A positive electrode active material and its preparation method and application
By developing doping-modified Na3V2(PO4)3 cathode active materials, the energy density and electrochemical performance of sodium batteries are improved, the problems of insufficient energy density of sodium batteries and the high cost of vanadium-based materials are solved, and high energy density and low cost are achieved. Cost of sodium battery applications.
Patent Information
- Application Number
- CN202210991524.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-18
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-08-18
AI Technical Summary
The energy density of sodium batteries is not as good as that of lithium batteries, and the high raw material cost of vanadium-based cathode materials limits their application.
Develop a cathode active material with the general molecular formula Nax-aAaVy-bMb(PO4)2-2c(DO4)2cFz-dQd. Through doping modification, the redox reaction capacity of Na ions and V elements is improved, and the V element is reduced. The molar percentage increases the energy density and increases the charge and discharge voltage through the introduction of phosphate groups and F elements.
It is possible to improve the energy density and electrochemical performance of sodium batteries at lower V element content, reduce material costs, and ensure structural stability and cycle performance.
Smart Images

Figure CN117638016B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of battery technology, and specifically to a positive electrode active material and a preparation method and application thereof. Background Art
[0002] At present, sodium batteries have the advantages of low cost, high safety, and fast charging capability, but the energy density of sodium batteries is not as good as that of lithium batteries. Improving the energy density of sodium batteries has gradually become a research hotspot. Na3V2(PO4)3 compound is one of the commonly used positive electrode active materials for sodium batteries. It has a high working voltage and good cyclability and safety. However, the high raw material cost of vanadium limits the application of vanadium-based positive electrode materials. Summary of the invention
[0003] In view of this, the embodiment of the present application provides a positive electrode active material. The average number of electrons that can be transferred per V element in the positive electrode active material during the charge and discharge process is greater than 1, so that a higher energy density can be achieved based on a lower vanadium content, so the amount of vanadium per unit energy storage is low, and the cost of the material is significantly reduced. In addition, on this basis, the positive electrode active material is doped and modified to further improve the electrochemical performance of the positive electrode active material.
[0004] The first aspect of the present application provides a positive electrode active material, wherein the molecular formula of the positive electrode active material includes Na x-a A a V y-b M b (PO4) 2-2c (DO4) 2c F z-d Q d , wherein the A element represents an alkali metal element doped to replace the Na element, the M element represents a metal element replacing the V element, the D element represents a doping element replacing the P element, the Q element represents a doping element replacing the F element, the D element includes at least one of Si and S, and the Q element includes at least one of Cl and O; 3.5≤x≤4.5, 0≤a≤0.15x, 0.8≤y≤1.1, 0≤b≤0.3y, 0≤c≤0.15, 0.8≤z≤1.1, 0≤d≤0.2z.
[0005] The above-mentioned positive electrode active material has a high content of active Na ions. During the charge and discharge process of the material, each V atom undergoes an oxidation-reduction reaction and can transfer more than one electron on average. Therefore, compared with the existing modified or unmodified Na3V2(PO4)3 materials, the above-mentioned positive electrode active material can have a higher specific capacity at a relatively low molar percentage of the V element, and thus has a higher energy density (that is, the content of the V element per unit of energy storage is low). In addition, the molar ratio of the phosphate group to the V element in the above-mentioned positive electrode active material is relatively high, and the introduced F element has a strong inductive effect, which is beneficial to improving the charge and discharge voltage of the positive electrode active material, so the energy density of the material can be further improved. On this basis, the Na x V y (PO4)2F z Doping modification can further improve the electrochemical properties of the material, such as ion and electronic conductivity. Controlling the doping amount of each doping element within a certain range can also avoid the situation where excessive doping causes the structure of the material to be destroyed or the material loses its electrochemical activity.
[0006] The second aspect of the present application provides a method for preparing a positive electrode active material, comprising the following steps:
[0007] (1) weighing a sodium source, a Na-doped A source, a vanadium source, a vanadium-doped M source, a phosphorus source, a phosphorus-doped D source, a fluorine source, and a fluorine-doped Q source in a molar ratio of Na:A:V:M:P:D:F:Q=(xa):a:(yb):b:(2-2c):2c:(zd):z, and mixing them to obtain a precursor material; wherein 3.5≤x≤4.5, 0≤a≤0.15x, 0.8≤y≤1.2, 0≤b≤0.3y, 0≤c≤0.15, 0.8≤z≤1.2, and 0≤d≤0.2z;
[0008] (2) calcining the precursor material in a protective atmosphere to obtain a positive electrode active material; wherein the molecular formula of the positive electrode active material includes Na x-a A a V y-b M b (PO4) 2-2c (DO4) 2c F z-d Q d ; The A element represents an alkali metal element doped to replace the Na element, the M element represents a metal element replacing the V element, the D element represents a doping element replacing the P element, and the Q element represents a doping element replacing the F element, the D element includes at least one of Si and S, and the Q element includes at least one of Cl and O.
[0009] The preparation method has simple steps and strong process controllability and is suitable for large-scale industrial preparation.
[0010] The third aspect of the present application provides a positive electrode plate, comprising the positive electrode active material provided in the first aspect of the present application. The positive electrode plate can be used to provide a sodium battery with high charge and discharge specific capacity, good rate performance and cycle stability, and low cost.
[0011] The fourth aspect of the present application provides a sodium battery, comprising the positive electrode plate provided in the third aspect of the present application.
[0012] The sodium battery has high charge and discharge specific capacity, good rate performance and cycle stability, and the cost of the sodium battery is low and the market competitiveness is strong. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 This is the X-ray diffraction (XRD) spectrum of the positive electrode active material of Example 9 of the present application;
[0014] Figure 2 The voltage-specific capacity curves of the batteries made from the positive electrode active materials of Example 9 and Comparative Example 2 of the present application. DETAILED DESCRIPTION
[0015] At present, sodium-ion batteries have the advantages of low cost, high safety, and fast charging capabilities, but the energy density of sodium-ion batteries is not as good as that of lithium-ion batteries. NASICON-type compounds are a class of polyanion materials with three-dimensional ion channels proposed by Professor Goodenough. When used in sodium-ion batteries, the most representative positive electrode active material is Na3V2(PO4)3 (hereinafter abbreviated as NVP). Although various literature reports have been published on the doping modification of one or more of the Na, V, and P positions of NVP materials to improve the energy density of NVP materials, the energy density improvement of such materials is mostly based on the following two principles: one is to stimulate the V element to undergo redox reactions at a higher valence state to a certain extent to increase the working voltage of the material, and the other is to increase the theoretical specific capacity of the material by reducing the molar mass of the material. However, each mole of doped and modified NVP material is still based on the V element undergoing V 5+ / V 4+ or V 4+ / V 3+ Theoretically, the V element can undergo a redox reaction based on V 5+ / V 4+ and V 4+ / V 3+However, the number of Na ions that can be released from the doped and modified NVP material is still limited, which cannot support the two-electron transfer reaction of the V element. Therefore, the improvement of the energy density of the material by the doping modification is limited. In other words, the capacity that each mole of V element in the material can contribute is still limited.
[0016] In order to solve the above problems, the present invention provides a positive electrode active material. The molecular formula of the positive electrode active material includes Na x-a A a V y-b M b (PO4) 2-2c (DO4) 2c F z-d Q d , wherein the A element represents an alkali metal element doped to replace the Na element, the M element represents a doping element doped to replace the V element, the D element represents a doping element doped to replace the P element, and the Q element represents a doping element doped to replace the F element; 3.5≤x≤4.5, 0.8≤y≤1.1, 0.8≤z≤1.1, 0≤a≤0.15x, 0≤b≤0.3y, 0≤c≤0.15, 0≤d≤0.2z.
[0017] The above positive electrode active material has a high molar content of active Na ions, which is because the V atoms in the positive electrode active material can achieve V 5+ / V 4+ and V 4+ / V 3+ The redox reaction of two electron transfer lays the foundation, so that some or all of the V atoms can undergo two electron transfer reactions, so that the average number of electrons that can be transferred by each V atom during the redox reaction is greater than 1. Therefore, compared with existing modified or unmodified NVP materials, the above-mentioned positive electrode active materials can have similar or higher specific capacity when the molar percentage of V element is relatively low, so they can have higher energy density (that is, the content of V element per unit energy storage energy is low). The higher Na ion content can also ensure that when the Na element is replaced by the A element, it will not affect the number of active alkali metal ions that can be released, and the lattice parameters can be adjusted by replacing other alkali metal ions, thereby improving the structural stability and electrochemical performance. In addition, the phosphate group in the above-mentioned positive electrode active material and the V element (PO4 3- The higher the molar ratio of V to anionic group, the more effective it is to increase the inductive effect of anionic groups on the V element, and the introduction of F atoms with stronger inductive effect is beneficial to increase the charge and discharge voltage of the positive electrode active material, so the energy density of the material can be further improved.
[0018] Furthermore, when there is M substitution or Q substitution, the ionic and electronic conductivity, structural stability and other properties of the material can be further improved. Controlling the doping amount of each doping element within a certain range can also avoid the situation where the structure of the material is destroyed or the material loses its electrochemical activity due to excessive doping.
[0019] In the present application, illustratively, the value of x can be 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, 4.4, 4.5, etc. Different values of x will change the proportion of V element or M element, or the content of F element or Q element can be adjusted to maintain the valence balance of the positive electrode active material.
[0020] In some embodiments of the present application, the value of x is in the range of 3.8-4.2. At this time, the content of active Na ions that can contribute to the capacity in the positive electrode active material is relatively higher, which can better support the two-electron transfer reaction during the charge and discharge process. In some specific embodiments, the value of x can be 4. At this time, illustratively, the molecular formula of the positive electrode active material can be Na4V(PO4)2F, etc.
[0021] In some embodiments of the present application, the A element includes but is not limited to at least one of K and Li. Li and K elements belong to the first main group alkali metal elements with Na elements and have similar properties. Doping a small amount of K or Li can slightly adjust the lattice parameters, which is more conducive to the rapid deintercalation of active Na ions and improves the ionic conductivity of the material.
[0022] In some embodiments of the present application, the value of y is in the range of 0.9-1.1. In some specific embodiments, the value of y is 1.
[0023] In some embodiments of the present application, the value of z is in the range of 0.9-1.1. At this time, while taking into account the stability of the material structure, it is more conducive to stimulating the V element to undergo redox reaction at a higher valence state, thereby ensuring that the material has a higher charge and discharge voltage and a higher energy density.
[0024] In some embodiments of the present application, the M element includes but is not limited to one or more of Fe, Cr, Al, Sc, Ga, In, Ti, Zr, Mn, Zn, Ni, Cu and Co. In other embodiments of the present application, in order to better balance the cost of the M element and the impact on the ion conductivity and working voltage of the material, the M element can be selected from one or more of Ti, Cr, Mn and Fe, among which Fe has the lowest cost.
[0025] In some embodiments of the present application, the D element includes but is not limited to at least one of Si and S. The above two elements replace part of the P atoms to improve the structural stability of the material and extend the cycle life of the material.
[0026] In some embodiments of the present application, the Q element includes at least one of Cl and O. The atomic radius of the above two elements is larger than that of F atoms. After Cl atoms and / or O atoms replace some F atoms, the material can be forced to undergo lattice expansion, thereby weakening the Coulomb force effect between Na ions and surrounding atoms, reducing the binding of surrounding atoms to Na ions, making it easier for Na ions to be removed / embedded, thereby improving the ionic conductivity of the material.
[0027] In some embodiments of the present application, the surface of the positive electrode active material also has a coating layer. Exemplarily, the material of the coating layer can be a conductive carbon material. The modification of the surface of the material by coating the conductive carbon material can significantly improve the electronic conductivity of the material, and can also generate a protective layer on the surface of the material, effectively reducing the risk of agglomeration of the granular material.
[0028] In some embodiments of the present application, the mass percentage of the conductive carbon material in the positive electrode active material is 1%-15%. Exemplarily, the mass percentage of the conductive carbon material in the positive electrode active material can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, etc. By controlling the content of the conductive carbon material within a suitable range, the thickness of the coating layer can be controlled within a suitable range, which can effectively ensure that the conductive carbon material can be fully wrapped on the surface of the positive electrode active material of the inner core, improve the electronic conductivity of the material, and prevent excessive conductive carbon material from reducing the percentage of the inner core positive electrode active material.
[0029] In the present application, based on the fact that the V element in the above-mentioned positive electrode active material can undergo a two-electron transfer reaction, the theoretical gram capacity of the positive electrode active material reaches 140mAh / g-160mAh / g. Correspondingly, in some embodiments of the present application, the gram capacity of the positive electrode active material is 80mAh / g-110mAh / g. Exemplarily, the gram capacity of the positive electrode active material can be 80mAh / g, 85mAh / g, 90mAh / g, 95mAh / g, 100mAh / g, 105mAh / g, 110mAh / g, etc. The V element in the above-mentioned material can undergo a two-electron transfer reaction, so although the molar percentage of the V element in the positive electrode active material is lower than that of Na3V2(PO4)3, the gram capacity of the positive electrode active material of the present application can still reach a relatively high level, which is conducive to significantly reducing the cost of raw materials.
[0030] The present invention also provides a method for preparing a positive electrode active material, comprising the following steps:
[0031] (1) weighing a sodium source, a Na-doped A source, a vanadium source, a vanadium-doped M source, a phosphorus source, a phosphorus-doped D source, a fluorine source, and a fluorine-doped Q source in a molar ratio of Na element: A element: V element: M element: P element: D element: F element: Q element = (xa): a: (yb): b: (2-2c): 2c: (zd): z, and mixing them to obtain a precursor material; wherein 3.5≤x≤4.5, 0.8≤y≤1.2, 0.8≤z≤1.2, 0≤a≤0.15x, 0≤b≤0.3y, 0≤c≤0.15, and 0≤d≤0.2z;
[0032] (2) calcining the precursor material in a protective atmosphere to obtain a positive electrode active material; wherein the molecular formula of the positive electrode active material includes Na x-a A a V y-b M b (PO4) 2-2c (DO4) 2c F z-d Q d ; Among them, the A element represents an alkali metal element doped to replace the Na element, the M element represents a doping element doped to replace the V element, the D element represents a doping element doped to replace the P element, and the Q element represents a doping element doped to replace the F element.
[0033] The above preparation method only needs to mix the raw materials in a preset ratio to obtain a precursor material, and then calcine at high temperature to obtain the battery material provided in the embodiment of the present application. This preparation method has simple steps, strong process controllability, and can realize large-scale industrial preparation.
[0034] In the present application, in order to compensate for the loss of alkali metal elements during the preparation process, alkali metal elements (Na element and A element) may be added in an excess amount of 10%.
[0035] In some embodiments of the present application, the mixing treatment method in step (1) includes but is not limited to a solid phase mixing method or a sol-gel method.
[0036] The specific steps of the solid phase mixing method may be: adding the sodium source, A source, vanadium source, M source, phosphorus source, D source, fluorine source and Q source into a ball mill in proportion, and mixing to obtain a precursor material.
[0037] The specific steps of the sol-gel method may be: adding the sodium source, A source, vanadium source, M source, phosphorus source, D source, fluorine source and Q source to a solvent in proportion, heating and stirring to react and generate a gel, and continuing heating and stirring to evaporate the solvent in the obtained gel to obtain the above-mentioned precursor material. The heating and stirring temperature may be 60°C-120°C.
[0038] In the present application, the above-mentioned solvent is a volatile solvent, and specifically can be one or more of water, ethanol, ethylene glycol, etc.
[0039] In the present application, the sodium source may be at least one of sodium acetate, sodium formate, sodium carbonate, sodium nitrate, sodium oxalate, sodium citrate, sodium acetylacetonate, and the like.
[0040] In the present application, the above-mentioned A source (A element is at least one of Li and K) can be at least one of the corresponding Li or K nitrate, oxalate, carbonate, acetate and acetylacetonate.
[0041] In the present application, the vanadium source includes but is not limited to at least one of vanadium sources in which the vanadium element is trivalent, tetravalent or pentavalent in the compound. For example, the vanadium source may be at least one of vanadium pentoxide, vanadium tetroxide, vanadium trioxide, ammonium metavanadate, sodium metavanadate, vanadium acetylacetonate and vanadyl acetylacetonate.
[0042] In the present application, the M source is a compound familiar to those skilled in the art. For example, at least one of an organic metal salt, a metal acid salt, and a metal oxide of a specific element corresponding to the M element. Exemplarily, when the M element is Ti, the M source can be at least one of tetrabutyl titanate, isopropyl titanate, tetraethyl titanate, etc.
[0043] In the present application, the above-mentioned phosphorus source can be at least one of phosphoric acid, sodium phosphate, sodium dihydrogen phosphate, disodium hydrogen phosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, ammonium phosphate, etc.
[0044] In the present application, the D source may be at least one of an acid, an ester or a salt of a specific doping element corresponding to the D element. For example, when the D element is Si, the D source may be tetraethyl silicate, sodium silicate or the like.
[0045] In the present application, the fluorine source may be at least one of sodium fluoride, ammonium fluoride, hydrofluoric acid, sodium bifluoride, and the like.
[0046] In the present application, the Q source may correspond to a compound of O and Cl. For example, when the Q element is O, the Q source may be sodium carbonate, sodium nitrate, a doped metal oxide, etc. When the Q element is Cl, the Q source may be sodium chloride, hydrogen chloride, etc.
[0047] In some embodiments of the present application, step (1) further includes adding a carbon source, such as an organic carbon source, to a solvent or a solid phase mixing device. After the organic carbon source is evenly mixed with the above raw materials, a precursor material with an organic carbon source is obtained, and then after calcination in step (2), the organic carbon source can be thermally cracked and carbonized, and finally a carbon coating layer is formed on the surface of the positive electrode active material.
[0048] In the present application, the organic carbon source is a material well known to those skilled in the art. For example, the organic carbon source can be at least one of citric acid, sodium citrate, oxalic acid, sodium oxalate, sucrose, fructose, ascorbic acid and glucose.
[0049] In some embodiments of the present application, the molar ratio of the mass of the carbon source added in step (1) to the V element in the raw material is (0.5-10): 1. By controlling the molar ratio of the organic carbon source to the V element in the raw material, the mass percentage of the carbon material in the finally formed positive electrode active material with a carbon coating layer can be controlled, thereby ensuring good electrochemical performance of the material.
[0050] In some embodiments of the present application, the calcination conditions in step (2) are: calcination at a temperature of 600° C.-900° C. for 1 h-24 h.
[0051] In the present application, the protective gas described in step (2) can specifically be at least one of argon, nitrogen, argon-hydrogen gas or nitrogen-hydrogen gas.
[0052] The embodiment of the present application also provides a positive electrode plate, comprising the positive electrode active material provided in the embodiment of the present application.
[0053] The positive electrode plate can be used to provide a sodium battery with high energy density, good cycle performance and safety performance.
[0054] In some embodiments of the present application, the positive electrode sheet generally includes a positive electrode current collector and a positive electrode active material layer disposed on at least one side of the positive electrode current collector, wherein the positive electrode active material layer contains the positive electrode active material. In addition, the positive electrode active material layer may also contain a binder and an optional conductive agent. Among them, the binder and the conductive agent may be conventional choices in the battery field.
[0055] The positive electrode current collector may be any material suitable for use as a current collector for a positive electrode sheet, including but not limited to metal single substance foil, alloy foil, metal-plated polymer film material, or the aforementioned material with carbon coated on the surface, etc. Among them, the metal single substance foil material may specifically be aluminum foil, the alloy foil material may be aluminum alloy foil, and the metal plated on the surface of the polymer film material may be an aluminum single substance layer or an aluminum alloy layer.
[0056] The present application also provides a sodium battery. x-a A a V y-b M b (PO4) 2-2c (DO4) 2c F z-d Q dThe material is used as the positive electrode active material, and has high energy density, good cycle performance and safety performance. The sodium battery can be used in 3C electronic products (such as mobile phones, tablet computers, etc.), transportation tools (such as cars, ships, etc.) or other electrical equipment to improve the performance and market competitiveness of electrical equipment.
[0057] Among them, the sodium battery can be a liquid battery using a liquid electrolyte, or a semi-solid or solid battery using a semi-solid electrolyte or a solid electrolyte. In some embodiments, the secondary battery may include the above-mentioned positive electrode sheet, negative electrode sheet, and a diaphragm and electrolyte disposed between the positive electrode sheet and the negative electrode sheet. In other embodiments, the sodium battery may include a positive electrode sheet, a negative electrode sheet, and a semi-solid electrolyte or a solid electrolyte disposed between the positive electrode sheet and the negative electrode sheet. In addition, when a semi-solid electrolyte or a solid electrolyte is used, the positive electrode sheet and the negative electrode sheet may also contain a semi-solid electrolyte material or a solid electrolyte material.
[0058] The technical solution of the present application is further described in detail below with multiple embodiments.
[0059] Example 1
[0060] 3.00mmol of sodium source-sodium acetate, 0.50mmol of vanadium source-vanadium pentoxide, 2.00mmol of phosphorus source-ammonium dihydrogen phosphate, 1.00mmol of fluorine source-sodium fluoride (Na element in sodium fluoride is also a sodium source, the same below) (that is, the molar ratio of Na element: V element: P element: F element is 4:1:2:1) is added to 30mL of deionized water, stirred and heated to 80°C, and stirred continuously at 80°C until the solvent evaporates to obtain a dry gel precursor material. The precursor material is collected and transferred to a tubular furnace, calcined at 700°C under argon atmosphere protection, and naturally cooled to room temperature after keeping warm for 8h to obtain the positive electrode active material-Na4V(PO4)2F.
[0061] Example 2
[0062] The only difference from Example 1 is that the raw material also contains a D source - ammonium sulfate, so that the molar ratio of Na element: V element: P element: S element: F element is 3.5:1.1:1.8:0.2:1.0, and the positive electrode active material - Na 3.5 V 1.1 (PO4) 1.8 (SO4) 0.2 F.
[0063] Example 3
[0064] The only difference from Example 1 is that the raw material also contains M source - manganese acetate and D source - tetraethyl silicate, so that the molar ratio of Na element: V element: Mn element: P element: Si element: F element is 4.5:0.7:0.3:1.8:0.2:1.0, and the positive electrode active material - Na 4.5 V 0.7 Mn 0.3 (PO4) 1.8 (SiO4) 0.2 F.
[0065] Example 4
[0066] The only difference from Example 1 is that the raw material also contains A source - potassium acetate, so that the molar ratio of Na element: K element: V element: P element: F element in the raw material is 3.4:0.6:1:2:1, and the positive electrode active material - Na 3.4 K 0.6 V(PO4)2F.
[0067] Example 5
[0068] The only difference from Example 1 is that the raw material also contains M source - manganese acetate, so that the molar ratio of Na element: V element: Mn element: P element: F element in the raw material is 4.3:0.7:0.3:2:1, and the above raw materials are added to a ball mill, a small amount of ethanol is added, and the ball milling is carried out at a speed of 400 rpm for 5 hours. The fully mixed raw materials are vacuum dried in a vacuum oven at 110°C for 2 hours to obtain a precursor material, which is transferred to a tubular furnace and calcined at 700°C under argon atmosphere protection. After keeping warm for 8 hours, it is naturally cooled to room temperature to obtain the positive electrode active material - Na 4.3 V 0.7 Mn 0.3 (PO4)2F.
[0069] Example 6
[0070] The only difference from Example 1 is that the raw material also contains a D source - sodium sulfate, so that the molar ratio of the raw material Na element: V element: P element: S element: F element is 3.7:1:1.7:0.3:1, and the positive electrode active material - Na 3.7 V(PO4) 1.7 (SO4) 0.3 F.
[0071] Example 7
[0072] The only difference from Example 1 is that the raw material also contains a Q source - sodium chloride, so that the molar ratio of Na element: V element: P element: F element: Cl element in the raw material is 4:1:2:0.8:0.2, and the positive electrode active material - Na4V(PO4)2F is finally prepared.0.8 Cl 0.2 .
[0073] Example 8
[0074] The difference from Example 1 is that the raw material also contains A source - potassium acetate, M source - manganese acetate, D source - sodium sulfate, Q source - sodium chloride, so that the molar ratio of Na element: K element: V element: Mn element: P element: S element: F element: Cl element in the raw material is 3.7: 0.3: 0.9: 0.1: 1.9: 0.1: 0.9: 0.1; the above raw materials are added to a ball mill, and then a small amount of ethanol is added, and the ball milling treatment is carried out at a speed of 400 rpm for 5 hours. The fully mixed raw materials are vacuum dried in a vacuum oven at 110°C for 2 hours to obtain a precursor material, which is transferred to a tubular furnace and calcined at 700°C under argon atmosphere protection. After keeping warm for 8 hours, it is naturally cooled to room temperature to obtain the positive electrode active material - Na 3.7 K 0.3 V 0.9 Mn 0.1 (PO4) 1.9 (SO4) 0.1 F 0.9 Cl 0.1 .
[0075] Example 9
[0076] Weigh 3.00mmol of sodium acetate as a sodium source, 0.50mmol of vanadium pentoxide as a vanadium source, 1.00mmol of sodium fluoride as a fluorine source, 2.00mmol of ammonium dihydrogen phosphate as a phosphorus source (i.e., the molar ratio of Na element: V element: P element: F element is 4:1:2:1), and 4.00mmol of citric acid as a carbon source. Add vanadium pentoxide to 30mL of deionized water, stir and heat to 80°C, add citric acid, stir for 10min, and obtain a blue clear solution; then add the above sodium acetate, sodium fluoride, and ammonium dihydrogen phosphate to the blue clear solution. Continue stirring at 80°C until evaporated to obtain a dry gel precursor material. Collect the dry gel, place it in a tubular furnace, calcine it at 700°C under the protection of an argon atmosphere, keep it warm for 8h, and then cool it naturally to room temperature to obtain a positive electrode active material-Na4V(PO4)2F with a carbon coating on the surface, recorded as Na4V(PO4)2F@C.
[0077] Example 10
[0078] The only difference from Example 10 is that the vanadium source is replaced by ammonium metavanadate, the fluorine source is replaced by ammonium fluoride, the phosphorus source is replaced by 85% phosphoric acid, and the molar ratio of Na element: V element: P element: F element is 4:1:2:1. The final positive electrode active material is Na4V(PO4)2F with a carbon coating layer on the surface, recorded as Na4V(PO4)2F@C.
[0079] Embodiment 11
[0080] Weigh 12.00mmol of sodium acetate as a sodium source, 2.00mmol of vanadium pentoxide as a vanadium source, 4.00mmol of sodium fluoride as a fluorine source, 8.00mmol of ammonium dihydrogen phosphate as a phosphorus source (i.e., the molar ratio of Na element: V element: P element: F element is 4:1:2:1), and 16.00mmol of citric acid as a carbon source. Place the above raw materials in a ball mill, add a small amount of ethanol, and mill at a speed of 400rpm for 5h. Collect the fully mixed raw materials and vacuum dry them in a vacuum oven at 110°C for 2h to obtain a precursor material, which is then transferred to a tube furnace and calcined at 700°C under argon atmosphere protection. After keeping the temperature for 8h, it is naturally cooled to room temperature to obtain a positive electrode active material - Na4V(PO4)2F with a carbon coating layer on the surface, recorded as Na4V(PO4)2F@C.
[0081] Comparative Example 1
[0082] A positive electrode active material, whose general molecular formula is Na3V2(PO4)3.
[0083] Comparative Example 2
[0084] Weigh 3.00mmol of sodium acetate as a sodium source, 1.00mmol of vanadium pentoxide as a vanadium source, 3.00mmol of ammonium dihydrogen phosphate as a phosphorus source (i.e., the molar ratio of Na element: V element: P element is 3:4:3), and 4.00mmol of citric acid as a carbon source. Add vanadium pentoxide to 30mL of deionized water, stir and heat to 80°C, add citric acid, stir for 10min, and obtain a blue clear solution; then add the above sodium acetate and ammonium dihydrogen phosphate to the blue clear solution. Continue stirring at 80°C until evaporated to obtain a dry gel precursor material. Collect the dry gel, place it in a tubular furnace, calcine it at 800°C under the protection of argon atmosphere, keep it warm for 6h, and then cool it naturally to room temperature to obtain the positive electrode active material-Na3V2(PO4)3 with a carbon coating on the surface, recorded as Na3V2(PO4)3@C.
[0085] Performance Testing
[0086] (1) XRD test was performed on some samples of the examples (specifically Example 9), and the results were as follows: Figure 1 shown.
[0087] (2) Electrochemical performance test, including the following steps:
[0088] a) The positive electrode active material, conductive agent-carbon black, and binder-PVDF provided in the above embodiments and comparative examples are added to the solvent N-methylpyrrolidone (NMP) at a mass ratio of 8:1:1, and then stirred in a vacuum mixer to form a stable and uniform positive electrode slurry. The above positive electrode slurry is coated on the current collector-aluminum foil to obtain a positive electrode sheet;
[0089] b) cutting a sodium metal sheet of suitable size as a negative electrode;
[0090] c) dissolving 1 mol of sodium salt -NaPF6 in 1 L of an organic solvent (the volume ratio of ethylene carbonate to diethyl carbonate is 1:1) to obtain an electrolyte;
[0091] d) In a glove box, under an Ar gas atmosphere, the positive electrode sheet, separator, and negative electrode sheet prepared in step (2) are alternately stacked and injected with electrolyte to prepare a CR2032 button battery.
[0092] e) Gram capacity test of positive electrode active material: Each of the above button cells was charged at a constant current of 0.1C until the voltage reached the corresponding cut-off voltage, and then discharged at a constant current of 0.1C to the corresponding cut-off voltage after standing for 5 minutes. The gram capacity of the material was measured, and the results are summarized in Table 1.
[0093] f) Charge and discharge voltage test: The battery of the embodiment and the comparative example battery are subjected to charge and discharge cycle test at a current density of 0.1C; wherein the charge cut-off voltage of the embodiment battery is 5.0V, the discharge cut-off voltage is 2.0V, and the charge and discharge curve of the battery is recorded; the charge cut-off voltage of the comparative example battery is 3.8V, and the discharge cut-off voltage is 2.5V. The charge and discharge curve of the battery is recorded, and the voltage value at the intersection of the charge and discharge curves is recorded as the charge and discharge voltage of the battery. The charge and discharge curves of Example 9 and Comparative Example 1 are shown in FIG. Figure 2 The rest of the data results are summarized in Table 1.
[0094] Table 1 Summary of electrochemical performance results of the positive electrode active materials of the batteries of various embodiments and comparative examples
[0095] Experiment number Molecular formula of positive electrode active material Gram capacity (mAh / g) Charge and discharge voltage (V) Example 1 <![CDATA[Na4V(PO4)2F]]> 80 3.75 Example 2 <![CDATA[Na 3.5 V 1.1 (PO4) 1.8 (SO4) 0.2 F]]> 82 3.76 Example 3 <![CDATA[Na 4.5 V 0.7 Mn 0.3 (PO4) 1.8 (SiO4) 0.2 F]]> 95 3.76 Example 4 <![CDATA[Na 3.4 K 0.6 V(PO4)2F]]> 85 3.78 Example 5 <![CDATA[Na 4.3 V 0.7 Mn 0.3 (PO4)2F]]> 102 3.78 Example 6 <![CDATA[Na 3.7 V(PO4) 1.7 (SO4) 0.3 F]]> 105 3.77 Example 7 <![CDATA[Na4V(PO4)2F 0.8 Cl 0.2 ]]> 88 3.79 Example 8 <![CDATA[Na 3.7 K 0.3 V 0.9 Mn 0.1 (PO4) 1.9 (SO4) 0.1 F 0.9 Cl 0.1 ]]> 108 3.81 Example 9 <![CDATA[Na4V(PO4)2F@C]]> 115 3.81 Example 10 <![CDATA[Na4V(PO4)2F@C]]> 105 3.80 Embodiment 11 <![CDATA[Na4V(PO4)2F@C]]> 100 3.80 Comparative Example 1 <![CDATA[Na3V2(PO4)3]]> 78 3.35 Comparative Example 2 <![CDATA[Na3V2(PO4)3@C]]> 107 3.37
[0096] It can be seen from the data in Table 1 that the positive electrode active material provided in the embodiment of the present application has a higher charge and discharge voltage than the NVP material; at the same time, by comparing Example 1 and Comparative Example 1, and Example 9 and Comparative Example 2, it can be seen that after excluding other influencing factors, the molar ratio of vanadium element / phosphorus element of the positive electrode active material of the embodiment is lower, but its gram capacity is higher than that of the corresponding comparative example, which fully illustrates the superiority of the positive electrode active material provided in the embodiment of the present application. In addition, the gram capacity of the positive electrode active materials in the above-mentioned embodiments did not reach their theoretical gram capacity. In this case, there are many factors that affect the material capacity. Therefore, it is understandable that there are differences in the measured gram capacity between the embodiments.
[0097] The above is an exemplary embodiment of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made thereto without departing from the principles of the present application. These improvements and modifications are also considered to be within the scope of protection of the present application.
Claims
1. A positive electrode active material, characterized in that: The molecular formula of the positive electrode active material includes Na x-a A a V y-b M b (PO4) 2-2c (DO4) 2c F z-d Q d , wherein the A element represents an alkali metal element doped to replace the Na element, the M element represents a metal element replacing the V element, the D element represents a doping element replacing the P element, and the Q element represents a doping element replacing the F element, the D element includes at least one of Si and S, and the Q element includes at least one of Cl and O; 3.5≤x≤4.5, 0≤a≤0.15x, 0.8≤y≤1.1, 0≤b≤0.3y, 0≤c≤0.15, 0.8≤z≤1.1, 0≤d≤0.2z; the M element includes at least one of Fe, Cr, Al, Sc, Ga, In, Ti, Zr, Mn, Zn, Ni, Cu and Co.
2. The positive electrode active material according to claim 1, characterized in that The A element includes at least one of K and Li.
3. The positive electrode active material according to claim 1, characterized in that The value of x is 3.8-4.
2.
4. The positive electrode active material according to claim 1, characterized in that The value of y is 0.9-1.
1.
5. The positive electrode active material according to claim 1, characterized in that The value of z is 0.9-1.
1.
6. The positive electrode active material according to claim 1, characterized in that The surface of the positive electrode active material also has a coating layer.
7. The positive electrode active material according to any one of claims 1 to 6, characterized in that: The gram capacity of the positive electrode active material is 80 mAh / g-110 mAh / g.
8. A method for preparing a positive electrode active material, characterized in that: The following steps are involved: (1) weighing a sodium source, a Na-doped A source, a vanadium source, a vanadium-doped M source, a phosphorus source, a phosphorus-doped D source, a fluorine source, and a fluorine-doped Q source in a molar ratio of Na:A:V:M:P:D:F:Q=(xa):a:(yb):b:(2-2c):2c:(zd):z, and mixing them to obtain a precursor material; wherein 3.5≤x≤4.5, 0≤a≤0.15x, 0.8≤y≤1.2, 0≤b≤0.3y, 0≤c≤0.15, 0.8≤z≤1.2, and 0≤d≤0.2z; (2) calcining the precursor material in a protective atmosphere to obtain a positive electrode active material; wherein the molecular formula of the positive electrode active material includes Na x-a A a V y-b M b (PO4) 2-2c (DO4) 2c F z-d Q d ; The A element represents an alkali metal element doped to replace the Na element, the M element represents a metal element replacing the V element, the D element represents a doping element replacing the P element, and the Q element represents a doping element replacing the F element, the D element includes at least one of Si and S, and the Q element includes at least one of Cl and O; the M element includes at least one of Fe, Cr, Al, Sc, Ga, In, Ti, Zr, Mn, Zn, Ni, Cu and Co.
9. The preparation method according to claim 8, characterized in that: The calcination conditions are: calcination at a temperature of 600° C.-900° C. for 1 h-24 h.
10. A positive electrode sheet, characterized in that: The positive electrode sheet comprises the positive electrode active material according to any one of claims 1 to 7.
11. A sodium battery, characterized in that: The sodium battery comprises the positive electrode sheet as claimed in claim 10.