodiments, the first opening 206 and the second opening 208 may independently have an aspect ratio in the range of 3:1 to 15:1, 6:1 to 15:1, 9:1 to 15:1, 12:1 to 15:1, or greater than 10:1.

[0073] refer to Figure 2B A titanium silicide (TiSi) layer 240 is deposited on the n-transistor 202. The titanium silicide (TiSi) layer 240 can have any suitable thickness. In some embodiments, the thickness of the titanium silicide (TiSi) layer 240 is... To date Within the range, or about To date Within the range, or about to approximately Within the range, or about to approximately Within the range. In one or more embodiments, the titanium silicide (TiSi) layer 240 has approximately The thickness.

[0074] refer to Figure 2C An optional first barrier layer 250 is formed on the titanium silicide (TiSi) layer 240 on the n-transistor 202. In one or more embodiments, the optional first barrier layer 250 comprises a metal. In one or more embodiments, the optional first barrier layer 250 comprises a metal nitride. In one or more embodiments, the optional first barrier layer 250 comprises one or more of titanium nitride (TiN), tantalum nitride (TaN), tungsten nitride (WN), and molybdenum nitride (MoN).

[0075] In one or more embodiments, the first opening 206 above the n-transistor 202 is filled with a first interstitial material 280. In one or more embodiments, the first interstitial material 280 is substantially free of voids or seams. In one or more embodiments, the first interstitial material 280 comprises one or more of tungsten (W), molybdenum (Mo), cobalt (Co), and ruthenium (Ru).

[0076] The gap-filling process may include any suitable gap-filling process known to those skilled in the art. In one or more embodiments, the gap-filling process includes exposing the semiconductor structure 200 to a metal precursor and a reactant. In some embodiments, the metal precursor includes one or more of molybdenum precursors, tungsten precursors, cobalt precursors, and ruthenium precursors.

[0077] refer to Figure 2DA mask layer 270 is formed on the top surfaces of the n-transistor 202 and the p-transistor 204. In one or more embodiments, the mask layer 270 comprises one or more of a hard mask layer 272 and a photoresist layer 274. The hard mask layer 272 may contain any suitable material known to those skilled in the art. In one or more embodiments, the hard mask layer 272 comprises silicon dioxide (SiO2). The photoresist layer 274 may contain any suitable material known to those skilled in the art. As those skilled in the art will recognize, although the photoresist layer 274 is shown as not present in the p-transistor, this is merely for ease of drawing. Those skilled in the art will understand that the hard mask layer 272 and the photoresist layer 274 are formed on the top surfaces of both the n-transistor 202 and the p-transistor 204. The process of forming the second opening 208 removes the photoresist layer 274. In one or more embodiments, the second opening 208 is formed over the p-transistor 204. The second opening 208 may be formed by any suitable process known to those skilled in the art. In one or more embodiments, the second opening 208 is formed by etching.

[0078] The second opening 208 may have any suitable aspect ratio. In one or more embodiments, the second opening may have an aspect ratio in the range of 3:1 to 15:1, 6:1 to 15:1, 9:1 to 15:1, 12:1 to 15:1, or greater than 10:1.

[0079] refer to Figure 2E The photoresist layer 280 is removed from the mask layer 270 of the n-transistor 202. The photoresist layer 280 can be removed by any suitable method known to those skilled in the art. In one or more embodiments, the photoresist layer 280 is removed by stripping.

[0080] refer to Figure 2F A molybdenum silicide (MoSi) layer 245 is selectively formed on the source / drain material 220 of the p-transistor 204. The molybdenum silicide (MoSi) layer 245 can be formed by any suitable process known to those skilled in the art. The molybdenum silicide (MoSi) layer 245 can have any suitable thickness. In some embodiments, the thickness of the molybdenum silicide (MoSi) layer 245 is... To date Within the range, or about To date Within the range, or about To date Within the range, or about To date Within the range. In one or more embodiments, the molybdenum silicide (MoSi) layer 245 has approximately The thickness.

[0081] The molybdenum silicide (MoSi) layer 245 can be formed using any suitable process known to those skilled in the art. In one or more embodiments, structure 200 is first cleaned to remove oxides from the surface. In some embodiments, the oxides are native oxides. In some embodiments, cleaning the surface forms a substantially oxide-free surface. As used in this way, the term "substantially oxide-free" means that the surface contains less than or equal to 5%, 2%, 1%, or 0.5% oxygen atoms. In one or more embodiments, anisotropic etching is used to remove oxides from the surface.

[0082] In one or more embodiments, a metal film is selectively formed on the source / drain material 220 to form the molybdenum silicide (MoSi) layer 245. In some embodiments, the semiconductor structure 200 is exposed to the metal precursor and reactants. The metal film can be deposited by an ALD deposition process, a CVD deposition process, or a combination thereof. In some embodiments, the metal film comprises a molybdenum silicide film.

[0083] In one or more embodiments, the metal precursor comprises a molybdenum precursor. In some embodiments, the molybdenum precursor comprises molybdenum halide. In some embodiments, the molybdenum halide comprises molybdenum fluoride, molybdenum chloride, or a combination thereof. In a particular embodiment, the molybdenum precursor comprises molybdenum fluoride. In other particular embodiments, the molybdenum precursor comprises molybdenum chloride. In one or more embodiments, a carrier gas is used to flow the precursor through a surface. In some embodiments, the carrier gas flows through an ampoule containing the precursor. In some embodiments, the carrier gas is an inert gas. In some embodiments, the inert gas comprises one or more of N2, Ar, and He.

[0084] In one or more embodiments, the reactants comprise an oxidizing agent, a reducing agent, or a combination thereof. In some embodiments, the reactants comprise hydrogen (H2), ammonia (NH3), silane, polysilane, or a combination thereof. In some embodiments, the silane is selected from one or more of disilane, trisilane, tetrasilane, higher silanes, and substituted silanes. In a particular embodiment, the reactants comprise silane to form a molybdenum silicide (MoSi) layer 245. In one or more embodiments, a carrier gas is used to flow the reactants through the surface. In some embodiments, the carrier gas is an inert gas. In some embodiments, the inert gas comprises one or more of N2, Ar, and He. In other embodiments, the reactant gas can flow continuously and the flow of the molybdenum precursor into the chamber can be opened and closed.

[0085] refer to Figure 2G The mask layer 270 formed on the top surfaces of each of the n-transistor 202 and the p-transistor 204 is removed. The mask layer 270 can be removed by any suitable method known to those skilled in the art. In some embodiments, the mask layer 270 is removed by etching or planarization.

[0086] In one or more embodiments, the second opening 208 above the p-transistor 204 is filled with a second gap-filling material 282. In one or more embodiments, the second gap-filling material 282 is substantially free of voids or seams. The first gap-filling material 280 and the second gap-filling material 282 may independently comprise any suitable gap-filling material known to those skilled in the art. In one or more embodiments, the second gap-filling material 282 comprises tungsten (W), molybdenum (Mo), or cobalt (C). o It may contain one or more of ruthenium (Ru) and arsenic (Ru). In one or more embodiments, the interstitial material 280 above the n transistor 202 is the same as the interstitial material 282 above the p transistor 204. In one or more embodiments, the interstitial material 280 is different from the interstitial material 282.

[0087] The gap-filling process may include any suitable gap-filling process known to those skilled in the art. In one or more embodiments, the gap-filling process includes exposing the semiconductor structure 200 to a metal precursor and a reactant. In some embodiments, the metal precursor includes one or more of molybdenum precursors, tungsten precursors, cobalt precursors, and ruthenium precursors.

[0088] In some embodiments, the gap filling process is a bottom-up gap filling process. In other embodiments, the gap filling process includes a conformal gap filling process.

[0089] Figure 3 A process flow diagram of method 300 for forming a semiconductor structure is shown. Figure 3 Showing the formation Figures 1A-1F and Figures 2A-2G Methods for any semiconductor structure shown in one or more embodiments.

[0090] In one or more embodiments, method 300 for forming a semiconductor structure includes, in operation 310, patterning a substrate to form a first opening and a second opening, the substrate including an n-transistor and a p-transistor, the first opening being over the n-transistor and the second opening being over the p-transistor. In operation 320, method 300 includes pre-cleaning the substrate. In operation 330, method 300 includes depositing titanium silicide (TiSi) layers on the n-transistor and p-transistor by plasma-enhanced chemical vapor deposition (PECVD). In operation 340, method 300 includes, as appropriate, depositing a first barrier layer on the titanium silicide (TiSi) layer and selectively removing the first barrier layer from the p-transistor. In operation 350, method 300 includes selectively forming a molybdenum silicide (MoSi) layer on the titanium silicide (TiSi) layer on the n-transistor and p-transistor. In operation 360, method 300 includes forming a second barrier layer on the molybdenum silicide (MoSi) layer. In operation 370, method 300 includes annealing the semiconductor structure.

[0091] In operation 310, method 300 includes patterning a substrate to form at least one of a first opening and a second opening. In one or more embodiments, the patterned substrate includes one or more patterning techniques known to those skilled in the art of microelectronics manufacturing.

[0092] In operation 320, method 300 includes pre-cleaning the substrate. In one or more embodiments, the pre-cleaning process is maintained under vacuum to ensure that no oxides are introduced / formed on the substrate surface during method 300. In some embodiments, the pre-cleaned substrate (or substrate surface) removes oxides from the surface. In some embodiments, the oxides are native oxides. In some embodiments, the cleaned surface forms a substantially oxide-free surface. As used in this way, the term "substantially oxide-free" means that the surface contains less than or equal to 5%, 2%, 1%, or 0.5% oxygen atoms. In one or more embodiments, anisotropic etching is used to remove oxides from the surface. In one or more embodiments, anisotropic etching removes more oxides from the surface of the source / drain material than from the dielectric material. In one or more embodiments, the pre-cleaned surface forms a substantially oxide-free source / drain material.

[0093] In operation 330, method 300 includes depositing titanium silicide (TiSi) layers on n-transistors and p-transistors by plasma-enhanced chemical vapor deposition (PECVD). In one or more embodiments, after depositing the titanium silicide (TiSi) layers on the n-transistors and p-transistors, a rapid thermal process (RTP) is performed. In one or more embodiments, the rapid thermal process (RTP) includes heating the titanium silicide (TiSi) layer to a temperature in the range of about 500°C to about 700°C. In one or more embodiments, the rapid thermal process (RTP) is performed for about 1 minute. In one or more embodiments, the rapid thermal process (RTP) removes unreacted metal from the titanium silicide (TiSi) layer.

[0094] In operation 340, method 300 may include, as appropriate, depositing a first barrier layer on the titanium silicide (TiSi) layer on the n-transistor and selectively removing the first barrier layer from the p-transistor. In one or more embodiments, selectively removing the first barrier layer from the p-transistor allows the molybdenum silicide (MoSi) layer on the p-transistor to form an ohmic contact with the titanium silicide (TiSi) layer on the p-transistor.

[0095] In some embodiments, the titanium silicide (TiSi) layers on both the n-transistor and p-transistor are protected from oxide formation by a first barrier layer. The first barrier layer can be formed by any process known to those skilled in the art. In one or more embodiments, at operation 340, the first barrier layer is formed by an atomic layer deposition (ALD) process. In one or more embodiments, at operation 340, the first barrier layer is formed by a physical vapor deposition (PVD) process.

[0096] In some embodiments, the first barrier layer is formed on a titanium silicide (TiSi) layer. In some embodiments, the titanium silicide (TiSi) layer is treated to form the first barrier layer. In some embodiments, the first barrier layer is formed by nitriding the titanium silicide (TiSi) layer. In some embodiments, the first barrier layer is formed by nitriding the titanium silicide (TiSi) layer using ammonia (NH3). In some embodiments, the first barrier layer is formed by nitriding the titanium silicide (TiSi) layer with plasma. In some embodiments, the plasma treatment includes nitrogen (N2) plasma treatment.

[0097] In one or more embodiments, a titanium silicon nitride (TiSiN) layer is formed by nitriding a titanium silicon nitride (TiSi) layer to form a first barrier layer. In one or more embodiments, the semiconductor structure having the titanium silicon nitride (TiSiN) layer has a lower Schottky barrier height than a semiconductor structure without the titanium silicon nitride (TiSiN) layer. In one or more embodiments, the semiconductor structure having the titanium silicon nitride (TiSiN) layer has a Schottky barrier height in the range of about 0.50 eV to about 0.55 eV. In one or more embodiments, the semiconductor structure without the titanium silicon nitride (TiSiN) layer has a Schottky barrier height in the range of about 0.6 eV to about 0.7 eV.

[0098] In some embodiments, operation 350, method 300 includes selectively forming a molybdenum silicide (MoSi) layer on a titanium silicide (TiSi) layer on an n-transistor and a p-transistor. In one or more embodiments, the molybdenum silicide (MoSi) layer is formed on a boron (B)-doped silicon-germanium (SiGe) substrate of the p-transistor. In one or more embodiments, after selectively forming the molybdenum silicide (MoSi) layer on the p-transistor, a rapid thermal processing (RTP) is performed. In one or more embodiments, the rapid thermal processing (RTP) includes heating the molybdenum silicide (MoSi) layer to a temperature in the range of about 500°C to about 700°C. In one or more embodiments, the rapid thermal processing (RTP) is performed for about 1 minute. In one or more embodiments, the rapid thermal processing (RTP) removes unreacted metal from the molybdenum silicide (MoSi) layer.

[0099] In another aspect of this disclosure, the method 300 for forming a semiconductor structure includes reducing the contact resistance of the semiconductor structure. In some embodiments, during operation 370, the semiconductor structure is annealed to reduce the contact resistance. In one or more embodiments, annealing the semiconductor structure produces a smooth surface. In one or more embodiments, during operation 370, annealing the semiconductor structure forms one or more ohmic and pseudo-ohmic contacts on the n-transistor and the p-transistor.

[0100] The semiconductor structure can be annealed using any process known to those skilled in the art. In some embodiments, the semiconductor structure is annealed by rapid thermal processing (RTP). In one or more embodiments, rapid thermal processing (RTP) involves annealing the semiconductor structure to a temperature in the range of about 500°C to about 700°C. In one or more embodiments, rapid thermal processing (RTP) involves annealing the semiconductor structure to a temperature of about 600°C.

[0101] In some embodiments, the annealed semiconductor structure has a root mean square (RMS) roughness in the range of 4% to less than 30%, 4% to less than 20%, 4% to less than 10%, 10% to less than 30%, 10% to less than 20%, or 20% to less than 30%.

[0102] In some embodiments, method 300 includes performing a gap-filling process. In one or more embodiments, the gap-filling process includes independently filling a first opening on the n-transistor and a second opening on the p-transistor. In some embodiments, the gap-filling process is a bottom-up gap-filling process. In other embodiments, the gap-filling process includes a conformal gap-filling process. In one or more embodiments, method 300 includes filling the first opening on the n-transistor with a first gap-filling material and filling the second opening on the p-transistor with a second gap-filling material. In one or more embodiments, each of the first and second gap-filling materials is substantially free of voids or seams. In one or more embodiments, each of the first and second gap-filling materials comprises one or more of tungsten (W), molybdenum (Mo), cobalt (Co), and ruthenium (Ru).

[0103] In one or more embodiments, method 300 includes optional post-processing operations.

[0104] Figure 4 A process flow diagram of method 400 for forming a semiconductor structure is shown. Figure 4 Showing the formation Figures 1A-1F and Figures 2A-2G Methods for any semiconductor structure shown in one or more embodiments.

[0105] In some embodiments, method 400 of forming a semiconductor structure includes, in operation 410, patterning a substrate to form a first opening, the substrate including an n-transistor and a p-transistor, the first opening being over the n-transistor. In operation 420, method 400 includes pre-cleaning the substrate. In operation 430, method 400 includes depositing a titanium silicide (TiSi) layer on the n-transistor by plasma-enhanced chemical vapor deposition (PECVD). In operation 430, method 400 may include forming a barrier layer on the titanium silicide (TiSi) layer on the n-transistor. In operation 440, method 400 includes filling the first opening with a first interstitial material. In operation 450, method 400 includes forming a mask layer on the top surface of the n-transistor. In operation 460, method 400 includes patterning the substrate to form a second opening over the p-transistor. In one or more embodiments, method 400 may include depositing a first barrier layer on the titanium silicide (TiSi) layer and selectively removing the first barrier layer from the p-transistor. In operation 470, method 400 includes selectively forming a molybdenum silicide (MoSi) layer on the p-transistor. In operation 480, method 400 includes annealing the semiconductor structure. In operation 490, method 400 includes filling the second opening with a second interstitial material.

[0106] In operation 410, method 400 includes patterning a substrate to form a first opening over the n transistors. In one or more embodiments, the patterned substrate includes one or more patterning techniques known to those skilled in the art of microelectronics manufacturing.

[0107] In operation 420, method 400 includes pre-cleaning the substrate. In one or more embodiments, the pre-cleaning process is maintained under vacuum to ensure that no oxides are introduced / formed on the substrate surface during method 400. In some embodiments, the pre-cleaned substrate (or substrate surface) removes oxides from the surface. In some embodiments, the oxides are native oxides. In some embodiments, the cleaned surface forms a substantially oxide-free surface. As used in this way, the term "substantially oxide-free" means that the surface contains less than or equal to 5%, 2%, 1%, or 0.5% oxygen atoms. In one or more embodiments, anisotropic etching is used to remove oxides from the surface. In one or more embodiments, anisotropic etching removes more oxides from the surface of the source / drain material than from the dielectric material. In one or more embodiments, the pre-cleaned surface forms a substantially oxide-free source / drain material.

[0108] In operation 430, method 400 includes depositing a titanium silicide (TiSi) layer on an n-transistor by plasma-enhanced chemical vapor deposition (PECVD). In one or more embodiments, after depositing the TiSi layer on the n-transistor, a rapid thermal processing (RTP) is performed. In one or more embodiments, the rapid thermal processing (RTP) involves heating the TiSi layer to a temperature in the range of about 500°C to about 700°C. In one or more embodiments, the rapid thermal processing (RTP) is performed for about 1 minute. In one or more embodiments, the rapid thermal processing (RTP) removes unreacted metal from the TiSi layer.

[0109] In operation 435, method 400 may include depositing a first barrier layer on a titanium silicide (TiSi) layer on the n-transistor. In some embodiments, the titanium silicide (TiSi) layer on the n-transistor is protected from oxide formation by the first barrier layer. The first barrier layer may be formed by any process known to those skilled in the art. In one or more embodiments, in operation 435, the first barrier layer is formed by an atomic layer deposition (ALD) process. In one or more embodiments, in operation 435, the first barrier layer is formed by a physical vapor deposition (PVD) process.

[0110] In some embodiments, the first barrier layer is formed on a titanium silicide (TiSi) layer. In some embodiments, the titanium silicide (TiSi) layer is treated to form the first barrier layer. In some embodiments, the first barrier layer is formed by nitriding the titanium silicide (TiSi) layer. In some embodiments, the first barrier layer is formed by nitriding the titanium silicide (TiSi) layer using ammonia (NH3). In some embodiments, the first barrier layer is formed by nitriding the titanium silicide (TiSi) layer with plasma. In some embodiments, the plasma treatment includes nitrogen (N2) plasma treatment.

[0111] In one or more embodiments, a titanium silicon nitride (TiSiN) layer is formed by nitriding a titanium silicon nitride (TiSi) layer to form a first barrier layer. In one or more embodiments, the semiconductor structure having the titanium silicon nitride (TiSiN) layer has a lower Schottky barrier height than a semiconductor structure without the titanium silicon nitride (TiSiN) layer. In one or more embodiments, the semiconductor structure having the titanium silicon nitride (TiSiN) layer has a Schottky barrier height in the range of about 0.50 eV to about 0.55 eV. In one or more embodiments, the semiconductor structure without the titanium silicon nitride (TiSiN) layer has a Schottky barrier height in the range of about 0.6 eV to about 0.7 eV.

[0112] In operation 440, method 400 includes filling a first opening with a first gap-filling material. In some embodiments, filling the first opening includes a bottom-up gap-filling process. In other embodiments, filling the first opening includes a conformal gap-filling process. In one or more embodiments, the first gap-filling material is substantially free of voids or seams. In one or more embodiments, the first gap-filling material includes one or more of tungsten (W), molybdenum (Mo), cobalt (Co), and ruthenium (Ru).

[0113] In some embodiments, operation 450, method 400 includes forming a mask layer on the top surface of the n-transistor. In one or more embodiments, the mask layer comprises one or more of a hard mask layer and a photoresist layer. The hard mask layer may contain any suitable material known to those skilled in the art. In one or more embodiments, the hard mask layer comprises silicon dioxide (SiO2). The photoresist layer may contain any suitable material known to those skilled in the art.

[0114] In operation 460, method 400 includes patterning a substrate to form a second opening over the p-transistor. In one or more embodiments, the patterned substrate includes one or more patterning techniques known to those skilled in the art of microelectronics manufacturing.

[0115] In operation 470, method 400 includes selectively forming a molybdenum silicide (MoSi) layer on a titanium silicide (TiSi) layer on a p-transistor. In one or more embodiments, after selectively forming the MoSi layer on the p-transistor, a rapid thermal processing (RTP) is performed. In one or more embodiments, the rapid thermal processing (RTP) includes heating the MoSi layer to a temperature in the range of about 500°C to about 700°C. In one or more embodiments, the rapid thermal processing (RTP) is performed for about 1 minute. In one or more embodiments, the rapid thermal processing (RTP) removes unreacted metal from the MoSi layer.

[0116] In another aspect of this disclosure, the method 400 for forming a semiconductor structure includes reducing the contact resistance of the semiconductor structure. In some embodiments, during operation 480, the semiconductor structure is annealed to reduce the contact resistance. In one or more embodiments, annealing the semiconductor structure produces a smooth surface. In one or more embodiments, during operation 480, annealing the semiconductor structure forms one or more ohmic and pseudo-ohmic contacts on the n-transistor and the p-transistor.

[0117] The semiconductor structure can be annealed using any process known to those skilled in the art. In some embodiments, the semiconductor structure is annealed by rapid thermal processing (RTP). In one or more embodiments, rapid thermal processing (RTP) involves annealing the semiconductor structure to a temperature in the range of about 500°C to about 700°C. In one or more embodiments, rapid thermal processing (RTP) involves annealing the semiconductor structure to a temperature of about 600°C.

[0118] In some embodiments, the annealed semiconductor structure has a root mean square (RMS) roughness in the range of 4% to less than 30%, 4% to less than 20%, 4% to less than 10%, 10% to less than 30%, 10% to less than 20%, or 20% to less than 30%.

[0119] In operation 490, method 400 includes filling the second opening with a second gap-filling material. In some embodiments, filling the second opening includes a bottom-up gap-filling process. In other embodiments, filling the second opening includes a conformal gap-filling process. In one or more embodiments, the second gap-filling material is substantially free of voids or seams. In one or more embodiments, the second gap-filling material includes one or more of tungsten (W), molybdenum (Mo), cobalt (Co), and ruthenium (Ru).

[0120] In one or more embodiments, method 400 includes optional post-processing operations.

[0121] Spatial terms such as “below,” “under,” “below,” “above,” and “above” may be used herein to facilitate description of the relationship between one element or feature and another, as illustrated in the figures. It should be understood that spatial terms are intended to cover different orientations of the device in use or operation other than those depicted in the figures. For example, if the device in the figures is flipped, an element described as “below” or “under” other elements or features would subsequently be oriented “above” other elements or features. Thus, the exemplary term “below” can cover both above and below orientations. The device may be oriented in other ways (rotated 90 degrees or in other orientations) and the spatial descriptors used herein shall be interpreted accordingly.

[0122] In the context of describing the materials and methods discussed herein (particularly in the context of the following claims), the terms “a / an” and “the”, and similar designations, shall be construed as encompassing both the singular and plural, unless otherwise stated herein or clearly contradicted by the context. Unless otherwise stated herein, the enumeration of numerical ranges herein is intended only as a shorthand method for individually referring to each individual value falling within that range, and each individual value is incorporated into the specification as if it were individually enumerated herein. Unless otherwise stated herein or clearly contradicted by the context, all methods described herein may be performed in any suitable order. The use of any and all instances or exemplary language (e.g., “such as”) provided herein is intended only to better elucidate the materials and methods and does not constitute a limitation on the scope, unless otherwise stated. No language in the specification should be construed as indicating that any unclaimed element is essential to the practice of the disclosed materials and methods.

[0123] Throughout this specification, references to "one embodiment," "some embodiments," "one or more embodiments," or "an embodiment" mean that a particular feature, structure, material, or characteristic described in connection with an embodiment is included in at least one embodiment of this disclosure. Therefore, the appearance of phrases such as "in one or more embodiments," "in some embodiments," "in one embodiment," or "in one embodiment" in various places throughout this specification does not necessarily represent the same embodiment of this disclosure. In one or more embodiments, the particular feature, structure, material, or characteristic is combined in any suitable manner.

[0124] Although the disclosure herein has been described with reference to specific embodiments, it should be understood that these embodiments are merely illustrative of the principles and applications of this disclosure. It will be apparent to those skilled in the art that various modifications and variations can be made to the methods and apparatus of this disclosure without departing from the spirit and scope of this disclosure. Therefore, this disclosure is intended to include modifications and variations within the scope of the appended claims and their equivalents.

Claims

1. A method for forming a semiconductor structure, the method comprising: A patterned substrate is used to form a first opening and a second opening, the substrate including an n transistor and a p transistor, the first opening being on the n transistor and the second opening being on the p transistor; Pre-clean the substrate; Titanium silicide (TiSi) layers are deposited on the n transistor and the p transistor by plasma-enhanced chemical vapor deposition (PECVD); A first barrier layer is deposited on the titanium silicide (TiSi) layer, and the first barrier layer is selectively removed from the p transistor; A molybdenum silicide (MoSi) layer is formed on the titanium silicide (TiSi) layer on the n transistor and the p transistor; A second barrier layer is formed on the molybdenum silicide (MoSi) layer; and The semiconductor structure is then annealed.

2. The method of claim 1, wherein the n-transistor comprises silicon (Si) doped with phosphorus (P), and the p-transistor comprises silicon germanium (SiGe) doped with boron (B).

3. The method of claim 1, wherein the first barrier layer comprises one or more of titanium nitride (TiN), tantalum nitride (TaN), tungsten nitride (WN), and molybdenum nitride (MoN).

4. The method of claim 3, wherein the first barrier layer is formed by one or more of atomic layer deposition (ALD) or physical vapor deposition (PVD) processes.

5. The method of claim 1, wherein the second barrier layer comprises molybdenum nitride (MoN), molybdenum silicide nitride (MoSi), and a PVD metal film.

6. The method of claim 1, further comprising: independently filling the first opening and the second opening with a gap-filling material.

7. The method of claim 6, wherein the gap-filling material is substantially free of voids or seams.

8. The method of claim 6, wherein the interstitial material comprises one or more of tungsten (W), molybdenum (Mo), cobalt (Co) and ruthenium (Ru).

9. The method of claim 1, wherein the step of annealing the semiconductor structure forms one or more of ohmic contacts and pseudo-ohmic contacts on the n transistor and the p transistor.

10. The method of claim 1, wherein the titanium silicide (TiSi) layer on the n-transistor has a Schottky barrier height in the range of about 0.4 eV to about 0.55 eV.

11. A semiconductor structure, the semiconductor structure comprising: The n transistor and the p transistor have a first opening on the n transistor and a second opening on the p transistor; Titanium silicide (TiSi) layers on the n transistor and the p transistor; A molybdenum silicide (MoSi) layer on the titanium silicide (TiSi) layer on each of the n transistors and the p transistors; A barrier layer on the titanium silicide (TiSi) layer on the n transistor and between the titanium silicide (TiSi) layer and the molybdenum silicide (MoSi) layer; and A first gap-filling material that fills the first opening above the n transistor and a second gap-filling material that fills the second opening above the p transistor.

12. The semiconductor structure of claim 11, wherein the barrier layer comprises one or more of titanium nitride (TiN), tantalum nitride (TaN), tungsten nitride (WN), and molybdenum nitride (MoN).

Citation Information

Patent Citations

  • Selective dual siliconide production using a maskless manufacturing process

    DE102019118061A1

  • Shared contact trench comprising dual silicide layers and dual epitaxial layers for source / drain layers of NFET and PFET devices

    US20200058563A1