A rapid prototyping method and mold for composite material components using HP-RTM

By calculating the resin amount and adjusting the injection parameters, combined with ultrasonic cutting and mold optimization, the problems of molding instability and thickness limitation in the HP-RTM process were solved, realizing the production of composite material products with high efficiency and low cost.

CN117621489BActive Publication Date: 2026-11-10BEIJING NAT INNOVATION INST OF LIGHTWEIGHT LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202210996947.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-19
Publication Date
2026-11-10
Estimated Expiration
2042-08-19

AI Technical Summary

Technical Problem

The existing HP-RTM process has problems such as unstable process parameter optimization, dry spots on the product surface, long molding cycle, high cost, and difficulty in producing thicker products.

Method used

By simulating and analyzing the resin volume, adjusting the injection head pressure and mixer flow rate, vacuuming after mold closing, using low-viscosity resin and high injection pressure, and combining with an ultrasonic cutter, the mold design is optimized to achieve rapid molding and efficient cutting.

Benefits of technology

It achieves stability of process parameters and improvement of molding efficiency, smooth product surface, shortened molding cycle, reduced cost, and can produce composite material products with a thickness of ≥40mm.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117621489B_ABST
    Figure CN117621489B_ABST
Patent Text Reader

Abstract

This invention relates to the field of materials processing technology, and particularly to a rapid prototyping method and mold for composite material components using HP-RTM. The HP-RTM rapid prototyping method for composite material components includes: calculating the required resin amount based on the needs of the composite material component to be manufactured; adjusting the pressure of the raw material components at the nozzle of the injection head before installing the injection head; preheating and degassing the raw material under vacuum, and adjusting the flow circulation mode of the mixer; mold preparation; laying the fiber product; pressing the mold; applying pressure to the press; vacuum pressure holding; resin injection; pressure holding and curing; and after pressure holding and curing, sequentially performing pressure release, vacuum breaking, ejector pin demolding, cooling, and flash removal. Composite material components prepared using the HP-RTM rapid prototyping method and mold provided by this invention have a shorter molding cycle, higher molding efficiency, lower manufacturing cost, and smooth double-sided surfaces. By adding preform preforming and preform cutting steps, products with a thickness ≥40mm can be prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of materials processing technology, and in particular to a rapid prototyping method and mold for composite material components using HP-RTM. Background Technology

[0002] Driven by environmental protection and energy conservation needs, lightweighting of automobiles has become a global trend in automotive development. With the advancement of lightweight molding technology, replacing traditional sheet metal parts with new composite material components is gradually becoming a trend in automotive applications. Composite materials have garnered widespread attention in the automotive industry due to their superior performance, with composite material molding processes consistently being a key research focus. High-pressure resin transfer molding (HP-RTM), as one of the advanced molding processes for composite materials, boasts advantages such as short molding cycles, high fiber volume fraction, and advanced automation, and has gained widespread recognition in composite material manufacturing.

[0003] HP-RTM (High-Pressure Resin-Liquid Molding) is a molding process that uses high pressure to inject a mixture of resin into a vacuum-sealed mold pre-laid with fiber reinforcement and inserts. The resin then flows through the mold, impregnates, cures, and is demolded to obtain a composite material product. The high injection pressure ensures that the resin is completely injected into the mold cavity and fully penetrates before curing. HP-RTM uses dry, continuous fibers and liquid resin as raw materials. The resin is injected into the dry fiber surface within the mold, then heated and pressurized, allowing for simultaneous impregnation and curing before demolding, significantly accelerating the entire production process. Currently, HP-RTM has been applied to a range of vehicle models, primarily for the production of structural components such as bumper brackets, leaf springs, side beams, side roof reinforcement panels, and trunk liners.

[0004] Currently, existing HP-RTM processes still have many problems that need to be solved, including unstable process parameter optimization, surface dry spots on products, long molding cycles, high costs, and difficulty in producing thicker products. Therefore, how to provide an HP-RTM process that is simple, requires less investment, has lower costs, produces products with smooth double sides, has high molding efficiency, and high product strength is a problem that urgently needs to be solved by those skilled in the art. Summary of the Invention

[0005] Based on the above analysis, the present invention aims to provide a rapid prototyping method and mold for composite material components using HP-RTM, which solves at least one of the following technical problems: 1. Unstable process parameter optimization and dry spots on the product surface; 2. Long molding cycle, low molding efficiency, and high manufacturing cost; 3. Difficulty in producing thicker products.

[0006] The objective of this invention is mainly achieved through the following technical solutions:

[0007] On the one hand, the present invention provides a rapid prototyping method for composite material components using HP-RTM, characterized by comprising the following steps:

[0008] Step 1: Based on the requirements of the composite material component to be prepared, calculate the required amount of resin through simulation analysis of the composite material component to be prepared; before installing the dispensing head, adjust the pressure of the raw material components at the nozzle of the dispensing head; preheat the raw material, perform vacuum degassing treatment, and adjust the flow circulation mode of the mixer;

[0009] Step 2: Clean the mold and spray an external release agent; control the mold temperature using a temperature control system to raise the temperature to the optimal molding temperature of the resin material;

[0010] Step 3: According to the layup design requirements of the composite material component to be prepared, cut and lay the fiber cloth in sequence according to the drawings;

[0011] Step 4: Place the fiber cloth into the mold cavity, and the press moves downward to close the mold;

[0012] Step 5: After the upper and lower molds are closed and locked, the press applies pressure to a certain level.

[0013] Step 6: Control the vacuum control valve through the mold vacuum system, open the vacuum control valve, and evacuate the cavity. Determine the vacuum level based on the vacuum gauge reading. Once the vacuum level reaches the process value, close the vacuum control valve through the vacuum system to keep the cavity in a vacuum state.

[0014] Step 7: Inject resin at a certain injection pressure according to the set injection flow rate and injection time. After completion, maintain pressure and cure. After maintaining pressure and curing, release pressure, break vacuum, eject the ejector pins to demold, cool, and remove flash in sequence.

[0015] Furthermore, the HP-RTM rapid prototyping method for composite material components also includes preform preforming and preform cutting;

[0016] The preforming of the blank involves transferring the laid-up fiber cloth to an oven for heating and insulation, then transferring it to a preforming press to apply pressure and press it into shape, and finally removing it after it has naturally cooled to room temperature.

[0017] The blank cutting involves transferring the pressed blank to a cutting fixture for fixation, and then cutting it into the shape of the target product using an ultrasonic cutting blade.

[0018] Furthermore, in step 1, the pressure of the raw material components at the nozzle of the dispensing head is 100-160 bar; the preheating conditions of the raw material are: resin temperature 85-90℃, curing agent temperature 45-50℃, and internal release agent temperature 25-30℃.

[0019] Furthermore, in step 2, the mold temperature is 60-120℃.

[0020] Furthermore, in step 5, the pressure is 1000-9000kN.

[0021] Further, in step 7, the mass ratio of resin, curing agent and internal release agent in the raw materials is 100:23:0-100:25:2;

[0022] The injection flow rate is 30-150 g / s, the injection time is 5-300 s, and the injection pressure is 100-160 bar.

[0023] Furthermore, in step 7, the pressure holding and curing time is 5-10 minutes.

[0024] Furthermore, in step 1, the flow circulation mode of the mixing machine is a low flow circulation mode.

[0025] On the other hand, the present invention also provides a composite material component HP-RTM rapid prototyping mold for realizing the molding method, including: an upper mold, a lower mold, a vacuum system, a sealing structure, an airtight structure, a temperature control system and a pressure control system, wherein the upper mold and the lower mold form a cavity;

[0026] The upper mold is provided with a vacuum control valve mounting port, and the cavity is connected to the vacuum system through the vacuum control valve in the vacuum control valve mounting port.

[0027] The vacuum control valve is equipped with a high-temperature resistant O-ring and a conical mechanical seal structure.

[0028] Furthermore, the vacuum control valve includes a valve stem and a valve sleeve, which form a conical mechanical seal structure.

[0029] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:

[0030] 1. Based on the preparation requirements of the composite material components to be prepared, the present invention calculates the required amount of resin through simulation analysis of the product, and ensures product quality by setting appropriate injection flow rate and injection pressure in the resin injection step.

[0031] 2. During resin injection, the higher mixing injection pressure (100-160 bar) and low viscosity resin greatly increase the resin injection flow rate, which allows the resin to penetrate quickly, facilitates the expulsion of air and the reduction of product voids, improves product quality, and shortens the molding process cycle (5-10 min).

[0032] 3. Existing methods involve vacuuming before mold closing and pressurization. Compared to existing methods, this invention performs mold closing and pressurization before vacuuming, which is more conducive to removing air bubbles from the product and saves operation time. The addition of a vacuum-breaking operation avoids damage to the mold and equipment caused by direct mold opening, which could affect the mold's sealing during cyclic production and consequently impact product quality.

[0033] 4. Existing HP-RTM processes cannot produce products with a thickness exceeding 20mm. This invention uses an ultrasonic cutting tool. By optimizing the tool's amplitude, speed, cutting angle, and path, it can quickly and efficiently cut out complete, high-quality blanks, improving efficiency. Combined with preforming process steps, it can produce products with complex structures and a thickness ≥40mm.

[0034] 5. This invention provides an HP-RTM rapid prototyping mold for composite material components. The sealed structure design effectively extends the mold life cycle, reduces the number of mold repairs in mass production, and enables precise control of mold temperature and injection pressure through temperature and pressure sensing systems. This allows for precise control of the resin curing process within the mold cavity, reducing defect rates, simplifying process debugging, and improving production efficiency.

[0035] In this invention, the above-described technical solutions can be combined with each other to achieve more preferred combinations. Other features and advantages of this invention will be set forth in the following description, and some advantages may become apparent from the description or be learned by practicing the invention. The objects and other advantages of this invention can be realized and obtained from what is particularly pointed out in the description and drawings. Attached Figure Description

[0036] The accompanying drawings are for illustrative purposes only and are not intended to limit the invention. Throughout the drawings, the same reference numerals denote the same parts.

[0037] Figure 1 This is a schematic diagram of the key steps of the method of the present invention;

[0038] Figure 2 This is a physical image of the finished product of Embodiment 1 of the present invention;

[0039] Figure 3 This is a physical image of the finished product of Embodiment 2 of the present invention;

[0040] Figure 4 This is a longitudinal sectional view of the HP-RTM rapid prototyping mold of the present invention;

[0041] Figure 5 This is a schematic cross-sectional view of the HP-RTM rapid prototyping mold of the present invention;

[0042] Figure 6 This is another longitudinal sectional view of the HP-RTM rapid prototyping mold of the present invention;

[0043] Figure 7 This is an enlarged schematic diagram of the sealing structure, encapsulation seal, and gas seal of the HP-RTM rapid prototyping mold vacuum control valve of the present invention.

[0044] The annotations in the attached figures are explained as follows:

[0045] 100-Upper mold, 101-Upper mold fixing plate, 102-Upper mold pad, 103-Upper mold heat insulation plate, 104-Upper mold core, 105-Upper mold insulation plate, 106-Pressure sensor, 107-Injection port, 108-Upper mold temperature sensor, 109-Guide sleeve, 110-Vacuum system, 111-Air nozzle, 112-Vacuum pipeline, 113-Vacuum cylinder, 114-Vacuum control valve, 1141-O-ring seal, 1142-Valve sleeve, 1143-Valve stem, 115-Vacuum oil circuit 116-Vacuum gauge, 120-Upper mold temperature controller, 200-Lower mold, 201-Lower mold fixing plate, 202-Lower mold pad, 203-Lower mold heat insulation plate, 204-Lower mold core, 205-Lower mold insulation plate, 206-Sealing glue, 207-Air seal, 208-Support block, 209-Guide post, 210-Ejection mechanism, 211-Push plate, 212-Ejector rod, 213-Ejection cylinder, 214-Lower mold temperature sensor, 220-Lower mold temperature controller, 300-Cavity. Detailed Implementation

[0046] Preferred embodiments of the present invention will now be described in detail with reference to the accompanying drawings, which form part of this application and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not intended to limit the scope of the present invention.

[0047] This invention provides a rapid prototyping method for composite material components using HP-RTM, comprising the following steps:

[0048] Step 1: Based on the requirements of the composite material component to be prepared, calculate the required amount of resin through simulation analysis of the composite material component to be prepared; before installing the dispensing head, adjust the pressure of the raw material components at the nozzle of the dispensing head; preheat the raw material, perform vacuum degassing treatment, and adjust the flow circulation mode of the mixer;

[0049] Step 2: Clean the mold and spray an external release agent; control the mold temperature using a temperature control system to raise the temperature to the optimal molding temperature of the resin material;

[0050] Step 3: According to the layup design requirements of the composite material component to be prepared, cut and lay the fiber cloth in sequence according to the drawings;

[0051] Step 4: Place the fiber cloth into the mold cavity, and the press moves downward to close the mold;

[0052] Step 5: After the upper and lower molds are closed and locked, the press applies pressure to a certain level.

[0053] Step 6: Control the vacuum control valve through the mold vacuum system, open the vacuum control valve, and evacuate the cavity. Determine the vacuum level based on the vacuum gauge reading. Once the vacuum level reaches the process value, close the vacuum control valve through the vacuum system to keep the cavity in a vacuum state.

[0054] Step 7: Inject resin at a certain injection pressure according to the set injection flow rate and injection time. After completion, maintain pressure and cure. After maintaining pressure and curing, release pressure, break vacuum, eject the ejector pins to demold, cool, and remove flash in sequence.

[0055] Specifically, the raw materials mentioned in step 1 are resin, curing agent, and internal release agent, and the pressure of the three components in the dispensing head is 100-160 bar.

[0056] The pressure values ​​of the three components need to be adjusted within the range of 100-160 bar according to the required injection flow rate. Increasing the injection flow rate requires a corresponding increase in pressure, and the pressure values ​​of the three components should not differ by more than 10 bar. Excessive differences will damage the dispensing head and affect injection accuracy. Below 100 bar, the injection pressure is too low, the injection flow rate is too small, affecting the molding cycle and effect; above 160 bar, the pressure on the dispensing head is too high, which can easily damage the equipment.

[0057] Specifically, in step 1, the preheating conditions for the raw materials are: resin temperature 85-90℃, curing agent temperature 45-50℃, and internal release agent temperature 25-30℃.

[0058] The resin temperature is 85-90℃, the curing agent temperature is 45-50℃, and the internal release agent temperature is 25-30℃. Under these temperature conditions, the viscosity of the resin, curing agent, and internal release agent is moderate, and the fluidity is good, which is conducive to fiber impregnation, improves the quality of the parts, and shortens the curing and molding cycle, thereby improving production efficiency.

[0059] Specifically, in step 1, the required amount of resin is calculated by simulating and analyzing the target product to be prepared using composite material parts processing simulation software, providing a basis for the amount of resin used in the actual production process.

[0060] The resin used in this invention is epoxy resin, and the curing agent is an amine curing agent. This resin system has high activity and can cure quickly.

[0061] Specifically, the flow circulation mode of the mixing machine is a low flow circulation mode.

[0062] To ensure the normal operation of the mixing machine and prevent pipe blockage due to increased viscosity caused by low resin temperature and stagnation, the equipment must be kept running to ensure resin circulation within the pipes, employing a low-flow circulation mode. It should be noted that the low-flow circulation mode, as described in this invention, refers to a flow rate that is half that used during normal production. This low-flow circulation mode is achieved by adjusting the resin delivery flow rate through external input of the required flow rate combined with adjusting the metering pump opening size.

[0063] Specifically, the external release agent mentioned in step 2 is model CLE-705, and the dosage is 10-20ml each time.

[0064] Clean the mold to remove impurities and keep it clean. The external release agent forms a smooth, dense film on the mold surface. This film adheres well to the mold surface, is not easily detached or damaged, and does not react or adhere to the target product, allowing the molded product to be easily removed. Use 10-20ml each time, spraying in small amounts multiple times to ensure the external release agent is completely and evenly coated on the mold surface.

[0065] Specifically, in step 2, the mold is heated to 60-120℃.

[0066] The mold needs to be heated to 60-120℃. Below this temperature, the resin viscosity is high and the fluidity is poor, resulting in poor curing effect. Above this temperature, the glass transition temperature of the raw material is exceeded, and the resin will cure immediately.

[0067] Specifically, unlike existing methods that first perform vacuuming and then mold closing and pressurization, this invention performs mold closing and pressurization first and then vacuuming (steps 4-5 and 6). Performing mold closing and pressurization first and then vacuuming is more conducive to removing air bubbles from the product and saves operation time.

[0068] Specifically, in step 5, the pressure is increased to 1000-9000kN.

[0069] The mold is pressurized by a hydraulic press, which supplies oil to the cylinder via an oil pump. A check valve maintains the pressure, and a regulating valve controls the oil pressure. If the pressure exceeds the set value, the valve releases oil to maintain the set pressure. The pressure must be between 1000-9000 kN to ensure that the clamping force is greater than the pressure generated within the mold cavity during injection, preventing resin from overflowing from the mold or damaging it.

[0070] Specifically, in step 7, the resin injection process is completed. The mass ratio of resin, curing agent and release agent in the raw materials is 100:23:0-100:25:2; the injection flow rate is 30-150g / s, the injection time is 5-300s, and the injection pressure is 100-160bar.

[0071] First, the mixer needs to be adjusted to high-pressure circulation mode, and all process parameters, such as injection flow rate and injection time, should be adjusted to the parameters used in actual production. Low-flow circulation mode is only for ensuring basic equipment operation; the equipment cannot complete the injection process in this mode. For actual injection, it needs to be switched to high-pressure circulation mode. By setting appropriate injection flow rate and injection pressure using a high-precision mixer, the required resin content can be further precisely measured based on the resin dosage calculated in step 1 (simulated product analysis), preventing resin waste.

[0072] Low injection flow rate is beneficial for fiber wetting, while high injection flow rate is beneficial for improving product production efficiency. Taking all factors into consideration, the resin injection flow rate of this invention is 30-250 g / s. Simultaneously, the higher mixing injection pressure (100-160 bar) and low-viscosity resin allow for rapid resin penetration, facilitating air removal and reducing product voids, thus improving product quality. Furthermore, it shortens the molding process cycle (5-10 min).

[0073] Specifically, the pressure holding and curing time is 5-10 minutes to ensure that the resin is completely cured.

[0074] Specifically, compared to existing processes, an operation to break the vacuum is added. This is because the mold cavity remains under vacuum after curing. Directly opening the mold would damage the mold and equipment, affecting the mold's sealing during subsequent production and ultimately impacting product quality.

[0075] A rapid prototyping method for composite materials using HP-RTM also includes preform preforming and preform cutting;

[0076] Preform preforming: Transfer the laid-up fiber cloth to an oven for heating and insulation, then transfer it to a preforming press for pressure pressing and shaping, and remove it after natural cooling to room temperature;

[0077] Blank cutting: The pressed blank is transferred to the cutting fixture and fixed, and then cut into the shape of the target product using an ultrasonic cutter.

[0078] Specifically, during the preforming of the blank, the oven temperature is 130-180℃ and the time is 60-120 minutes. Within this temperature and time range, the setting powder in the fiber cloth melts and sets under these conditions, ensuring that the fiber bundles do not loosen after pressing, making them easy to cut.

[0079] Specifically, the conditions for using ultrasonic cutting in blank cutting are: air supply pressure 6-8 bar, amplitude 37-42%, and cutting speed 20-60 mm / s.

[0080] Ultrasonic cutting technology involves converting electric current into electrical energy using an ultrasonic generator. This high-frequency electrical energy is then converted into mechanical vibrations of the same frequency by a transducer. These mechanical vibrations are then transmitted to the cutting blade via an amplitude modulator. The cutting blade transfers the received vibrational energy to the cutting surface of the workpiece, thus cutting the blank.

[0081] An air supply pressure of 6-8 bar ensures sufficient air volume, allowing the cutter to cool down promptly and extend its service life. An amplitude of 37-42% ensures effective cutting of the blank without damaging the cutter due to excessive vibration. A cutting speed of 20-60 mm / s guarantees a smooth, secure cut, accurate edges, and prevents deformation, warping, fraying, stringing, or wrinkling. Furthermore, maintaining a 90° angle between the cutter tip and the ground, and keeping the cutting path parallel to the outer edge of the mold, minimizes shape errors in the blank during cutting, resulting in a complete, high-quality blank.

[0082] Traditional cutting tools and technologies cannot effectively cut the blank, resulting in the inability of existing HP-RTM processes to produce products with a thickness exceeding 20mm. This invention uses an ultrasonic cutting tool, which optimizes the amplitude, speed, cutting angle, and path of the tool to quickly and efficiently cut out complete, high-quality blanks, improving efficiency. Combined with preforming process steps, it can produce products with complex structures and a thickness ≥40mm.

[0083] The HP-RTM molding process features a large mold closing clearance, high injection pressure, and the use of low-viscosity resin with a fast resin injection flow rate, which can significantly shorten the molding process cycle. The inventors discovered in their research that the cycle length of the existing HP-RTM process is positively correlated with the number of mold repairs during production. Mold repairs stem from blockages in the mold's injection port and vacuum port, leading to damage to the mold's sealing structure. In cyclical production, damage to the mold's sealing structure easily causes vacuum failure, resulting in the entire vacuum system of the mold becoming filled with resin, causing irreversible damage to the mold and equipment, and resulting in a shorter mold lifespan.

[0084] In addition, the existing mold temperature and pressure control accuracy is low, which cannot effectively monitor the pressure and temperature changes during the composite material molding process, resulting in a long trial production cycle for qualified samples and high production costs for the products.

[0085] Based on this, the present invention also provides an HP-RTM rapid prototyping mold for composite material components, used to realize the above-mentioned molding method.

[0086] A composite material component HP-RTM rapid prototyping mold includes: an upper mold 100, a lower mold 200, a vacuum system 110, a sealing structure 206, an airtight structure 207, a temperature control system, and a pressure control system, wherein the upper mold 100 and the lower mold 200 form a cavity 300.

[0087] The upper mold 100 is provided with a vacuum control valve mounting port, and the cavity 300 is connected to the vacuum system 110 through the vacuum control valve 114 in the vacuum control valve mounting port.

[0088] The vacuum control valve 114 is equipped with a high-temperature resistant O-ring 1141 and a conical mechanical seal structure.

[0089] Specifically, the vacuum control valve includes a valve stem 1143 and a valve sleeve 1142, which form a conical mechanical seal structure.

[0090] In one possible implementation, the valve stem 1143 includes a first equal-diameter segment, a curved segment, and a second equal-diameter segment connected sequentially. The inner wall of the valve sleeve 1142 includes a first equal-diameter segment, a curved segment, and a second equal-diameter segment whose diameters decrease sequentially and are connected sequentially. The valve sleeve 1142 is fitted onto the valve stem 1143, with a clearance fit between the first equal-diameter segment of the valve stem 1143 and the first equal-diameter segment of the inner wall of the valve sleeve 1142, a transition fit between the curved segment of the valve stem 1143 and the curved segment of the inner wall of the valve sleeve 1142, and a transition fit between the second equal-diameter segment of the valve stem 1143 and the second equal-diameter segment of the inner wall of the valve sleeve 1142.

[0091] In the molding method of this invention, after the mold is closed and pressurized, a vacuum needs to be drawn. The cavity 300 is connected to the vacuum system 110 through the vacuum control valve 114 in the vacuum control valve mounting port. To facilitate vacuuming, the gap at the end of the cavity is smaller than the gap in the middle of the cavity along the resin flow direction. The cavity end of the vacuum control valve has a horizontal opening end. Compared with the cavity end part at its front end, this horizontal opening end is provided with an expansion section to facilitate the flow of vacuum air, improve vacuuming efficiency, and obtain a higher vacuum rate.

[0092] The vacuum control valve mounting port is located in the upper mold 100, within the horizontal mating section area at the end of the cavity 300 of the upper mold 100 and lower mold 200. Considering that the cavity 300 has a preform accommodating space and provides a resin flow filling space, the HP-RTM process has a large mold closing clearance and a high injection pressure, and the low-viscosity resin used has the characteristic of fast injection flow rate, in order to achieve vacuuming while effectively controlling the speed of pressurized resin injection and minimizing the possibility of resin entering the vacuum control valve, the horizontal length of the horizontal opening end at the cavity end is greater than the wall thickness of the second equal diameter section of the valve sleeve 1142, but less than the sum of the wall thickness of the second equal diameter section of the valve sleeve 1142 and the diameter of the second equal diameter section of the valve stem 1143. The mating clearance between the valve sleeve 1142 and the valve stem 1143 is not completely located within the horizontal area of ​​the horizontal opening end at the cavity end.

[0093] Since the fitting clearance between the valve sleeve 1142 and the valve stem 1143 is located in the horizontal region of the horizontal opening at the end of the cavity, in order to further prevent resin from entering the vacuum control valve and causing blockage of the mold injection port and vacuum port, resulting in damage to the mold sealing structure, the vacuum control valve of the present invention also includes a high-temperature resistant O-ring.

[0094] The number of high-temperature resistant O-rings is multiple. In one possible embodiment, three sets of high-temperature resistant O-rings 1141 are provided on the mating surfaces of the valve sleeve 1142 and the valve stem 1143. The first and second sets of high-temperature resistant O-rings 1141 are located on the second equal diameter section of the valve stem 1143 and the second equal diameter section of the inner wall of the valve sleeve 1142. The third set of high-temperature resistant O-rings 1141 is located on the curved section of the valve stem 1143 and the curved section of the inner wall of the valve sleeve 1142.

[0095] Specifically, sealing ring mounting grooves are respectively opened on the first equal diameter section, the curved section and the second equal diameter section of the valve stem 1143, and high temperature resistant O-rings are installed in the sealing ring mounting grooves.

[0096] Since the cavity is formed by the mating of an upper mold and a lower mold, to facilitate vacuuming, one side wall of the vacuum control valve mounting port is flush with the edge of the horizontal opening at the end of the cavity, and the valve sleeve 1142 is fitted with the upper mold core 104 of the upper mold. To prevent resin from entering the mating surface between the valve sleeve 1142 and the upper mold core 104, a high-temperature resistant O-ring 1141 is provided between the valve sleeve 1142 and the upper mold core 104. A sealing ring mounting groove is provided on the outer surface of the valve sleeve 1142, and the high-temperature resistant O-ring 1141 is installed in the sealing ring mounting groove.

[0097] The present invention is provided with four sets of high-temperature resistant O-rings 1141. Three sets of high-temperature resistant O-rings are sequentially sleeved on the valve stem 1143 along the axial direction of the valve stem 1143. The first and second sets of high-temperature resistant O-rings 1141 are located on the cylindrical mating surface of the second equal diameter section, and the third set of high-temperature resistant O-rings 1141 is located on the conical mating surface of the curved section. The fourth set is located on the mating surface between the valve sleeve 1142 and the upper mold core 104 of the upper mold.

[0098] To further improve sealing performance, the spacing between the first, second, and third sets of high-temperature O-rings gradually increases along the axial direction of valve stem 1143. The fourth set of high-temperature O-rings is located between the second and third sets of high-temperature O-rings, and the second and fourth sets of high-temperature O-rings partially overlap in the axial direction.

[0099] To further improve sealing performance, the spacing between the first, second, and third sets of high-temperature resistant O-rings is as follows: The first set of high-temperature resistant O-rings is positioned on the cylindrical mating surface of the second equal-diameter section of the valve stem 1143, at half the length of the second equal-diameter section from bottom to top (the measurement reference is the length of the second equal-diameter section of the valve stem 1143, with the starting point being the lower end face). The second set of high-temperature resistant O-rings is positioned on the cylindrical mating surface of the second equal-diameter section of the valve stem 1143, starting from bottom to top... At 3 / 4 of the length of the second equal-diameter segment (measurement reference is the length of the second equal-diameter segment of valve stem 1143, starting from the lower end face), the third set of high-temperature resistant O-rings 1141 is located on the tapered mating surface of valve stem 1143. At 1 / 2 of the sum of the lengths of the curved segment and the second equal-diameter segment of valve stem 1143 (measurement reference is the sum of the lengths of the curved segment and the second equal-diameter segment of valve stem 1143, starting from the lower end face), the fourth set of high-temperature resistant O-rings is located on the mating surface between valve sleeve 1142 and upper mold core 104 of upper mold. The dimensions of the first, second, third, and fourth sets of high-temperature resistant O-rings meet the standardization requirements.

[0100] Through the above structural design, the mold sealing structure is not easily damaged in the molding cycle production of the present invention, thereby avoiding vacuum failure and effectively extending the life cycle of the mold.

[0101] Compared with existing molds, this invention uses a metal mechanical seal and a high-temperature resistant sealing ring to seal the vacuum control valve, which effectively extends the mold life cycle and reduces the number of mold repairs in mass production.

[0102] It should be noted that, due to the unique characteristics of the HP-RTM molding process, the lifespan of the mold sealing structure directly affects the mold's cycle life. Thermosetting resin is liquid before curing and solid after curing. In actual production, existing sealing structures are prone to damage to the sealing rings or resin adhesion to the mechanical seal. In subsequent production cycles, this can easily lead to vacuum system failure, causing the entire vacuum system to become filled with resin, resulting in irreversible damage to the mold and equipment. To address these issues, four sets of high-temperature resistant O-rings and conical mechanical seals are installed at the vacuum control valve from bottom to top. Each sealing structure functions to isolate the resin and provide a seal, effectively preventing resin overflow and air leakage. Even if one set of seals fails, the subsequent sets will remain effective, allowing the production cycle to continue uninterrupted, effectively extending the mold's lifespan.

[0103] Specifically, the sealing structure 206 is located on the parting surface of the lower mold core 104 and is situated outside the cavity. The air seal structure 207 is located outside the sealing structure 206, near the edge of the mold, specifically on the outer side of the horizontal opening end of the cavity. The sealing structure 206 and the air seal structure 207 are sequentially arranged thereon.

[0104] Specifically, the ends of the upper mold 100 and the lower mold 200 are fitted together by steps, and the air seal 207 structure is located at the mating surface of the upper mold 100 and the lower mold 200.

[0105] The sealing structure achieves a vacuum effect, and the airtight structure can effectively form a secondary sealed space, making the entire cavity 300 space more reliable.

[0106] Furthermore, the upper mold 100 includes an upper mold fixing plate 101, an upper mold pad 102, an upper mold heat insulation plate 103, an upper mold core 104, an upper mold insulation plate 105, an injection port 107, and a guide sleeve 109.

[0107] The upper mold pad 102 is connected to the upper mold fixing plate 101, and the upper mold core 104 is connected to the other side of the upper mold pad 102. An upper mold heat insulation plate 103 is installed between the upper mold core 104 and the upper mold pad 102. An upper mold insulation plate 105 covers the periphery of the upper mold core 104. The injection port 107 is connected to the upper mold core 104, with its bottom surface flush with the lower surface of the upper mold core 104. The guide sleeve 109 is connected to the upper mold core 104 and is concentric with the guide post 209. The gap between the injection port 107 and the injection nozzle of the HP-RTM high-pressure injection molding equipment is sealed by a high-temperature resistant O-ring.

[0108] Furthermore, the lower mold 200 includes a lower mold fixing plate 201, a lower mold pad 202, a lower mold heat insulation plate 203, a lower mold core 204, a lower mold insulation plate 205, a support block 208, and a guide post 209.

[0109] The lower mold pad 202 is connected to the lower mold fixing plate 201. The other end of the lower mold pad 202 is connected to the lower mold core 204. The lower mold heat insulation plate 203 is installed between the lower mold pad 202 and the lower mold core 204. The lower mold insulation plate 205 is connected to the lower mold core 204 and covers the outside of the lower mold core 204. The support block 208 is connected to the upper end face of the lower mold core 204. The guide post 209 is connected to the upper end face of the lower mold core 204 and is concentric with the guide sleeve 109.

[0110] Specifically, the temperature control system includes an upper mold temperature control system and a lower mold temperature control system; the upper mold temperature control system includes an upper mold temperature controller 120 and an upper mold temperature sensor 108.

[0111] Specifically, the mold also includes a pressure control system, which includes a pressure sensor 106.

[0112] Specifically, the upper mold core 104 has a length of 'a', and the upper mold temperature sensor 108 is connected to the side of the upper mold core 104 and is disposed on the upper mold core. Place, Place, The upper mold temperature controller 120 is located inside the upper mold core 104 and is connected to the side of the upper mold core 104.

[0113] Specifically, the lower mold core 204 has the same length as the upper mold core 104, and the lower mold temperature sensor 214 is connected to the outside of the lower mold core 204 and is disposed on the lower mold core. Place, Place, The lower mold temperature controller 220 is located inside the lower mold core 204 and is connected to the outside of the lower mold core 204.

[0114] Specifically, pressure sensors 106 are respectively disposed at the connection points of the upper mold core 104 and the cavity 300. The pressure sensors 106 are connected to the upper mold core 104 and are flush with the upper surface of the cavity 300.

[0115] The temperature and pressure control systems can effectively provide feedback on pressure changes and mold temperature changes during the entire injection molding process of thermosetting resin. By combining this data with the overall quality data of the prototype parts, the injection pressure and mold temperature can be adjusted, effectively reducing the trial production cycle of qualified prototype parts and lowering the production cost of the product.

[0116] Specifically, the lower mold 200 includes an ejection mechanism 210, which consists of a push plate 211, an ejector rod 212, and an ejection cylinder 213. The ejector rod 212 is provided with a high-temperature resistant O-ring seal, and there are two sets of high-temperature resistant O-ring seals, which are arranged sequentially below the ejection height of the ejector rod.

[0117] To ensure synchronized and automatic ejection of the resin product, the number and position of the ejector pins need to meet certain conditions. Specifically, there are four ejector pins 212, each positioned in the lower mold core. Place, Place, Place, At the location, the push rod 212 is connected and fixed to the push plate 211. Each of the four ends of the push plate 211 is provided with an ejection cylinder 213. One end of the ejection cylinder 213 is connected and fixed to the push plate 211, and the other end of the ejection cylinder 213 is connected and fixed to the lower mold fixing plate 201. The oil circuits of the four ejection cylinders 213 are connected in series.

[0118] It should be noted that when the ejector cylinder 213 ejects, the ejector rod 212 will be ejected simultaneously, thereby ensuring the product is ejected smoothly. This avoids damage to the product's shape due to asynchronous ejection of the ejector rod 212, or the product being ejected at one end while the other end is stuck in the cavity 300. The synchronous ejection of the ejector rod 212 makes the production process more stable and reliable, and reduces the defect rate.

[0119] The composite material components prepared by the HP-RTM rapid prototyping method and mold provided by this invention have a shorter molding cycle, higher molding efficiency, lower manufacturing cost, and smooth double-sided products. By adding preforming and cutting steps, products with a thickness of ≥40mm can be prepared.

[0120] Example 1

[0121] A rapid prototyping method for composite material components using HP-RTM is provided for fabricating composite flat panel parts. The process includes the following steps:

[0122] (1) The required amount of resin was calculated to be 300g through simulation analysis. Before installing the injection head, the pressure of each component of the injection head was adjusted to 120bar. The HUNTSMAN 3585 epoxy resin, HUNTSMAN 3831 amine curing agent and internal release agent were preheated and vacuum degassed. The resin temperature was 80℃, the curing agent temperature was 45℃ and the internal release agent temperature was 25℃. The mixer was adjusted to a small flow circulation mode.

[0123] (2) Clean the impurities on the mold surface, start the press, and open the mold; apply CLE-705 external release agent evenly to the mold surface in small amounts multiple times, with each application being 10ml; heat the mold to 95℃.

[0124] (3) Use an automatic cutting machine to cut carbon fiber cloth into pieces of fixed shape, size and quantity according to the drawings. The thickness of a single layer is 0.6mm, and there are 5 layers in total. Lay them into the mold in the design order.

[0125] (4) After the press mold is closed and locked, apply a clamping force of 5000kN;

[0126] (5) Open the vacuum control valve and evacuate for 3 minutes;

[0127] (6) After vacuuming is completed, close the vacuum control valve. Adjust the mixer to high-pressure circulation mode, mix HUNTSMAN3585 epoxy resin, HUNTSMAN 3831 amine curing agent and QZ12-IRA release agent in a mass ratio of 100:24:0.5 until uniform, and then inject the mixture into the fiber cloth in the mold through the injection head installed in the mold at the set injection flow rate of 50g / s and injection time of 6s.

[0128] (7) Hold pressure and cure for 10 minutes to allow the resin to cure and form quickly; after the curing process is completed, release the pressure, open the vacuum control valve to break the vacuum environment, and open the mold; after opening the mold, take out the product, cool it and remove the flash to obtain a composite material flat part.

[0129] Example 2

[0130] A rapid prototyping method for composite material components using HP-RTM (High-Performance-Time Molding) is provided for fabricating composite material leaf springs. The process includes the following steps:

[0131] (1) The required amount of resin was calculated to be 2100g through simulation. The pressure of each component in the dispensing head was adjusted to 140bar. The HUNTSMAN 3585 epoxy resin, HUNTSMAN 3831 amine curing agent and internal release agent were preheated and vacuum degassed. The resin temperature was 80℃, the curing agent temperature was 40℃ and the internal release agent temperature was 28℃. The mixer was adjusted to a low flow circulation mode.

[0132] (2) Clean the impurities on the mold surface, start the press, and open the mold; apply CLE-705 external release agent evenly to the mold surface in small amounts multiple times, with each application being 15ml; heat the mold to 90℃.

[0133] (3) Use an automatic cutting machine to cut carbon fiber cloth into pieces of fixed shape, size and quantity according to the drawings. The cut fiber cloth has 34 layers in total, with a single layer thickness of 1.2mm. After stacking in the layup order, it is transferred to the preforming press for pressing. After pressing, take out the blank with a thickness of 40mm and place it on the cutting fixture for fixing. Use an ultrasonic cutting knife installed on the robotic arm for cutting. The air supply pressure is 0.65MPa, the amplitude is 42%, the cutting speed is 20mm / s, the blade tip is always kept at 90° to the ground, and the cutting path is always kept parallel to the outer edge of the mold. Transfer the cut blank to the forming mold.

[0134] (4) After the press mold is closed and locked, apply a clamping force of 9000kN;

[0135] (5) Open the vacuum control valve and evacuate for 5 minutes;

[0136] (6) After vacuuming is completed, close the vacuum control valve. Adjust the mixer to high-pressure circulation mode, mix HUNTSMAN3585 epoxy resin, HUNTSMAN 3831 amine curing agent and QZ12-IRA release agent at a mass ratio of 100:24:0.5 until uniform, and then inject the mixture into the fiber cloth in the mold through the injection head installed in the mold at the set injection flow rate of 70g / s and injection time of 30s;

[0137] (7) Hold pressure and cure for 5 minutes to allow the resin to cure and form quickly; after the curing process is completed, release the pressure, open the vacuum control valve to break the vacuum environment, and open the mold; after opening the mold, take out the product, cool it and remove the flash to obtain a composite material leaf spring component with a thickness of 40mm.

[0138] Table 1 Comparison of molding data between embodiments of the present invention and existing processes.

[0139]

[0140] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.

Claims

1. A rapid prototyping method for composite material components using HP-RTM, characterized in that, The molding process is carried out using HP-RTM rapid prototyping molds, which include an upper mold, a lower mold, a vacuum system, a sealing structure, an airtight structure, a temperature control system, a pressure control system, and an ejection mechanism. The upper mold and the lower mold form a cavity. The upper mold is provided with a vacuum control valve mounting port, and the cavity is connected to the vacuum system through the vacuum control valve in the vacuum control valve mounting port; the vacuum control valve includes a valve stem and a valve sleeve, the valve stem and the valve sleeve forming a conical mechanical seal structure, the mating surfaces of the valve sleeve and the valve stem are provided with three sets of high-temperature resistant O-rings, and a fourth set of high-temperature resistant O-rings is provided between the valve sleeve and the upper mold core of the upper mold; the sealing structure is provided on the parting surface of the lower mold core of the lower mold and located outside the cavity, and the gas sealing structure is provided outside the sealing structure; The ejection mechanism includes four ejector rods, which are respectively located at 1 / 5a, 2 / 5a, 3 / 5a, and 4 / 5a of the lower mold core. The four ejector rods are mounted on the push plate, and each of the four ends of the push plate is provided with an ejection cylinder. The oil circuits of the four ejection cylinders are connected in series to achieve synchronous ejection. The temperature control system includes an upper mold temperature controller, a lower mold temperature controller, an upper mold temperature sensor, and a lower mold temperature sensor. The upper mold temperature sensor is located at 1 / 5a, 1 / 2a, and 4 / 5a of the upper mold core, and the lower mold temperature sensor is located at 1 / 5a, 1 / 2a, and 4 / 5a of the lower mold core; where a is the length of the upper mold core and the lower mold core. The pressure control system includes pressure sensors, which are respectively disposed at the connection points of the upper mold core and the two ends of the cavity, and are flush with the upper surface of the cavity; The method includes the following steps: Step 1: Based on the requirements of the composite material component to be prepared, calculate the required amount of resin through simulation analysis of the composite material component to be prepared; before installing the dispensing head, adjust the pressure of the raw material components at the nozzle of the dispensing head to 100-160 bar, and the pressure values ​​of the three components should not differ from each other by more than 10 bar; preheat the raw material, degas it under vacuum, and adjust the flow circulation mode of the mixer. The mixing machine uses a low-flow circulation mode, which is half the normal production flow rate. The preheating conditions for the raw materials are: resin temperature 85-90℃, curing agent temperature 45-50℃, and internal release agent temperature 25-30℃. The mass ratio of resin to curing agent in the raw materials is 100:23-100:25, and the mass ratio of resin to internal release agent is 100:0-100:

2. The resin is epoxy resin, and the curing agent is an amine-based curing agent. Step 2: Clean the mold and spray the external release agent; control the mold temperature through the temperature control system and raise it to 60-120℃; Step 3: According to the layup design requirements of the composite material component to be prepared, cut and lay the fiber cloth in sequence according to the drawings; Step 4: Transfer the laid-up fiber cloth to an oven for heating and insulation, then transfer it to a pre-forming press to apply pressure and press it into shape. After naturally cooling to room temperature, remove it to form a blank. Transfer the blank to a cutting fixture for fixation, and use an ultrasonic cutter to cut it into the shape of the target product. The conditions for ultrasonic cutting are: air supply pressure of 6-8 bar, cutting speed of 20-60 mm / s, the blade tip always keeping 90° to the ground during cutting, and the cutting path always keeping parallel to the outer edge of the mold; the oven heating temperature is 130-180℃, and the time is 60-120 min, so that the setting powder in the fiber cloth melts and sets, and the fiber bundles are kept intact after pressing. Step 5: Place the blank processed in step 4 into the mold cavity, and the press moves down to close the mold. Step 6: After the upper and lower molds are closed and locked, the press applies pressure. Step 7: After the press is pressurized, the vacuum control valve is controlled by the mold vacuum system. The vacuum control valve is opened to evacuate the cavity. The vacuum level is judged according to the vacuum gauge value to make the cavity reach a vacuum state. The vacuum control valve is closed by the vacuum system to make the cavity a vacuum state. Step 8: Inject resin at a certain injection pressure according to the set injection flow rate and injection time. After completion, maintain pressure and cure. After maintaining pressure and curing, release pressure, break vacuum, eject the ejector pin, cool, and remove flash in sequence. During injection, adjust the mixer to high-pressure circulation mode, with an injection flow rate of 30-150 g / s, an injection time of 5-300 s, and an injection pressure of 100-160 bar. The ejector rod demolding is achieved through the ejection mechanism. The oil circuits of the four ejection cylinders are connected in series, so that the four ejector rods are ejected synchronously, ensuring that the product is demolded smoothly. The thickness of the composite material component is ≥40mm.

2. The method according to claim 1, characterized in that, In step 2, the mold temperature is 60-95℃.

3. The method according to claim 1, characterized in that, In step 6, the pressure applied by the press is 1000-9000kN.

4. The method according to claim 1, characterized in that, In step 8, the pressure holding and curing time is 5-10 minutes.

Citation Information

Patent Citations

  • Manufacturing technology for FRP composite material plate spring body

    CN107553935A

  • Carbon fiber product HP-RTM forming process

    CN109910327A

  • Resin film permeation forming method of large-thickness resin-based composite material

    CN111409291A

  • Quick fashioned HP -RTM mould of combined material

    CN208452039U