A method for preparing TC21 titanium alloy super-large bar

Through the processes of open forging in the β single-phase zone, intermediate forging and forming forging in the α+β two-phase zone, combined with 'three-dimensional commutation' and octagonal forging, the problem of insufficient specifications of the existing TC21 titanium alloy rods was solved, and the diameter TC21 titanium alloy oversized rods with a unit weight of 500mm to 600mm and a unit weight of more than 4 tons meet the needs of the aerospace industry and improve the structural uniformity and performance of the product.

CN117619928BActive Publication Date: 2024-10-25西部超导材料科技股份有限公司
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202311706073.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-13
Publication Date
2024-10-25
Estimated Expiration
2043-12-13

AI Technical Summary

Technical Problem

The current maximum specifications of TC21 titanium alloy rods cannot meet the development needs of the aerospace industry. Especially in the context of large-scale and integrated aircraft structural design, it is impossible to prepare ultra-large rods with a diameter of more than 400mm and a unit weight of more than 2 tons.

Method used

It adopts the process of 3 fires of billet forging in the β single-phase zone, 3 fires of intermediate forging in the α+β two-phase zone and 2 fires of forming forging in the α+β two-phase zone, combined with the 'three-dimensional commutation' and the eight-way forging method. Transform the as-cast columnar grains, improve the 'dead zone' of forging deformation, improve the uniformity of the bar structure, and prepare super-large TC21 titanium alloy bars with a diameter of 500mm to 600mm and a single weight of more than 4 tons.

Benefits of technology

It significantly improves the organizational uniformity and performance of the bar, meets the large-scale and integrated design requirements for the main load-bearing structural components of new aircraft, and ensures that the organization and performance of the product comply with aviation standards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117619928B_ABST
    Figure CN117619928B_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a TC21 titanium alloy super-large-size bar, comprising the following steps: step one, β single-phase region blanking forging three times: the first time is subjected to upsetting and drawing forging to obtain an intermediate blank ingot with a square cross section; the second and third times are subjected to "three-dimensional reversing" upsetting and drawing forging to obtain an intermediate blank ingot with a square cross section and a grain size of 3.5 mm to 5.5 mm; step two, α+β two-phase region intermediate forging three times: in each fire, the intermediate blank ingot is first upset and then drawn and forged into a blank with a square cross section, and finally drawn and forged into an intermediate blank with an octagonal cross section; step three, α+β two-phase region forming forging two times: in the first fire, the intermediate blank is drawn and forged into a blank with a circular cross section, and in the second fire, the circular blank is rounded into a bar blank with a circular cross section and a size that meets requirements. The present invention improves the uniformity of the rod structure, and can prepare TC21 titanium alloy super-large-size rods with a diameter of 500 mm to 600 mm and a single weight of more than 4 tons, the structure and performance of which meet the requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nonferrous metal processing technology, and specifically relates to a method for preparing a TC21 titanium alloy super-large specification bar. Background Art

[0002] TC21 titanium alloy is a new type of high-strength, high-toughness, and high-damage tolerance titanium alloy independently developed by my country with independent intellectual property rights. It belongs to the Ti-Al-Sn-Zr-Mo-Cr-Nb (-Ni-Si) two-phase titanium alloy with excellent strength, plasticity, fracture toughness and low crack growth rate. It is widely used in the aerospace industry, especially in the field of aircraft structural parts, such as large aircraft frames, beams and other key load-bearing components.

[0003] Nowadays, with the concept of large-scale and integrated aircraft structure design, there is a demand for larger specifications of TC21 titanium alloy bars. At present, the maximum specification of TC21 titanium alloy bars is Φ≤400mm, and the unit weight is less than 2 tons, which cannot meet the development needs of the aerospace industry. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a super-large-size TC21 titanium alloy bar. The present invention improves the uniformity of the bar structure and can prepare super-large-size TC21 titanium alloy bars with a diameter of 500 mm to 600 mm and a unit weight of more than 4 tons, which meet the requirements of structure and performance.

[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0006] A method for preparing a TC21 titanium alloy super-large bar comprises the following steps:

[0007] Step 1: Forging in β single phase region for 3 times:

[0008] In the first fire, the TC21 titanium alloy ingot is subjected to upsetting and drawing forging to obtain an intermediate billet ingot with a square cross section; in the second and third fires, "three-dimensional reversing" upsetting and drawing forging are performed to obtain an intermediate billet ingot with a square cross section and a grain size of 3.5 mm to 5.5 mm;

[0009] Step 2: Forging 3 times in the middle of the α+β two-phase region:

[0010] In each firing, the intermediate billet ingot is firstly upset forged, then drawn and forged into a billet with a square cross section, and finally further drawn and lengthened into an intermediate billet with an octagonal cross section;

[0011] Step 3: α+β two-phase zone forming forging 2 times:

[0012] In the first fire, the intermediate billet is stretched and forged into a billet with a circular cross section. In the second fire, the circular billet is rounded into a rod billet with a circular cross section and dimensions that meet the requirements.

[0013] Preferably, in step 1, the specification of the TC21 titanium alloy ingot is Φ690mm-Φ720mm, and the unit weight is greater than 5 tons.

[0014] Preferably, in step 1, the first heating temperature is Tβ+(150-250)°C, the holding time is 450min-600min, and the cumulative forging ratio is 5.5-7.5.

[0015] Preferably, in step 1, the heating temperature for the second to third firings is Tβ+(50-150)°C, the holding time is 450min-600min, and the cumulative forging ratio of the two firings is controlled at 12-14.

[0016] Preferably, in the step 1, the "three-dimensional reversal" means that the intermediate billet ingot of each fire is first subjected to upsetting forging along the axial direction and then to stretching forging along the radial direction.

[0017] Preferably, in the step 2, the heating temperature of each fire is Tβ-(20-50)°C, the holding time is 360min-540min, and the cumulative forging ratio of the three fires is 12-18.

[0018] Preferably, in step three, the first heating temperature is Tβ-(30-60)°C, the holding time is 320min-450min, and after being taken out of the furnace, the billet is drawn and forged into a round billet with a diameter of Φ530mm-Φ630mm.

[0019] Preferably, the drawing deformation is controlled at 30% to 40%, and the final forging temperature is not less than 750°C.

[0020] Preferably, in the step three, the second heating temperature is Tβ-(40~70)℃, the holding time is 300min~420min, and after being taken out of the furnace, the rod is rounded into a rod blank with a diameter of Φ510mm~Φ610mm, and the rod blank is processed to prepare TC21 titanium alloy super-large-size rods with a diameter of Ф500mm~Ф600mm and a single weight greater than 4 tons.

[0021] Preferably, the rounding deformation is controlled at 5% to 15%, and the final forging temperature is not less than 700°C.

[0022] The beneficial effects of the present invention are:

[0023] This preparation method is based on the evolution characteristics of TC21 titanium alloy plastic processing organization. It adopts the process of single-phase area blank forging → two-phase area intermediate forging → forming forging, combined with "three-dimensional reversing" and eight-way forging methods, which significantly refines the cast columnar grains, effectively improves the forging deformation "dead zone", and improves the uniformity of the bar organization. It can prepare TC21 titanium alloy super-large-size bars with a diameter of Ф500mm to Ф600mm and a single weight of more than 4 tons, which meet the organization and performance requirements. It meets the large-scale and integrated design requirements of the main load-bearing structural components of new aircraft. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a low-magnification microstructure diagram of the head, middle and tail cross-sections of the TC21 titanium alloy Φ500mm super-large specification bar prepared in Example 1 of the present invention, wherein Figure a is a low-magnification microstructure diagram of the cross-section of the head of the bar, Figure b is a low-magnification microstructure diagram of the cross-section of the middle of the bar, and Figure c is a low-magnification microstructure diagram of the cross-section of the tail of the bar.

[0025] Figure 2 It is a 500× high-magnification microstructure diagram of the head, middle and tail cross-sections R / 2 of the TC21 titanium alloy Φ500mm super-large specification bar prepared in Example 1 of the present invention, wherein Figure a is the high-magnification microstructure at the R / 2 position of the head cross-section of the bar, Figure b is the high-magnification microstructure at the R / 2 position of the middle cross-section of the bar, and Figure c is the high-magnification microstructure at the R / 2 position of the tail cross-section of the bar. DETAILED DESCRIPTION

[0026] In order to make the purpose, technical solution and advantages of the present invention more clear, the technical solution of the present invention will be clearly and completely described below in conjunction with the drawings and embodiments of the present invention.

[0027] The present invention provides a method for preparing an ultra-large-size TC21 titanium alloy bar, which adopts a process of single-phase region blanking forging → two-phase region intermediate forging → forming forging, and specifically comprises the following steps:

[0028] Step 1: Forging in β single phase region for 3 times:

[0029] The specifications of the titanium alloy ingots are Φ690mm~Φ720mm in diameter and the single weight is greater than 5 tons. The TC21 titanium alloy ingots are subjected to upsetting and drawing forging in the first fire. First, the ingots are heated to the temperature of the β single-phase region and kept warm. After being taken out of the furnace, they are forged with a large deformation amount to obtain an intermediate billet ingot with a square cross-section. The material is cooled by air after forging.

[0030] The second and third forgings are carried out by the "three-dimensional reversing" forging method. First, the ingot is heated to the temperature of the β single-phase region and kept warm. After it is taken out of the furnace, it is subjected to "three-dimensional reversing" upsetting and drawing forging, and finally an intermediate billet ingot with a square cross-section and a grain size of 3.5mm to 5.5mm is obtained. After each forging, the intermediate billet ingot is cooled by air.

[0031] When forging in the single-phase zone, the heating temperature of the first fire is Tβ+(150~250)℃, the holding time is 450min~600min, and upsetting and drawing forging are carried out after the furnace is taken out. The cumulative forging ratio is 5.5~7.5, the upsetting reduction rate is 40mm / s~50mm / s, the drawing reduction rate is 70mm / s~80mm / s, and the feed amount during drawing is 300mm~400mm, and finally the intermediate billet ingot with a square cross section is obtained. The heating temperature of the second to third fires is Tβ+(50~150)℃, and the holding time is 450min~600min. Each fire adopts "three-dimensional reversing" upsetting and drawing forging, that is, each fire intermediate billet ingot is first upset forged along the axial direction, and then drawn along the radial direction. This forging method can eliminate the deformation "dead zone". The cumulative forging ratio of the two fires is controlled at 12-14 to ensure that the β grains are fully refined and homogenized. The upsetting reduction rate is 40mm / s-50mm / s, the drawing reduction rate is 70mm / s-80mm / s, and the feed amount during drawing is 300mm-400mm. Finally, an intermediate billet ingot with a square cross-section is obtained.

[0032] Based on the plastic deformation microstructure evolution characteristics of TC21 titanium alloy, by reasonably designing the deformation amount of forging fire above the phase transformation point (single-phase zone), combined with the "three-dimensional reversing" forging method to eliminate the forging deformation "dead zone", the cast β grains were refined from 20mm~40mm to a uniform 3.5mm~5.5mm.

[0033] Step 2: Forging 3 times in the middle of the α+β two-phase region:

[0034] In each firing, the intermediate billet ingot is heated to the temperature of the α+β two-phase region and kept warm. After being taken out of the furnace, it is first upset and forged, then drawn and forged into a billet with a square cross-section, and finally further drawn into an intermediate billet with an octagonal cross-section. The material is cooled by air after forging.

[0035] During the intermediate forging in the two-phase zone, the heating temperature of each fire is Tβ-(20~50)℃, the holding time is 360min~540min, and after the upsetting and drawing forging are completed, the drawing forging is continued to form an intermediate billet with an octagonal cross section, and the cumulative forging ratio of the three fires is 12~18. The upsetting reduction rate is 20mm / s~30mm / s, the drawing reduction rate is 40mm / s~60mm / s, the feed amount during drawing is 200mm~300mm, and the cooling method of the intermediate billet after each fire forging is air cooling.

[0036] Step 3: α+β two-phase zone forming forging 2 times:

[0037] In the first firing, the intermediate billet is heated to the temperature of the α+β two-phase region and kept warm. After being taken out of the furnace, it is drawn and forged into a billet with a circular cross section. The material is cooled by air after forging.

[0038] In the second fire, the round billet is heated to the temperature of the α+β two-phase region and kept warm. After being taken out of the furnace, it is shaped and forged to be rounded into a bar billet with a circular cross-section and dimensions that meet the requirements. The material is cooled by air after forging.

[0039] During the forming forging, the heating temperature of the first fire is Tβ-(30~60)℃, the holding time is 320min~450min, and after being taken out of the furnace, it is drawn and forged into a round billet with a diameter of Φ530mm~Φ630mm. The drawing deformation is controlled at 30%~40%, the final forging temperature is not less than 750℃, and the round billet is cooled by air after forging. The heating temperature of the second fire is Tβ-(40~70)℃, the holding time is 300min~420min, and after being taken out of the furnace, it is shaped and forged, and rounded into a rod billet with a diameter of Φ510mm~Φ610mm. The rounding deformation is controlled at 5%~15%, and the final forging temperature is not less than 700℃. The cooling method of the rod billet after forging is air cooling.

[0040] The rod blanks with a diameter of Φ510mm~Φ610mm are mechanically processed to finally produce TC21 titanium alloy super-large-sized bars with a diameter of Ф500mm~Ф600mm and a single weight of more than 4 tons.

[0041] The present invention is further described in detail below in conjunction with specific embodiments.

[0042] Example 1

[0043] 1) Single phase area billet forging 3 times:

[0044] The steel is forged in one piece using an ingot with a single weight of 5.2 tons and a diameter of Ф690mm. The phase transition point of the ingot is 960℃.

[0045] The first fire ingot is directly heated to 1170℃ and kept warm for about 450min~600min. After being taken out of the furnace, it is subjected to upsetting and drawing forging. The total forging ratio of upsetting and drawing is controlled at 5.5~7.5, the upsetting reduction rate is 40mm / s~50mm / s, the drawing reduction rate is 70mm / s~80mm / s, and the feed amount during drawing is 300mm~400mm. An intermediate billet ingot with a square cross-section is obtained, and the intermediate billet ingot is air-cooled after forging.

[0046] The intermediate billet ingots of the second and third fires are directly heated to 1100℃ and kept warm for about 450min to 600min. After being taken out of the furnace, they are subjected to "three-dimensional reversing" upsetting and drawing forging, that is, the intermediate billet ingots of each fire are first upset forged along the axial direction, and then drawn forged along the radial direction. The cumulative forging ratio of the two fires is controlled at 12 to 14, the upsetting reduction rate is 40mm / s to 50mm / s, the drawing reduction rate is 70mm / s to 80mm / s, and the feed amount during drawing is 300mm to 400mm, and the intermediate billet ingot with a square cross section is obtained. The intermediate billet ingot is air-cooled after each fire forging.

[0047] 2) Two-phase zone intermediate billet forging 3 times:

[0048] The first fire intermediate billet ingot is directly heated to 940℃ and kept for about 360min~450min. After being taken out of the furnace, it is subjected to upsetting, drawing and octagonal forging, that is, the intermediate billet ingot is upset and drawn along the axial direction to obtain an intermediate billet with a square cross section, and then it is drawn and forged along the axial direction to obtain an intermediate billet with an octagonal cross section. The forging ratio of each fire is controlled at 4~6, the upsetting reduction rate is 20mm / s~30mm / s, the drawing reduction rate is 40mm / s~60mm / s, the feed amount during drawing is 200mm~300mm, and the intermediate billet is air-cooled after forging.

[0049] The intermediate billet of the 2nd and 3rd fires is directly heated to 930℃ and 920℃ and kept for about 360min~450min. After being taken out of the furnace, it is subjected to upsetting, drawing and octagonal forging. The forging method is the same as the 1st fire. The forging ratio of each fire is controlled at 4~6, the upsetting reduction rate is 20mm / s~30mm / s, the drawing reduction rate is 40mm / s~60mm / s, the feed amount during drawing is 200mm~300mm, and the intermediate billet is air-cooled after each fire forging.

[0050] 3) Forming forging 2 times:

[0051] The intermediate billet of the first fire is directly heated to 910℃ and kept at this temperature for about 320min~450min. After being taken out of the furnace, it is drawn and forged to a round billet with a diameter of Φ530mm. The drawing deformation is controlled at 30%~40%, the drawing reduction rate is 30mm / s~40mm / s, the feed amount during drawing is 200mm~300mm, and the final forging temperature is not less than 750℃. The round billet is air-cooled after forging.

[0052] The second round billet is heated to 900℃ and kept for about 300min-420min. After it is taken out of the furnace, it is shaped and forged to be rounded into a billet with a diameter of Φ510mm. The deformation is controlled at 5%-15%, and the final forging temperature is not less than 700℃. After forging, the billet is air-cooled.

[0053] The rod blank with a diameter of Φ510mm is machined to produce a super-large TC21 titanium alloy rod with a diameter of Φ500mm and a single weight of 4.2 tons. (Note: The size of the finished product after machining is Φ500mm)

[0054] The TC21 titanium alloy Φ500mm super-large bar prepared in Example 1 was sawn into Φ500mm×75mm specimens at the head, middle and tail and subjected to heat treatment. The high and low magnification microstructures and transverse room temperature mechanical properties of the cross-sections of the head, middle and tail of the bar were tested.

[0055] The diameter of the TC21 titanium alloy super-large bar is Φ500mm, the length is about 4700mm, and the unit weight is about 4.2 tons. Figure 1 This is a low-magnification microstructure diagram of the cross-section of the head, middle and tail of the TC21 titanium alloy Φ500mm super-large bar prepared by this forging method. It can be seen that the low-magnification microstructure is uniform and fuzzy, and no metallurgical defects are found. Figure 2 This is the high-magnification structure of the R / 2 position of the head, middle and tail cross-section of the TC21 titanium alloy Φ500mm super-large bar prepared by this forging method. It can be seen that the high-magnification structure is composed of equiaxed and a small amount of short rod-shaped primary α phase. The high-magnification structure is uniform, and no abnormalities such as thermal structure are seen. The transverse room temperature tensile performance test results of the head, middle and tail cross-section of the TC21 titanium alloy Φ500mm super-large bar prepared by this forging method at the R / 2 position are shown in Table 1. The test results all meet the requirements of aviation standards, with good uniformity and a certain margin. In summary, the TC21 titanium alloy super-large bar prepared by this forging method has good overall consistency and uniformity in structure and performance.

[0056] Table 1 Room temperature tensile properties of TC21 titanium alloy Φ500mm super large bar

[0057] .

Claims

1. A method for preparing TC21 titanium alloy super-large bar, characterized in that: The following steps are involved: Step 1: Forging in β single phase region for 3 times: In the first fire, the TC21 titanium alloy ingot is subjected to upsetting and drawing forging to obtain an intermediate billet ingot with a square cross section; in the second and third fires, "three-dimensional reversing" upsetting and drawing forging are performed to obtain an intermediate billet ingot with a square cross section and a grain size of 3.5 mm to 5.5 mm; The heating temperature of the first fire is Tβ+(150~250)℃, the holding time is 450min~600min, and the cumulative forging ratio is 5.5~7.

5. The heating temperature of the second to third fires is Tβ+(50~150)℃, the holding time is 450min~600min, and the cumulative forging ratio of the two fires is controlled at 12~14. "Three-dimensional reversal" means that the intermediate billet ingot of each fire is firstly subjected to upsetting forging along the axial direction, and then to drawing forging along the radial direction; Step 2: Forging 3 times in the middle of the α+β two-phase region: In each firing, the intermediate billet ingot is firstly upset forged, then drawn and forged into a billet with a square cross section, and finally further drawn and lengthened into an intermediate billet with an octagonal cross section; The heating temperature of each fire is Tβ-(20~50)℃, the holding time is 360min~540min, and the cumulative forging ratio of three fires is 12~18; Step 3: α+β two-phase zone forming forging 2 times: In the first fire, the intermediate billet is stretched and forged into a billet with a circular cross section, and in the second fire, the circular billet is rounded into a bar billet with a circular cross section and meeting the required size; The heating temperature of the first fire is Tβ-(30~60)℃, and the holding time is 320min~450min. After being taken out of the furnace, it is drawn and forged into a round billet with a diameter of Φ530mm~Φ630mm. The heating temperature of the second fire is Tβ-(40~70)℃, and the holding time is 300min~420min. After being taken out of the furnace, it is rounded into a rod billet with a diameter of Φ510mm~Φ610mm. The rod billet is processed to prepare TC21 titanium alloy super-large size bars with a diameter of Ф500mm~Ф600mm and a single weight greater than 4 tons.

2. The method for preparing the TC21 titanium alloy super-large bar according to claim 1, characterized in that: In the step 1, the specification of the TC21 titanium alloy ingot is Φ690mm-Φ720mm, and the unit weight is greater than 5 tons.

3. The method for preparing the super-large-size TC21 titanium alloy bar according to claim 1, characterized in that: In the step 3, during the first tempering, the drawing deformation is controlled at 30% to 40%, and the final forging temperature is not less than 750°C.

4. The method for preparing the super-large-size TC21 titanium alloy bar according to claim 1, characterized in that: In the step 3, during the second tempering, the rounding deformation is controlled at 5% to 15%, and the final forging temperature is not less than 700°C.

Citation Information

Patent Citations

  • Preparation method of TC21 titanium alloy large-specification bar

    CN103510030A

  • Forging method for high temperature resistance titanium alloy large-size bars used for engines

    CN106734796A

  • Preparation method of TC11 titanium alloy large-size bars

    CN107858618A

  • Forging method of ultrahigh-toughness TB18 titanium alloy large-specification forging stock

    CN114603074A

  • Preparation method of TA15 titanium alloy large-specification flat plate forging stock

    CN116140515A