A perovskite solar cell and its fabrication method, and a photovoltaic module.
By employing a two-step method to prepare perovskite layers in perovskite solar cells, forming a heterojunction where a first perovskite sublayer fills the valley bottom and a second perovskite sublayer covers the valley tip, the problem of difficult cation solution diffusion is solved, thereby improving electron transport and device efficiency.
Patent Information
- Application Number
- CN202311648430.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-01
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-12-01
AI Technical Summary
In existing perovskite solar cells, the high density of the lead halide framework layer makes it difficult for the cation solution to diffuse to the valley of the pyramid base, resulting in incomplete lead iodide reaction, which hinders the separation and transport of photogenerated carriers, leading to low device efficiency.
A two-step method was used to prepare the perovskite layer. First, a lead halide framework layer was deposited on the substrate by vapor deposition. Then, a cationic solution was coated to form a first perovskite sublayer that filled the valley bottom and a second perovskite sublayer that covered the valley tip, forming a heterojunction and improving electron transport performance.
This effectively solves the problem of difficult transport of photogenerated electrons to the bottom cell, improves the interfacial contact performance and electron transport performance of the perovskite layer, reduces photogenerated carrier recombination, and improves device efficiency.
Smart Images

Figure CN117641950B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of solar cells, and more particularly to a perovskite solar cell, its preparation method, and a photovoltaic module. Background Technology
[0002] The perovskite layer is an important component of perovskite solar cells. Currently, the perovskite layer produced in industrial perovskite solar cells is mainly prepared by vapor deposition-solution method. That is, a lead halide framework layer is first vapor deposited on a pyramid-shaped substrate, and then a cationic solution is coated on the lead halide framework layer. The cationic solution diffuses into the lead halide framework layer to react and form perovskite.
[0003] However, the high density of the vapor-deposited lead halide framework layer makes it difficult for the cation solution to diffuse to the valleys of the pyramid substrate, resulting in incomplete lead iodide reaction at the valleys. This residual lead iodide hinders the separation of photogenerated carriers, leading to severe recombination between residual lead iodide and holes and electrons at the perovskite interface. This impedes the transport of photogenerated electrons or holes to the bottom cell, resulting in low device efficiency. Summary of the Invention
[0004] To address the problem of low device efficiency caused by the difficulty in transferring photogenerated electrons to the bottom cell, this application provides a perovskite solar cell, its fabrication method, and a photovoltaic module.
[0005] In one aspect, this application provides a perovskite solar cell.
[0006] This perovskite solar cell includes:
[0007] The base has a velvety surface structure, which has valley peaks and valley bottoms;
[0008] The perovskite layer includes a first perovskite sublayer and a second perovskite sublayer disposed above a substrate. The first perovskite sublayer fills the valley bottom of the substrate, and the second perovskite sublayer covers the first perovskite sublayer and the valley tip. A heterojunction is formed between the first perovskite sublayer and the second perovskite sublayer. The second perovskite sublayer is obtained by reacting a lead halide framework layer with a cation solution.
[0009] As an optional implementation, in the embodiments of the present invention, the perovskite solar cell has a nip structure or a pin structure. When the perovskite solar cell has a nip structure, the band gap of the first perovskite sublayer is 1.72 eV to 2.3 eV, and the band gap of the second perovskite sublayer is 1.63 eV to 1.72 eV, with the band gap of the first perovskite sublayer being larger than that of the second perovskite sublayer. When the perovskite solar cell has a pin structure, the band gap of the first perovskite sublayer is 1.2 eV to 1.63 eV, and the band gap of the second perovskite sublayer is 1.63 eV to 1.72 eV, with the band gap of the first perovskite sublayer being smaller than that of the second perovskite sublayer.
[0010] As an optional implementation, in an embodiment of the present invention, the band gap difference between the first perovskite sublayer and the second perovskite sublayer is 0.05 eV to 0.58 eV.
[0011] When the band gap of the first perovskite sublayer is 1.72 eV to 2.3 eV, the first perovskite sublayer is Cs. x1 FA y1 MA 1-x1-y1 Pb(I z Br 1-z1 )3, wherein x1 = 0~1, y1 = 0~1, and z1 = 0~1; when the band gap of the first perovskite sublayer is 1.2eV~1.63eV, the first perovskite sublayer is FA. x2 MA 1-x2 Pb y2 Sn 1-y2 (I z2 B r1-z2 )3, wherein x2 = 0 to 1, y2 = 0 to 1, and z2 = 0 to 1.
[0012] As an optional implementation, in an embodiment of the present invention, the velvet structure is a pyramid structure, the first perovskite sublayer filling the valley has an inverted pyramid shape, the second perovskite sublayer includes alternating peaks and flat sections, the peaks are located above the valley tips and the shapes of the peaks and valley tips are matched, and the flat sections are located above the first perovskite sublayer.
[0013] As an optional implementation, in an embodiment of the present invention, the thickness of the first perovskite sublayer is 100 nm to 500 nm, and the thickness of the second perovskite sublayer is 500 nm to 1 μm.
[0014] As an optional implementation, in an embodiment of the present invention, the lead halide framework layer has alternating sharp framework portions and flat framework portions, the sharp framework portions being located above the valley tips and matching the shape of the sharp framework portions with the valley tips, and the flat framework portions being located above the first perovskite sublayer; and / or, the thickness of the lead halide framework layer is 350 nm to 800 nm.
[0015] As an optional implementation, in embodiments of the present invention, the lead halide framework layer comprises lead iodide and cesium bromide; and / or,
[0016] The solute in the cation solution includes one or more of iodoformamidine, bromoformamidine, chloroformamidine, iodoformamine, bromoformamine, and chloroformamine, and the solvent in the cation solution includes one or two of anhydrous ethanol and isopropanol.
[0017] As an optional implementation, in an embodiment of the present invention, the concentration of iodoformamidine in the cation solution is 0.3 mol / L to 0.6 mol / L, the concentration of bromomethylamine is 0 mol / L to 0.2 mol / L, the concentration of chloromethylamine is 0 mol / L to 0.15 mol / L, the concentration of bromoformamidine is 0 mol / L to 0.6 mol / L, the concentration of chloroformamidine is 0 mol / L to 0.2 mol / L, and the concentration of iodoformamidine is 0 mol / L to 0.2 mol / L.
[0018] As an optional implementation, in an embodiment of the present invention, the perovskite solar cell is a perovskite-silicon tandem solar cell, the substrate includes a texturized silicon substrate cell and a composite layer and a first transport layer sequentially stacked on the texturized silicon substrate cell, the perovskite layer being stacked on the surface of the first transport layer, and the perovskite solar cell further includes:
[0019] A second transport layer stacked on the perovskite layer on the side of the texturized silicon substrate cell away from the cell.
[0020] A transparent electrode layer stacked on the side of the second transport layer facing away from the textured silicon substrate cell;
[0021] One of the first transport layer and the second transport layer is an electron transport layer, and the other is a hole transport layer;
[0022] It also includes a positive electrode and a negative electrode, wherein the positive electrode forms an ohmic contact with the transparent electrode layer and the negative electrode forms an ohmic contact with the texturized silicon bottom cell.
[0023] As an optional implementation, in embodiments of the present invention, the texturized silicon bottom cell includes one or more of the following: emitter passivation and back contact cell, tunnel oxide passivation contact cell, heterojunction cell, heterojunction back contact crystalline silicon cell, and tunnel oxide passivation back contact cell; and / or,
[0024] The composite layer is made of one or both of indium tin oxide and indium zinc oxide; the hole transport layer is made of one or more of nickel oxide, cuprous oxide, Spiro-TTB, and cuprous thiocyanate; and / or,
[0025] The material of the electron transport layer includes C. 60 ; and / or,
[0026] The material of the transparent electrode layer includes one or both of indium tin oxide and indium zinc oxide.
[0027] As an optional implementation, in embodiments of the present invention, the thickness of the composite layer is 20 nm to 30 nm; and / or,
[0028] The thickness of the hole transport layer is 20nm to 30nm; and / or,
[0029] The thickness of the electron transport layer is 10 nm to 30 nm; and / or,
[0030] The thickness of the transparent electrode layer is 80nm to 120nm.
[0031] As an optional implementation, in an embodiment of the present invention, the perovskite solar cell further includes:
[0032] A passivation layer located between the perovskite layer and the electron transport layer; and / or an antireflection layer located on the side of the transparent electrode layer opposite to the fabrication of the texturized silicon substrate cell.
[0033] As an optional implementation, in an embodiment of the present invention, the material of the passivation layer includes C. 60 The material of the antireflective layer includes one or two of fullerene derivatives PCBM; and / or, the material of the antireflective layer includes one or two of magnesium fluoride and lithium fluoride.
[0034] As an optional implementation, in embodiments of the present invention, the thickness of the passivation layer is 1 nm to 5 nm; and / or,
[0035] The thickness of the antireflective layer is 100nm to 120nm.
[0036] As an optional implementation, in an embodiment of the present invention, the perovskite solar cell is a single-junction perovskite solar cell, the substrate includes a textured transparent electrode layer and a first transport layer stacked on the textured transparent electrode layer, the perovskite layer is stacked on the surface of the first transport layer, and the perovskite solar cell further includes:
[0037] A second transport layer is stacked on the side of the perovskite layer away from the textured transparent electrode layer, wherein one of the first transport layer and the second transport layer is an electron transport layer and the other is a hole transport layer;
[0038] It also includes a positive electrode and a negative electrode, wherein the positive electrode forms an ohmic contact with the second transport layer and the negative electrode forms an ohmic contact with the textured transparent electrode layer.
[0039] Secondly, this application provides a method for preparing a perovskite solar cell.
[0040] The fabrication method of perovskite solar cells includes the following steps:
[0041] Provide a substrate: the surface of the substrate has a velvety structure, the velvety structure having valley peaks and valley bottoms;
[0042] Preparation of the first perovskite sublayer: The first perovskite sublayer is deposited on the substrate by solution deposition, followed by annealing to obtain the first perovskite sublayer filling the valley bottom;
[0043] Preparation of the second perovskite sublayer: A lead halide framework layer for shape preservation is prepared on the first perovskite sublayer, so that the lead halide framework layer covers the first perovskite sublayer and the valley tip. A cationic solution is coated on the lead halide framework layer, and annealing is performed to form a perovskite heterojunction between the first perovskite sublayer and the second perovskite sublayer, thus obtaining the perovskite layer.
[0044] As an optional implementation, in embodiments of the present invention, the solution method includes any one of spin coating, blade coating, spray coating, or slot coating; and / or,
[0045] The lead halide framework layer is prepared by a dual-source co-evaporation process using lead iodide and cesium bromide, wherein the evaporation rate ratio of lead iodide to cesium bromide is 5:1 to 10:1; and / or,
[0046] Methods for applying the cationic solution include spin coating and slot coating; and / or,
[0047] In the step of preparing the first perovskite sublayer, the annealing treatment is either direct annealing or antisolvent engineering combined with thermal annealing. In the direct annealing, the annealing temperature is 80℃~150℃ and the annealing time is 10min~30min. In the antisolvent engineering combined with thermal annealing, the antisolvent includes one or more of diethyl ether, toluene, ethyl acetate, chlorobenzene, and chloroform, and the thermal annealing temperature is 100℃~150℃ and the thermal annealing time is 10min~30min; and / or,
[0048] In the step of preparing the second perovskite sublayer, the annealing treatment is carried out at a humidity of 5%RH to 60%RH, with an inert gas stream blowing through the surface of the lead halide framework layer after coating with the cationic solution, and annealing at 80℃ to 100℃ for 15 min to 30 min.
[0049] As an optional implementation, in an embodiment of the present invention, the perovskite solar cell is a perovskite-silicon tandem solar cell, and the method for preparing the perovskite solar cell further includes the following steps:
[0050] Preparation of the substrate: A texturized silicon substrate cell is provided, a composite layer is prepared on the texturized silicon substrate cell, and a first transport layer is prepared on the composite layer;
[0051] Preparation of the perovskite layer: The perovskite layer is prepared on the substrate, and the perovskite layer is stacked on the surface of the first transport layer;
[0052] Fabrication of a second transport layer: A second transport layer is fabricated on the perovskite layer, wherein one of the first transport layer and the second transport layer is an electron transport layer and the other is a hole transport layer;
[0053] Fabrication of a transparent electrode layer: The transparent electrode layer is fabricated on the second transport layer;
[0054] A positive electrode and a negative electrode are prepared to obtain the perovskite solar cell.
[0055] As an optional implementation, in the embodiments of the present invention, the composite layer is prepared by magnetron sputtering; and / or, the hole transport layer is prepared by physical vapor deposition or evaporation; and / or, the electron transport layer is prepared by evaporation; and / or, the transparent electrode layer is prepared by magnetron sputtering, and the positive electrode is prepared by evaporation; and / or, the negative electrode is prepared by evaporation.
[0056] As an optional implementation, in an embodiment of the present invention, a passivation layer is further prepared between the perovskite layer and the electron transport layer, the passivation layer being prepared by vapor deposition; and / or, an antireflection layer is prepared on the side of the transparent electrode layer away from the texturized silicon substrate, the antireflection layer being prepared by vapor deposition.
[0057] As an optional implementation, in an embodiment of the present invention, the perovskite solar cell is a single-junction perovskite solar cell, and the method for preparing the perovskite solar cell further includes the following steps:
[0058] Preparation of the substrate: A textured transparent electrode layer is provided, and a first transport layer is prepared on the textured transparent electrode layer;
[0059] Preparation of the perovskite layer: The perovskite layer is prepared on the substrate, and the perovskite layer is stacked on the surface of the first transport layer;
[0060] Fabrication of a second transport layer: A second transport layer is fabricated on the perovskite layer, wherein one of the first transport layer and the second transport layer is an electron transport layer and the other is a hole transport layer;
[0061] A positive electrode and a negative electrode are prepared to obtain the perovskite solar cell.
[0062] Thirdly, embodiments of the present invention provide a photovoltaic module, which includes the perovskite solar cell described in the first aspect or the perovskite solar cell prepared by the preparation method described in the second aspect.
[0063] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0064] This invention provides a perovskite solar cell in which a first perovskite sublayer fills the valley of the substrate, preventing lead iodide residue at the interface between the perovskite layer and the substrate. This solves the problem of lead iodide residue at the perovskite layer interface, which is detrimental to interface contact and hinders electron transport, thus improving the contact performance and electron transport performance of the perovskite layer interface. In addition to preventing lead iodide formation at the interface, the first perovskite sublayer deposited in the valley also combines with the second perovskite sublayer to form a local heterojunction. The bandgap structure and built-in electric field of this heterojunction enhance the charge separation and transport capabilities within the perovskite layer at the valley, better promoting electron separation and photogenerated electron and hole transfer at the interface. This reduces photogenerated carrier recombination at the valley bottom, overcoming the defect that residual lead iodide easily forms a high-energy barrier with the perovskite layer, hindering photogenerated carrier separation, and improving device efficiency. Attached Figure Description
[0065] To more clearly illustrate the technical solutions in the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0066] Figure 1This is a schematic diagram of a two-step method for preparing perovskite layers, combining thermal evaporation and solution methods.
[0067] Figure 2 In the present invention, (A) is a schematic diagram of the recombination of photogenerated carriers at the interface before the deposition of the first perovskite sublayer, as disclosed in the embodiment of the present invention, and (B) is a schematic diagram of the built-in electric field formed at the interface between the first perovskite and the second perovskite after the deposition of the first perovskite sublayer, as disclosed in the embodiment of the present invention, and the promoting effect of the built-in electric field on the separation of photogenerated holes.
[0068] Figure 3 This is a schematic diagram of the preparation of the perovskite layer disclosed in the embodiments of the present invention;
[0069] Figure 4 This is a schematic diagram of a perovskite solar cell disclosed in an embodiment of the present invention;
[0070] Figure 5 This is a schematic diagram of the preparation steps for the first perovskite sublayer;
[0071] Figure 6 This is a top-view SEM image of the first perovskite sublayer.
[0072] Icons: 100, Substrate; 11, Texturized Silicon Substrate; 12, Composite Layer; 13, First Transport Layer; 14, Passivation Layer; 200, Perovskite Layer; 21, First Perovskite Sublayer; 211, Perovskite Precursor Solution; 22, Second Perovskite Sublayer; 221, Lead Halide Framework Layer; 2211, Sharp Framework Section; 2212, Flat Framework Section; 222, Cation Solution; 223, Sharp Peak Section; 224, Flat Section; 300, Second Transport Layer; 400, Transparent Electrode Layer; 500, Antireflection Layer; 600, Positive Electrode; 700, Negative Electrode. Detailed Implementation
[0073] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0074] There are two methods for preparing perovskite layers on textured substrates. The first method involves a one-step solution coating process to apply a perovskite precursor solution onto the textured substrate. This method maintains the uniformity of the perovskite layer composition, with no localized lead iodide residues or impurities. However, this one-step solution method is suitable for preparing perovskite layers on polished substrates or silicon-based solar cells with a pyramid height of less than 1 μm. When the pyramid height exceeds 2 μm, the perovskite layer prepared by the one-step solution method cannot completely cover the pyramid tip of the substrate, leading to short circuits or low device efficiency. The second method is a two-step process combining vapor deposition and solution preparation to prepare the perovskite layer. (Refer to...) Figure 1 By first depositing a shape-preserving lead halide framework layer onto a textured substrate, and then coating a cationic solution onto the lead halide framework layer, a perovskite layer with excellent texture preservation can be obtained. This method is not limited by the height of the pyramid and can achieve better shape preservation on taller pyramid substrates.
[0075] However, the lead halide framework layer prepared by vapor deposition has a high degree of density. When the lead halide framework layer is thick, the cation solution has difficulty diffusing to the bottom of the dense lead halide framework layer, resulting in insufficient reaction of lead iodide at the bottom and a tendency for reaction residue to occur. (Refer to...) Figure 2 In part (A), these residual lead iodide particles hinder the separation of photogenerated carriers, causing severe recombination of residual lead iodide with holes and electrons at the perovskite interface, which hinders the transport of photogenerated electrons or holes to the bottom cell, resulting in low device efficiency.
[0076] Furthermore, the thicker the lead halide framework layer, the more lead iodide remains at the bottom of the valley, and the greater the obstruction to electron transport.
[0077] This application provides a perovskite solar cell and its preparation method, as well as a photovoltaic module, which can effectively solve the problem of difficulty in the transmission of photogenerated electrons or holes to the bottom cell, and at the same time solve the problem that lead iodide residue is prone to appear at the bottom of the valley of the thick perovskite layer, so as to better improve the light absorption effect of the perovskite solar cell.
[0078] The technical solution of the present invention will be further described below with reference to the embodiments and accompanying drawings.
[0079] In a first aspect, embodiments of this application provide a perovskite solar cell.
[0080] This perovskite solar cell includes:
[0081] A substrate 100 with a velvety surface structure, wherein the velvety surface structure has valley peaks and valley bottoms;
[0082] The perovskite layer 200 includes a first perovskite sublayer 21 and a second perovskite sublayer 22 disposed above the substrate 100. The first perovskite sublayer 21 fills the valley bottom of the substrate 100, and the second perovskite sublayer 22 covers the first perovskite sublayer 21 and the valley tip. A heterojunction is formed between the first perovskite sublayer 21 and the second perovskite sublayer 22. The second perovskite sublayer 22 is obtained by reacting a lead halide framework layer 221 with a cation solution 222.
[0083] The structural relationship between the perovskite layer 200 and the substrate 100 is shown below. Figure 3 This application fills the valley of the substrate 100 with a first perovskite sublayer 21, avoiding the presence of lead iodide residue at the interface between the perovskite layer 200 and the substrate 100. This solves the problem of lead iodide residue at the interface of the perovskite layer 200, which is detrimental to interface contact and hinders electron transport, thus improving the contact performance and electron transport performance of the perovskite layer 200 interface. In addition to preventing lead iodide from appearing at the interface, the first perovskite sublayer 21 deposited at the valley also combines with the second perovskite sublayer 22 to form a local heterojunction. The bandgap structure and built-in electric field of this heterojunction enhance the charge separation and transport capabilities within the perovskite layer at the valley, better promoting electron separation and photogenerated electron and hole transfer at the interface. This reduces photogenerated carrier recombination at the valley bottom, overcoming the defect that residual lead iodide easily forms a high-energy barrier with the perovskite layer 200, hindering photogenerated carrier separation, and improving device efficiency.
[0084] The textured substrate 100 described above can be provided by a textured silicon substrate or other textured conductive substrate. The specific type of substrate 100 is not specifically limited. For example, when the substrate 100 is selected as a textured silicon substrate, the resulting solar cell is a perovskite silicon tandem solar cell. When the substrate 100 is selected as a textured transparent conductive glass substrate, the resulting solar cell is a single-junction perovskite solar cell.
[0085] In some embodiments, the perovskite solar cell has a nip structure or a pin structure. When the perovskite solar cell has a nip structure, the band gap of the first perovskite sublayer 21 is 1.72 eV to 2.3 eV, and the band gap of the second perovskite sublayer 22 is 1.63 eV to 1.72 eV, with the band gap of the first perovskite sublayer 21 being larger than that of the second perovskite sublayer 22. When the perovskite solar cell has a pin structure, the band gap of the first perovskite sublayer 21 is 1.2 eV to 1.63 eV, and the band gap of the second perovskite sublayer 22 is 1.63 eV to 1.72 eV, with the band gap of the first perovskite sublayer 21 being smaller than that of the second perovskite sublayer 22.
[0086] When a perovskite solar cell has a pin structure, the first perovskite sublayer 21 is made of a perovskite material with a band gap of 1.2 eV to 1.63 eV, such as FA. x MA 1-x Pb y Sn 1-y (I z B r1-z )3, where x² = 0 to 1, y² = 0 to 1, z² = 0 to 1. (This is achieved through FA.) x MA 1-x Pb y Sn 1-y (I z B r1-z )3 cation FA + MA + Sn 2+ and Pb 2+ Or I- with Br - The ratio can be freely adjusted to achieve a band gap of 1.2 eV to 1.63 eV for the first perovskite sublayer 21.
[0087] The second perovskite sublayer 22 is prepared by reacting the lead halide framework layer 221 with the cation solution 222 to obtain a perovskite layer 200 with a band gap of 1.63 eV to 1.72 eV. The band gap of the second perovskite sublayer 22 can be freely adjusted in the range of 1.63 eV to 1.72 eV by adjusting the ratio of Cs to FA and MA elements or the ratio of I to Br.
[0088] After annealing, a heterojunction is formed between the first perovskite sublayer 21 and the second perovskite sublayer 22. The band structure of the heterojunction bends and the built-in electric field is enhanced, which promotes the separation of holes and electrons in the perovskite layer 200.
[0089] from Figure 2 A comparison of parts (A) and (B) shows that when the above-mentioned perovskite tandem solar cell has a nip structure, the band gap of the first perovskite sublayer 21 is selected as 1.72 eV to 2.3 eV. Electrons are transported from the second perovskite sublayer 22 with a band gap of 1.63 eV to 1.72 eV towards the first perovskite sublayer 21 with a band gap of 1.72 eV to 2.3 eV. A heterojunction is formed through the first perovskite sublayer 21 and the second perovskite sublayer 22 with the aforementioned band gap. The built-in electric field of this heterostructure can effectively promote the charge separation and transport capabilities within the perovskite, thereby improving the cell's conversion efficiency.
[0090] When the above-mentioned perovskite tandem solar cell has a pin structure, the band gap of the first perovskite sublayer 21 is selected to be 1.2eV to 1.63eV. Electrons are transported from the first perovskite sublayer 21 with a band gap of 1.2eV to 1.63eV to the second perovskite sublayer 22 with a band gap of 1.63eV to 1.72eV, thereby improving the electron separation and transport capabilities inside the perovskite, and thus improving the efficiency of the device.
[0091] Furthermore, the first perovskite sublayer 21 with a band gap of 1.72 eV to 2.3 eV and the second perovskite sublayer 22 with a band gap of 1.63 eV to 1.72 eV absorb light of different wavelengths. The combination of the two as the perovskite layer 200 is beneficial to increase the light absorption of the perovskite layer 200 in the short wavelength range, improve the spectral utilization rate, and thus improve the overall efficiency of the electric field.
[0092] Preferably, the band gap difference between the first perovskite sublayer 21 and the second perovskite sublayer 22 is 0.05 eV to 0.58 eV.
[0093] When the band gap difference between the first perovskite sublayer 21 and the second perovskite sublayer 22 is 0.05 eV to 0.58 eV, the built-in electric field of the aforementioned heterostructure effectively promotes electron transport. However, if the band gap difference is too high, it can easily damage the perovskite structure and decrease the stability of the perovskite layer 200. Conversely, if the band gap difference is too small, the potential energy of the built-in electric field is too low, resulting in insufficient carrier migration capacity, decreased electron migration efficiency, and consequently, reduced energy conversion efficiency. More preferably, the band gap difference between the first perovskite sublayer 21 and the second perovskite sublayer 22 is 0.05 eV to 0.1 eV.
[0094] In some embodiments, the thickness of the first perovskite sublayer 21 is 100 nm to 500 nm, and the thickness of the second perovskite sublayer 22 is 500 nm to 1 μm.
[0095] A first perovskite sublayer 21 with a thickness of 100nm to 500nm is stacked at the bottom of the pyramid substrate 100, which provides better filling effect at the bottom of the pyramid substrate 100. This can better shorten the diffusion path of the cation solution 222 in the lead halide framework layer 221, and better reduce the reaction difficulty between the cation solution 222 and the lead halide framework layer 221, thereby better reducing the residual lead iodide reaction. Furthermore, by limiting the thickness of the first perovskite sublayer 21 to a specific range, the heterojunction formed between the first perovskite sublayer 21 and the second perovskite sublayer 22 is closer to the interface, which is more effective in improving charge separation at the interface, thereby further reducing the recombination of electrons and holes at the interface and improving the conversion efficiency of the battery.
[0096] The thickness of the first perovskite sublayer 21 is too low, resulting in a longer diffusion path of the cation solution 222 in the lead halide framework layer 221. This increases the difficulty of the reaction between the cation solution 222 and the lead iodide at the bottom, and increases the amount of lead iodide remaining in the perovskite layer 200.
[0097] The excessive thickness of the first perovskite sublayer 21 is detrimental to obtaining a lead halide framework layer 221 with a textured surface and shape-preserving effect. Furthermore, the relatively large distance between the heterojunction formed between the first and second perovskite sublayers 21 and the interface results in poor charge separation at the interface. In addition, the excessive thickness of the wide-bandgap first perovskite sublayer 21 leads to low visible light absorption and an excessively long diffusion length of photogenerated carriers, resulting in increased recombination and ultimately reducing device efficiency.
[0098] For example, the thickness of the first perovskite sublayer 21 can be 100nm, 200nm, 300nm, 400nm, 500nm, etc. The thickness of the second perovskite sublayer 22 can be 500nm, 700nm, 900nm, 1000nm, 1μm, etc.
[0099] In some embodiments, the lead halide framework layer 221 includes alternating pointed framework portions 2211 and flat framework portions 2212, the pointed framework portions 2211 being located above the valley tips and matching the shape of the valley tips, and the flat framework portions 2212 being located above the first perovskite sublayer 21; and / or, the thickness of the lead halide framework layer 221 is 350 nm to 800 nm.
[0100] For example, the thickness of the lead halide framework layer 221 can be 300nm, 350nm, 400nm, 450nm, 500nm, 550nm, 600nm, 650nm, 700nm, 750nm and 800nm, etc.
[0101] It should be noted that, referring to Figure 3 The thickness of the first perovskite sublayer 21 is h1, which is the distance from the bottom of the valley of the substrate 100 to the top of the first perovskite sublayer 21. The thickness of the lead halide framework layer 221 is h2, which is the distance from the tip of the valley of the substrate 100 to the top of the framework portion of the lead halide framework layer 221. The thickness of the second perovskite sublayer 22 is h3, which is the distance from the tip of the valley of the substrate 100 to the top of the peak portion 223 of the second perovskite sublayer 22.
[0102] In some embodiments, the velvet structure is a pyramid structure, with the first perovskite sublayer 21 filled in the valley having an inverted pyramid shape, and the second perovskite sublayer 22 including alternating peaks 223 and flattened portions 224, the peaks 223 being located above the valley tips and matching the shape of the peaks 223, and the flattened portions 224 being located above the first perovskite sublayer 21.
[0103] The first perovskite sublayer 21 fills the valley bottom and does not completely cover the valley tip of the substrate 100. Therefore, the second perovskite sublayer 22 uses the surface of the first perovskite sublayer 21 and the valley tip as the growth substrate 100, and finally obtains a perovskite layer 200 with the shape of the peak 223 and the shape of the valley tip preserved, and the shape of the flattened part 224 and the shape of the first perovskite sublayer 21 preserved.
[0104] Because the first perovskite sublayer 21 filling the valley has an inverted pyramid shape, it replaces the lead halide framework layer 221 in filling the valley. This shortens the diffusion distance of the cation solution 222 within the lead halide framework layer 221, making it easier for the cation solution 222 to enter the bottom of the lead halide framework layer 221 and react fully with lead iodide. Therefore, the scheme of this application can effectively reduce the reaction difficulty between the lead halide framework layer 221 and the cation solution 222, overcoming the limitation that when the lead halide framework layer 221 is thick, the cation solution 222 has difficulty entering the bottom of the lead halide framework layer 221 to react fully with lead iodide. This is highly advantageous for preparing perovskite layers 200 with higher thicknesses.
[0105] The perovskite layer 200, composed of the second perovskite sublayer 22 and the first perovskite sublayer 21, not only avoids lead iodide residue at the valley bottom, but also possesses unique structural advantages as it is not a traditional conformal structure: the peak 223 of the second perovskite sublayer 22 matches the shape of the valley tip. This conformal structure allows the perovskite layer 200 to retain the light-trapping advantage unique to the textured structure, which helps reduce light reflection. Simultaneously, it also has a flattened portion 224, on which subsequent functional films grown along the surface of the second perovskite sublayer 22 grow, improving coverage uniformity and reducing the likelihood of functional film material accumulating at the valley bottom. Figure 2 and Figure 4 As shown (see the structure of the perovskite layer 200, which is not completely conformal), Figure 2 , Figure 4 (This illustration shows the stacking order of the various films in a perovskite solar cell, but does not depict structures that are not fully conformally grown.) A passivation layer 14 is stacked on the perovskite layer 200. The passivation layer 14, which grows conformally along the structure of the perovskite layer 200, provides more uniform coverage and more thorough passivation. For example, the positive electrode 600, compared to contacting the pyramid-shaped transparent electrode layer 400, has a larger and flatter contact surface with the transparent electrode layer 400, which grows conformally along the structure of the perovskite layer 200, resulting in higher contact stability. Therefore, preparing subsequent films on the perovskite layer 200 with the above structure can improve the passivation effect of the passivation layer 14 and simultaneously improve the electrode charge collection efficiency, thereby improving the energy conversion efficiency of the cell.
[0106] In some embodiments, the lead halide framework layer 221 comprises lead iodide and cesium bromide; and / or,
[0107] The solute of cationic solution 222 includes one or more combinations of iodoformamidine, bromoformamidine, chloroformamidine, iodoformamine, bromoformamine, and chloroformamine, and the solvent of cationic solution 222 includes one or two of anhydrous ethanol and isopropanol.
[0108] The proportions and concentrations of the above-mentioned cationic components can be adjusted appropriately according to the requirements of the usage environment. Furthermore, in cationic solution 222, the concentrations of formamidinium iodoformide are 0.3 mol / L to 0.6 mol / L, the concentrations of methyl bromide are 0 mol / L to 0.2 mol / L, the concentrations of methyl chloroformide are 0 mol / L to 0.15 mol / L, the concentrations of formamidinium iodoformide are 0 mol / L to 0.6 mol / L, the concentrations of methyl bromide are 0 mol / L to 0.2 mol / L, and the concentrations of methyl bromide are 0 mol / L to 0.2 mol / L.
[0109] In some embodiments, the perovskite solar cell is a perovskite-silicon tandem solar cell, as referenced. Figure 4 The substrate 100 includes a texturized silicon substrate 11 and a composite layer 12 and a first transport layer 13 sequentially stacked on the texturized silicon substrate. A perovskite layer 200 is stacked on the surface of the first transport layer 13. The perovskite solar cell also includes:
[0110] A second transport layer 300 is stacked on the side of the perovskite layer 200 facing away from the texturized silicon substrate cell 11;
[0111] A transparent electrode layer 400 is stacked on the side of the second transport layer 300 facing away from the textured silicon bottom cell 11;
[0112] One of the first transport layer 13 and the second transport layer 300 is an electron transport layer, and the other is a hole transport layer;
[0113] It also includes a positive electrode 600 and a negative electrode 700. The positive electrode 600 forms an ohmic contact with the transparent electrode layer 400, and the negative electrode 700 forms an ohmic contact with the texturized silicon bottom cell 11.
[0114] It should be noted that one of the first transport layer 13 and the second transport layer 300 is an electron transport layer and the other is a hole transport layer. That is, when the first transport layer 13 is an electron transport layer, the second transport layer 300 is a hole transport layer, and when the first transport layer 13 is a hole transport layer, the second transport layer 300 is an electron transport layer.
[0115] The aforementioned textured silicon substrate 11 has a pyramid structure. The composite layer 12 and electron transport layer stacked on the textured silicon substrate 11 are both conformally grown films following the pyramid shape of the textured silicon substrate 11. The perovskite layer 200 stacked on the electron transport layer has reduced lead iodide residue and improved crystallinity. Although it matches the structure of the electron transport layer, it is not completely conformally grown relative to the textured silicon substrate 11, composite layer 12, and electron transport layer (see the structure of the not completely conformally grown perovskite layer 200 for details). Figure 3 , Figure 4 The diagram illustrates the overall structure of the perovskite solar cell (excluding the partially conformal perovskite layer 200). However, the light-trapping effect of this partially conformal structure retains the advantages of light trapping to some extent, while also possessing the advantages of good contact stability and better contact effect. Therefore, the defects in the hole transport layer and transparent electrode layer 400 grown along the structure of the perovskite layer 200 are reduced, ultimately improving the energy conversion efficiency of the resulting perovskite tandem solar cell.
[0116] In some embodiments, the texturized silicon bottom cell 11 includes one or more of the following: emitter passivation and back contact cell, tunnel oxide passivation contact cell, heterojunction cell, heterojunction back contact crystalline silicon cell, and tunnel oxide passivation back contact cell; and / or,
[0117] The composite layer 12 is made of one or both of indium tin oxide and indium zinc oxide; the hole transport layer is made of one or more of Spiro-OMeTAD, PTAA, and cuprous thiocyanate, wherein Spiro-OMeTAD is 2,2′,7,7′-tetra(N,N-di-p-methoxyphenylamine))9,9′-spirodifluorene, and PTAA is poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine]; and / or,
[0118] The electron transport layer material includes one or both of tin oxide and titanium dioxide; and / or,
[0119] The transparent electrode layer 400 is made of one or both of indium tin oxide and indium zinc oxide.
[0120] In some embodiments, the thickness of the composite layer 12 is 20 nm to 30 nm; and / or,
[0121] The hole transport layer has a thickness of 20 nm to 30 nm; and / or,
[0122] The thickness of the electron transport layer is 10 nm to 30 nm; and / or,
[0123] The thickness of the transparent electrode layer 400 is 80nm to 120nm.
[0124] In some embodiments, the perovskite solar cell further includes:
[0125] Passivation layer 14, which is located between perovskite layer 200 and electron transport layer; and / or,
[0126] Antireflection layer 500 is located on the side of transparent electrode layer 400 away from the fabricated textured silicon substrate 11.
[0127] In some embodiments, the material of the passivation layer 14 includes lithium fluoride; and / or,
[0128] The antireflective layer 500 is made of one or both of magnesium fluoride and lithium fluoride.
[0129] In the above-mentioned film layers, the passivation layer 14 on the heterojunction bottom cell grows conformally along the pyramid shape of the heterojunction bottom cell. Since the structure of the perovskite layer 200 is similar to the pyramid structure, but not completely conformally, the antireflection layer 500 prepared subsequently grows conformally along the structure of the perovskite layer 200.
[0130] In some embodiments, the passivation layer 14 has a thickness of 1 nm to 5 nm; and / or, the antireflection layer 500 has a thickness of 100 nm to 120 nm.
[0131] In some embodiments, the perovskite solar cell is a single-junction perovskite solar cell, the substrate 100 includes a textured transparent electrode layer and a first transport layer 13 stacked on the textured transparent electrode layer, the perovskite layer 200 is stacked on the surface of the first transport layer 13, and the single-junction perovskite solar cell further includes:
[0132] A second transport layer 300 is stacked on the side of the perovskite layer 200 away from the textured transparent electrode layer. One of the first transport layer 13 and the second transport layer 300 is an electron transport layer, and the other is a hole transport layer.
[0133] It also includes a positive electrode 600 and a negative electrode 700. The positive electrode 600 forms an ohmic contact with the second transport layer 300, and the negative electrode 700 forms an ohmic contact with the textured transparent electrode layer.
[0134] For example, the textured transparent electrode layer is textured conductive glass.
[0135] It should be noted that one of the first transport layer 13 and the second transport layer 300 is an electron transport layer and the other is a hole transport layer. That is, when the first transport layer 13 is an electron transport layer, the second transport layer 300 is a hole transport layer, and when the first transport layer 13 is a hole transport layer, the second transport layer 300 is an electron transport layer.
[0136] Secondly, embodiments of this application provide a method for preparing a perovskite solar cell.
[0137] The fabrication method of perovskite solar cells includes the following steps:
[0138] Substrate 100 is provided: The surface of substrate 100 is a velvety structure with valley tips and valley bottoms;
[0139] Preparation of the first perovskite sublayer 21: The first perovskite sublayer 21 is deposited on the substrate 100 by solution method, followed by annealing to obtain the first perovskite sublayer 21 filling the valley bottom.
[0140] Preparation of the second perovskite sublayer 22: A lead halide framework layer 221 for shape preservation is prepared on the first perovskite sublayer 21, so that the lead halide framework layer 221 covers the first perovskite sublayer 21 and the valley tip. A cationic solution 222 is coated on the lead halide framework layer 221, and annealing is performed to form a perovskite heterojunction between the first perovskite sublayer 21 and the second perovskite sublayer 22, resulting in perovskite layer 200.
[0141] Reference Figure 5 In the step of preparing the first perovskite sublayer 21, a perovskite precursor solution 211 is coated on the substrate 100. Taking advantage of the fluidity of the perovskite precursor solution 211, the perovskite precursor solution 211 accumulates autonomously at the bottom of the valley of the substrate 100. Then, the solvent is removed by annealing, so that the first perovskite sublayer 21 grows along the shape of the valley of the substrate 100, resulting in a first perovskite sublayer 21 with an inverted pyramid shape that is adapted to the size of the valley of the substrate 100.
[0142] The first perovskite sublayer 21 at the bottom of the valley is prepared using a one-step solution method. The material used is perovskite, avoiding the use of lead iodide, which would easily lead to lead iodide residue at the bottom of the valley. At the same time, during the preparation of the first perovskite sublayer 21 by the above solution method, the solution for preparing the first perovskite sublayer 21 flows along the pyramid slope at the bottom of the valley and accumulates there. After annealing, it forms an inverted pyramid shape that matches the shape of the valley bottom.
[0143] The second perovskite sublayer 22 is prepared by a two-step method: first, a shape-preserving lead halide framework layer 221 is deposited, and then a cationic solution 222 is coated on the lead halide framework layer 221. The cationic solution 222 diffuses into the lead halide framework layer 221, and annealing causes the lead halide framework layer 221 and the cationic solution 222 to react and crystallize rapidly, forming the second perovskite sublayer 22. The lead halide framework layer 221 is grown on the alternating surfaces of the first perovskite sublayer 21 and the valley tip surfaces not covered by the first perovskite sublayer 21 as the growth substrate 100. Therefore, the lead halide framework layer 221 is grown according to the alternating surfaces of the first perovskite sublayer 21 and the valley tip surfaces not covered by the first perovskite sublayer 21. The resulting lead halide framework layer 221 has alternating sharp framework portions 2211 and flat framework portions 2212, wherein the sharp framework portions 2211 are located above the valley tips, and the shape of the sharp framework portions 2211 is consistent with the shape of the valley tips, and the flat framework portions 2212 are located above the first perovskite sublayer 21. Compared to the conventional two-step method, the first perovskite sublayer 21 replaces the bottom of the lead halide framework layer 221, thus shortening the thickness of the flat framework portion 2212. After the cationic solution 222 is coated, the diffusion distance on the lead halide framework layer 221 is shortened, which is conducive to the cationic solution 222 fully contacting and reacting with the bottom of the lead halide framework layer 221, thereby effectively reducing the residual lead iodide at the bottom of the lead halide framework layer 221 and improving the crystal quality of the perovskite layer 200.
[0144] Furthermore, the heterojunction formed between the first perovskite sublayer 21 and the second perovskite sublayer 22 of the above structure is close to the valley bottom. The built-in electric field built by this heterostructure helps to further reduce electron or hole recombination at the perovskite interface and improve the electron or hole transport efficiency at the perovskite interface.
[0145] In some embodiments, the solution method includes any one of spin coating, blade coating, spray coating, or slot coating; and / or,
[0146] The lead halide framework layer 221 is prepared by a dual-source co-evaporation process, in which lead iodide and cesium bromide are deposited at a rate of 5:1 to 10:1; and / or,
[0147] Methods for applying cationic solution 222 include spin coating and slot coating; and / or,
[0148] In the step of preparing the first perovskite sublayer 21, the annealing treatment is either direct annealing or antisolvent engineering combined with thermal annealing. In direct annealing, the annealing temperature is 80℃~150℃ and the annealing time is 10min~30min. In antisolvent engineering combined with thermal annealing, the antisolvent includes one or more of diethyl ether, toluene, ethyl acetate, chlorobenzene and chloroform, and the thermal annealing temperature is 100℃~150℃ and the thermal annealing time is 10min~30min.
[0149] In the step of preparing the second perovskite sublayer 22, the annealing treatment is carried out at a humidity of 5%RH to 60%RH, with an inert gas stream blowing through the surface of the lead halide framework layer 221 after coating with cationic solution 222, and annealing at 80℃ to 100℃ for 15 min to 30 min.
[0150] Compared to direct annealing, the process of combining anti-solvent engineering with annealing is beneficial to improving the crystallinity of the first perovskite sublayer 21, reducing defects, and obtaining a perovskite layer 200 with better performance.
[0151] The lead halide framework layer 221 prepared by the above-mentioned evaporation rate ratio is beneficial to adjust the band gap of the second perovskite sublayer 22 to be between 1.63 eV and 1.72 eV. At the same time, the lead halide framework layer 221 has a high degree of density. The first perovskite sublayer 21 replaces the lead halide framework layer 221 to fill the valley bottom. The cation solution 222 can also easily diffuse to the valley bottom of the lead halide framework layer 221. This effectively reduces the residual lead iodide reaction at the bottom of the highly dense lead halide framework layer 221, improves the reaction degree of the lead halide framework layer 221, and thus improves the crystal quality of the perovskite layer 200.
[0152] Using the first perovskite sublayer 21 and the valley tip together as the substrate 100 for preparing the lead halide framework layer 221, a dual-source co-evaporation process is employed to co-deposit lead iodide and cesium bromide on the surface of the substrate 100. The evaporation rate ratio of lead iodide to cesium bromide is 5:1 to 10:1. The lead halide framework layer 221 uses the valley tip and the first perovskite sublayer 21 as the growth substrate 100. The thickness of the lead halide framework layer 221 along the vertical direction is determined, such as the distance from the valley tip of the substrate 100 to the tip of the lead halide framework layer 221. The distance to the top of the framework 2211 is preset to h2. Then, lead iodide and cesium bromide are deposited by a dual-source co-evaporation process, so that a specific ratio of lead iodide and cesium bromide grows along the valley tip and the surface of the first perovskite sublayer 21 until the distance from the valley tip of the substrate 100 to the top of the lead halide framework 221 reaches h2, thus obtaining the lead halide framework 221. On this basis, the second perovskite sublayer 22 is obtained by reacting the lead halide framework 221 with the cation solution 222.
[0153] Next, the ambient humidity was controlled to be less than 10% RH and the temperature to be 25℃. The cationic solution 222 was coated onto the surface of the lead halide framework layer 221 using spin coating or slot coating. After coating, during the annealing process at a humidity of 5% RH to 60% RH, an inert gas stream at room temperature or below room temperature was introduced to purge the surface of the lead halide framework layer 221 coated with the cationic solution 222. This lowered the perovskite phase transition temperature and prevented the first perovskite sublayer 21 from being destroyed and recrystallized during the annealing of the second perovskite sublayer 22 due to excessively high annealing temperature, which would lead to the destruction of the heterojunction interface. The inert gas flow rate was 10 sccm to 1000 sccm. Meanwhile, during the annealing process, the first perovskite sublayer 21 deposited at the bottom induces the perovskite crystal orientation after the reaction of the cation solution 222 with the lead halide framework layer 221. Furthermore, the diffusion path of the cation solution 222 in the lead halide framework layer 221 becomes shorter, which is conducive to a more complete reaction of lead iodide at the bottom, thereby reducing the residual lead iodide reaction and improving the electron transport effect of the perovskite layer 200.
[0154] In some embodiments, the perovskite solar cell is a perovskite-silicon tandem solar cell, and the method for preparing the perovskite solar cell further includes the following steps:
[0155] Substrate 100: A texturized silicon bottom cell 11 is provided, a composite layer 12 is prepared on the texturized silicon bottom cell 11, and a first transport layer 13 is prepared on the composite layer 12;
[0156] Preparation of perovskite layer: A perovskite layer 200 is prepared on substrate 100, and the perovskite layer 200 is stacked on the surface of the first transport layer 13.
[0157] Fabrication of the second transport layer 300: The second transport layer 300 is fabricated on the perovskite layer 200, wherein one of the first transport layer 13 and the second transport layer 300 is an electron transport layer and the other is a hole transport layer.
[0158] Fabrication of transparent electrode layer 400: A transparent electrode layer 400 is fabricated on the second transport layer 300;
[0159] Positive electrode 600 and negative electrode 700 were prepared to obtain a perovskite solar cell.
[0160] It should be noted that one of the first transport layer 13 and the second transport layer 300 is an electron transport layer and the other is a hole transport layer. That is, when the first transport layer 13 is an electron transport layer, the second transport layer 300 is a hole transport layer, and when the first transport layer 13 is a hole transport layer, the second transport layer 300 is an electron transport layer.
[0161] In some embodiments, the composite layer 12 is fabricated by magnetron sputtering; and / or, the hole transport layer is fabricated by physical vapor deposition or evaporation; and / or, the electron transport layer is fabricated by evaporation; and / or, the transparent electrode layer 400 is fabricated by magnetron sputtering, and the positive electrode 600 is fabricated by evaporation; and / or, the negative electrode 700 is fabricated by evaporation.
[0162] In some embodiments, a passivation layer 14 is also prepared between the perovskite layer 200 and the electron transport layer, and the passivation layer 14 is prepared by vapor deposition; and / or, an antireflection layer 500 is prepared on the side of the transparent electrode layer 400 away from the textured silicon bottom cell 11, and the antireflection layer 500 is prepared by vapor deposition.
[0163] In some embodiments, the perovskite solar cell is a single-junction perovskite solar cell, and the fabrication method of the perovskite solar cell further includes the following steps:
[0164] Fabrication of substrate 100: A textured transparent electrode layer is provided, and a first transport layer is fabricated on the textured transparent electrode layer;
[0165] Preparation of perovskite layer: The perovskite layer 200 is prepared on the substrate 100, and the perovskite layer 200 is stacked on the surface of the first transport layer 13.
[0166] Fabrication of the second transport layer: A second transport layer 300 is fabricated on the perovskite layer 200, wherein one of the first transport layer 13 and the second transport layer 300 is an electron transport layer and the other is a hole transport layer.
[0167] Positive electrode 600 and negative electrode 700 were prepared to obtain a perovskite solar cell.
[0168] It should be noted that one of the first transport layer 13 and the second transport layer 300 is an electron transport layer and the other is a hole transport layer. That is, when the first transport layer 13 is an electron transport layer, the second transport layer 300 is a hole transport layer, and when the first transport layer 13 is a hole transport layer, the second transport layer 300 is an electron transport layer.
[0169] Thirdly, embodiments of the present invention provide a photovoltaic module, which includes the perovskite solar cell described in the first aspect or the perovskite solar cell prepared by the preparation method described in the second aspect.
[0170] The technical solution of the present invention will be further described below with reference to the embodiments and accompanying drawings.
[0171] Example 1
[0172] This embodiment provides a perovskite solar cell, comprising:
[0173] Substrate 100: Heterojunction base cell, the surface of which has a pyramidal textured structure with a height of 2-3 μm. A composite layer 12, made of indium tin oxide and 25 nm thick, is stacked on the front side of the heterojunction base cell. An electron transport layer, made of tin oxide and 25 nm thick, is stacked on the side of the composite layer 12 facing away from the textured silicon base cell 11. A passivation layer 14, made of C, is stacked on the side of the electron transport layer facing away from the textured silicon base cell 11. 60 The thickness is 3nm. The heterojunction base cell has a pyramid textured structure. The composite layer 12, electron transport layer and passivation layer 14 on the heterojunction base cell are all grown in a conformal manner along the pyramid shape of the heterojunction base cell, so that the substrate 100 has valley peaks and valley bottoms.
[0174] Perovskite layer 200: The perovskite layer is stacked on the surface of the passivation layer 14. The perovskite layer 200 includes a first perovskite sublayer 21 and a second perovskite sublayer 22. The first perovskite sublayer 21 is Cs 0.4 FA 0.4 MA 0.2 Pb(I 0.5 Br 0.5 3. The band gap is 2.0 eV. The first perovskite sublayer 21 fills the valley bottom and has an inverted pyramid shape matching the shape of the valley bottom. The thickness of the first perovskite sublayer 21 is 250 nm. The second perovskite sublayer 22 is formed by reacting a lead iodide framework layer and a cation solution 222. The second perovskite sublayer 22 covers the first perovskite sublayer 21 and the valley tip surface. The band gap is 1.68 eV. The second perovskite sublayer 22 includes alternating peaks 223 and flattened portions 224. The peaks 223 are located above the valley tips and their shapes match the valley tips. The flattened portions 224 are located above the first perovskite sublayer 21. The thickness of sublayer 22200 is 450 nm, so the obtained perovskite layer 200 is partially conformal. In the cation solution 222, the concentrations of formamidine iodoformin are 0.45 mol / L, methyl bromide is 0.15 mol / L, methyl chloroformide is 0.1 mol / L, formamidine iodoformin is 0.3 mol / L, methyl chloroformin is 0.1 mol / L, and methyl bromide is 0.1 mol / L. The solvent of cation solution 222 is anhydrous ethanol.
[0175] Hole transport layer: Stacked on the side of the perovskite layer 200 away from the textured silicon substrate 11, the hole transport layer is made of Sprio-OMeTAD and has a thickness of 22.5nm.
[0176] Transparent electrode layer 400: Stacked on the side of the hole transport layer away from the textured silicon bottom cell 11. The transparent electrode layer 400 is made of tungsten-doped indium oxide and has a thickness of 100 nm.
[0177] Antireflection layer 500: An antireflection layer 500 is stacked on the side of the transparent electrode layer 400 away from the textured silicon bottom cell 11. The antireflection layer 500 is made of magnesium fluoride and has a thickness of 110 nm.
[0178] Positive electrode 600 and negative electrode 700: It also includes positive electrode 600 and negative electrode 700. Both positive electrode 600 and negative electrode 700 are silver electrodes. The thickness of positive electrode 600 and negative electrode 700 is 275nm. Positive electrode 600 forms an ohmic contact with transparent electrode layer 400, and negative electrode 700 forms an ohmic contact with heterojunction bottom cell.
[0179] The hole transport layer, transparent electrode layer 400 and antireflection layer 500, which are prepared after the perovskite layer 200, are grown in a conformal manner along the structure of the perovskite layer 200.
[0180] This embodiment also provides a method for preparing the above-mentioned perovskite solar cell, including the following steps:
[0181] Preparation of substrate 100: A heterojunction bottom cell with a pyramidal textured surface is provided. A patterned composite layer 12 is prepared on the front side of the heterojunction bottom cell by magnetron sputtering. An electron transport layer is prepared on the composite layer 12 by vapor deposition. A passivation layer 14 is prepared on the electron transport layer by vapor deposition to obtain substrate 100. Substrate 100 has valley peaks and valley bottoms.
[0182] Preparation of perovskite layer 200: The perovskite layer includes a first perovskite sublayer and a second perovskite sublayer. The above-mentioned substrate is used as the growth substrate of the perovskite layer. The preparation method of the first perovskite sublayer 21 is as follows: Take the perovskite precursor solution 211 and use the slit coating method to coat the perovskite precursor solution 211 on the side of the passivation layer 14 away from the heterojunction bottom cell. Utilizing the fluidity of the perovskite precursor solution 211, the perovskite precursor solution 211 flows autonomously and accumulates at the bottom of the valley. Then, it is annealed at 115°C for 22 min to obtain the first perovskite sublayer 21. The first perovskite sublayer 21 has an inverted pyramid shape that matches the shape of the valley.
[0183] The preparation method of the second perovskite sublayer 22 is as follows: Lead iodide and cesium bromide are deposited by a dual-source co-evaporation process, and the evaporation rate ratio is controlled at 7.5:1 to obtain a lead iodide framework layer. The lead iodide framework layer includes alternating sharp framework portions 2211 and flat framework portions 2212. The sharp framework portions 2211 are located above the valley tips, and the shapes of the sharp framework portions 2211 and the valley tips are matched. The flat framework portions 2212 are located above the first perovskite sublayer 21. The thickness of the lead iodide framework layer is 350 nm. Under the controlled ambient humidity of 10% and temperature of 25°C, a cationic solution is spin-coated onto the lead iodide framework layer. 222, continue to control the ambient humidity at 10%, and purge the surface of the lead iodide framework layer coated with the cationic solution 222 by introducing 200 sccm of Ar at room temperature. Control the heating temperature at 150°C and anneal for 22 min to obtain the second perovskite sublayer 22. The second perovskite sublayer 22 has alternating peaks 223 and flattened parts 224. The peaks 223 are located above the valleys, and the shapes of the peaks 223 and valleys match. The flattened parts 224 are located above the first perovskite sublayer 21, and the first perovskite sublayer 21 and the second perovskite sublayer 22 form a heterojunction.
[0184] Preparation of hole transport layer: A hole transport layer was prepared on the perovskite layer 200 by vapor deposition.
[0185] Preparation of transparent electrode layer 400: Transparent electrode layer 400 is prepared on hole transport layer by magnetron sputtering;
[0186] Preparation of positive electrode 600 and negative electrode 700: Positive electrode 600 is deposited on transparent electrode layer 400 by evaporation at a certain rate. The positive electrode 600 forms an ohmic contact with the transparent electrode layer 400, and the negative electrode 700 is deposited on the back of the heterojunction bottom cell by evaporation at a certain rate. This allows the negative electrode 700 to form an ohmic contact with the heterojunction bottom cell.
[0187] Preparation of antireflection layer 500: The antireflection layer 500 is prepared on the transparent electrode layer 400 by vapor deposition, with an evaporation rate of... The refractive index n is 1.4.
[0188] Example 2
[0189] This embodiment provides a perovskite solar cell, which differs from Embodiment 1 in that: the band gap of the first perovskite sublayer 21 is 2.3 eV, and the band gap of the second perovskite sublayer 22 is 1.72 eV, while the rest remains the same as Embodiment 1.
[0190] Example 3
[0191] This embodiment provides a perovskite solar cell, which differs from Embodiment 1 in that the band gap of the first perovskite sublayer 21 is 1.73 eV and the band gap of the second perovskite sublayer 22 is 1.68 eV, while the rest remains the same as in Embodiment 1.
[0192] Example 4
[0193] This embodiment provides a perovskite solar cell, which differs from Embodiment 1 in that the thickness of the first perovskite sublayer 21 is 100 nm, while the rest remains the same as in Embodiment 1.
[0194] Example 5
[0195] This embodiment provides a perovskite solar cell, which differs from Embodiment 1 in that the thickness of the first perovskite sublayer 21 is 500 nm, while the rest remains the same as in Embodiment 1.
[0196] Comparative Example 1
[0197] This comparative example provides a perovskite solar cell, which differs from Example 1 in that: a first perovskite sublayer 21 is not prepared, such as... Figure 1 As shown, the preparation method of the perovskite layer 200 includes the following steps:
[0198] Preparation of perovskite layer 200: Using the composite layer 12, electron transport layer and passivation layer 14 stacked on the heterojunction bottom cell as the substrate 100 for preparing perovskite layer 200, lead iodide and cesium bromide are deposited on the passivation layer 14 using a dual-source co-evaporation process, and the evaporation rate ratio is controlled at 7.5:1, so that lead iodide and cesium bromide with a specific evaporation rate ratio grow conformally along the surface of substrate 100 to obtain a conformally oriented lead iodide framework layer with a thickness of 350 nm. Under the control of ambient humidity of 10% and temperature of 25°C, cationic solution 222 is spin-coated on the lead iodide framework layer. The ambient humidity is then controlled at 10%, and the layer is annealed at 150°C for 22 min to obtain a perovskite layer 200 with a thickness of 450 nm that has excellent conformal effect. The rest is consistent with Example 1.
[0199] Comparative Example 2
[0200] This comparative example provides a perovskite solar cell, which differs from Example 1 in that the perovskite material of the first perovskite sublayer 21 is Cs. 0.2 FA 0.7 MA 0.1 Pb(I 0.4 Br 0.6 )3, the band gap is 1.68eV, the band gap of the second perovskite sublayer is 1.68eV, and the rest is consistent with Example 1.
[0201] Experiment 1
[0202] A top-view SEM scan of the first perovskite sublayer of Example 1 was performed to obtain a top view of the first perovskite sublayer. Figure 6 .
[0203] In Example 1, in conjunction with the above Figure 6 It can be seen that during the preparation of the perovskite layer, the first perovskite sublayer does not completely cover the pyramid surface of the substrate, but fills the valley bottom of the substrate, while the valley apex of the substrate is the part not covered by the first perovskite sublayer.
[0204] Experiment 2
[0205] The performance of perovskite solar cells was tested using the Wavelabs solar simulator under the following conditions: AM1.5, 1000 W / m. 2 The test environment temperature was 25℃. Before testing, the light source was calibrated to simulate sunlight intensity using a standard silicon cell. Performance tests included energy conversion efficiency, open-circuit voltage, short-circuit current, and fill factor.
[0206] The test results of the above embodiments and comparative perovskite solar cells are shown in Table 1.
[0207] Table 1
[0208]
[0209] As can be seen from the data in Table 1, the short-circuit current of Example 1 is 0.44 mA / cm higher than that of Comparative Example 1. 2 The open-circuit voltage was 0.065V higher than that of the first control, the fill factor was 0.09% lower, and the overall power conversion efficiency was 1.62% higher. This indicates that although the perovskite layer was not completely conformed and the light trapping effect was reduced when the first perovskite sublayer was pre-deposited to the bottom of the valley before the second perovskite sublayer was prepared, the residual lead iodide in this not completely conformed perovskite layer was low, the interface stability was high, and the interaction with the subsequent film layers was better. Therefore, the perovskite tandem solar cell prepared from this perovskite layer has a better power conversion efficiency.
[0210] A comparison of the data from Example 1 and Comparative Example 2 shows that the short-circuit current in Example 1 is 0.53 mA / cm higher than that in Comparative Example 2. 2 The open-circuit voltage is 0.117V higher than that of Comparative Example 1, the fill factor is 9.55% higher than that of Comparative Example 1, and the overall power conversion efficiency is 5.92% higher than that of Comparative Example 2. This proves that when there is no band difference between the first perovskite sublayer and the second perovskite sublayer, the charge at the interface cannot be separated. At the same time, an unnecessary interface is added, which leads to severe recombination between the first and second perovskite layers, affecting the current, open-circuit voltage, and fill factor, resulting in low device efficiency.
[0211] A comparison of the data from Examples 1, 2, and 3 shows that Example 1 has the highest energy conversion efficiency, followed by Example 2, and Example 3 has the lowest. This indicates that the perovskite layer formed by the combination of the first and second perovskite sublayers with different band gaps has a significant impact on the energy conversion efficiency of the perovskite tandem solar cell. In Examples 1 to 3, the local heterojunctions formed between the first and second perovskite sublayers with different band gaps have different abilities to promote charge and hole separation. When the band gap difference between the first and second perovskite sublayers is limited to a specific range, the open-circuit voltage of the perovskite tandem solar cell is significantly improved, and the energy conversion efficiency is further improved. When the band gap difference increases, it is easier to cause damage to the perovskite structure, and the stability of the perovskite layer also decreases. Therefore, the energy conversion efficiency of Example 3 is reduced. When the band gap difference is too small, the potential energy of the built-in electric field is too low, the carrier migration ability is insufficient, the electron migration efficiency decreases, and the energy conversion efficiency is reduced.
[0212] A comparison of the experimental results from Examples 1, 4, and 5 shows that Example 1 has the highest energy conversion efficiency, followed by Example 4, and Example 5 has the lowest. This demonstrates that the thickness of the first perovskite sublayer has a significant impact on the overall performance of the perovskite layer. On the one hand, a lower thickness of the first perovskite sublayer results in a heterojunction formed between the first and second perovskite sublayers closer to the interface, which is more effective in improving charge separation at the interface. On the other hand, an increase in the thickness of the first perovskite sublayer leads to a more significant reduction in the diffusion distance of the cation solution in the lead iodide framework layer during the preparation of the second perovskite sublayer, which is more conducive to reducing the excess lead iodide in the second perovskite sublayer and improving the crystallinity of the perovskite layer. When the thickness of the first perovskite sublayer is limited to a specific range, the short-circuit current and fill factor of the perovskite tandem solar cell are further improved, resulting in higher energy conversion efficiency.
[0213] The perovskite solar cells, their preparation methods, and photovoltaic modules disclosed in the embodiments of the present invention have been described in detail above. Specific examples have been used to illustrate the principles and implementation methods of the present invention. The descriptions of the above embodiments are only for the purpose of helping to understand the perovskite solar cells, their preparation methods, photovoltaic modules, and their core ideas of the present invention. At the same time, for those skilled in the art, there will be changes in the specific implementation methods and application scope based on the ideas of the present invention. Therefore, the content of this specification should not be construed as a limitation of the present invention.
Claims
1. A perovskite solar cell, characterized in that: The perovskite solar cell includes: The base has a velvety surface structure, which has valley peaks and valley bottoms; The perovskite layer includes a first perovskite sublayer and a second perovskite sublayer disposed above a substrate. The first perovskite sublayer fills the valley bottom of the substrate, and the second perovskite sublayer covers the first perovskite sublayer and the valley tip. A heterojunction is formed between the first perovskite sublayer and the second perovskite sublayer. The second perovskite sublayer is obtained by reacting a lead halide framework layer with a cation solution. The thickness of the first perovskite sublayer is 100 nm to 500 nm, and the thickness of the second perovskite sublayer is 500 nm to 1 μm.
2. The perovskite solar cell according to claim 1, characterized in that: The perovskite solar cell has a nip structure or a pin structure. When the perovskite solar cell has a nip structure, the band gap of the first perovskite sublayer is 1.72 eV to 2.3 eV, and the band gap of the second perovskite sublayer is 1.63 eV to 1.72 eV, with the band gap of the first perovskite sublayer being larger than that of the second perovskite sublayer. When the perovskite solar cell has a pin structure, the band gap of the first perovskite sublayer is 1.2 eV to 1.63 eV, and the band gap of the second perovskite sublayer is 1.63 eV to 1.72 eV, with the band gap of the first perovskite sublayer being smaller than that of the second perovskite sublayer.
3. The perovskite solar cell according to claim 2, characterized in that: The band gap difference between the first perovskite sublayer and the second perovskite sublayer is 0.05 eV to 0.58 eV.
4. The perovskite solar cell according to claim 2, characterized in that: When the band gap of the first perovskite sublayer is 1.72 eV to 2.3 eV, the first perovskite sublayer is Cs. x1 FA y1 MA 1-x1-y1 Pb(I z Br 1-z1 )3, wherein x1 = 0~1, y1 = 0~1, and z1 = 0~1; when the band gap of the first perovskite sublayer is 1.2 eV~1.63 eV, the first perovskite sublayer is FA. x2 MA 1-x2 Pb y2 Sn 1-y2 (I z2 B r1-z2 )3, wherein x2=0~1, y2=0~1, and z2=0~1.
5. The perovskite solar cell according to claim 1, characterized in that: The velvet structure is a pyramid structure. The first perovskite sublayer filling the valley has an inverted pyramid shape. The second perovskite sublayer includes alternating peaks and flat sections. The peaks are located above the valley tips and their shapes match the valley tips. The flat sections are located above the first perovskite sublayer.
6. The perovskite solar cell according to claim 1, characterized in that: The lead halide framework layer has alternating sharp and flat framework portions, with the sharp framework portions corresponding to the valley tips and matching the shape of the valley tips, and the flat framework portions corresponding to the first perovskite sublayer; and / or, the thickness of the lead halide framework layer is 350 nm to 800 nm.
7. The perovskite solar cell according to claim 1, characterized in that: The solute in the cation solution includes one or more of iodoformamidine, bromoformamidine, chloroformamidine, iodoformamine, bromoformamine, and chloroformamine, and the solvent in the cation solution includes one or two of anhydrous ethanol and isopropanol.
8. The perovskite solar cell according to claim 7, characterized in that: In the cationic solution, the concentration of formamidinium iodoformide is 0.3 mol / L to 0.6 mol / L, the concentration of methyl bromide is 0 mol / L to 0.2 mol / L, the concentration of methyl chloroformide is 0 mol / L to 0.15 mol / L, the concentration of formamidinium iodoformide is 0 mol / L to 0.6 mol / L, the concentration of methyl bromide is 0 mol / L to 0.2 mol / L, and the concentration of methyl bromide is 0 mol / L to 0.2 mol / L.
9. The perovskite solar cell according to claim 1, characterized in that: The perovskite solar cell is a perovskite-silicon tandem solar cell. The substrate includes a texturized silicon substrate cell and a composite layer and a first transport layer sequentially stacked on the texturized silicon substrate cell. The perovskite layer is stacked on the surface of the first transport layer. The perovskite solar cell further includes: A second transport layer stacked on the perovskite layer on the side of the texturized silicon substrate cell away from the cell. A transparent electrode layer stacked on the side of the second transport layer facing away from the textured silicon substrate cell; One of the first transport layer and the second transport layer is an electron transport layer, and the other is a hole transport layer; It also includes a positive electrode and a negative electrode, wherein the positive electrode forms an ohmic contact with the transparent electrode layer and the negative electrode forms an ohmic contact with the texturized silicon bottom cell.
10. The perovskite solar cell according to claim 9, characterized in that: The texturized silicon bottom cell includes one or more of the following: emitter passivation and back contact cell, tunnel oxide passivation contact cell, heterojunction cell, heterojunction back contact crystalline silicon cell, and tunnel oxide passivation back contact cell; and / or, The composite layer is made of one or both of indium tin oxide and indium zinc oxide; the hole transport layer is made of one or more of nickel oxide, cuprous oxide, Spiro-TTB, and cuprous thiocyanate; and / or, The material of the electron transport layer includes C. 60 ; and / or, The material of the transparent electrode layer includes one or both of indium tin oxide and indium zinc oxide.
11. The perovskite solar cell according to claim 9, characterized in that: The thickness of the composite layer is 20 nm to 30 nm; and / or, The thickness of the hole transport layer is 20 nm to 30 nm; and / or, The thickness of the electron transport layer is 10 nm to 30 nm; and / or, The thickness of the transparent electrode layer is 80 nm to 120 nm.
12. The perovskite solar cell according to claim 9, characterized in that: The perovskite solar cell also includes: A passivation layer, wherein the passivation layer is located between the perovskite layer and the electron transport layer; and / or, An antireflection layer is located on the side of the transparent electrode layer opposite to the fabrication of the texturized silicon substrate cell.
13. The perovskite solar cell according to claim 12, characterized in that: The material of the passivation layer includes C. 60 and one or two of the fullerene derivatives PCBM; and / or, The antireflective layer is made of one or both of magnesium fluoride and lithium fluoride.
14. The perovskite solar cell according to claim 12, characterized in that: The thickness of the passivation layer is 1 nm to 10 nm; and / or, The thickness of the antireflection layer is 100 nm to 120 nm.
15. The perovskite solar cell according to claim 1, characterized in that: The perovskite solar cell is a single-junction perovskite solar cell. The substrate includes a textured transparent electrode layer and a first transport layer stacked on the textured transparent electrode layer. The perovskite layer is stacked on the surface of the first transport layer. The perovskite solar cell further includes: A second transport layer is stacked on the side of the perovskite layer away from the textured transparent electrode layer, wherein one of the first transport layer and the second transport layer is an electron transport layer and the other is a hole transport layer; It also includes a positive electrode and a negative electrode, wherein the positive electrode forms an ohmic contact with the second transport layer and the negative electrode forms an ohmic contact with the textured transparent electrode layer.
16. A method for preparing a perovskite solar cell, characterized in that: The method for preparing the perovskite solar cell according to any one of claims 1-15 includes the following steps: Provide a substrate: the surface of the substrate has a velvety structure, the velvety structure having valley peaks and valley bottoms; Preparation of the first perovskite sublayer: The first perovskite sublayer is deposited on the substrate by solution deposition, followed by annealing to obtain the first perovskite sublayer filling the valley bottom; Preparation of the second perovskite sublayer: A lead halide framework layer is prepared on the first perovskite sublayer, so that the lead halide framework layer covers the first perovskite sublayer and the valley tip. A cationic solution is coated on the lead halide framework layer, and annealing is performed to form a perovskite heterojunction between the first perovskite sublayer and the second perovskite sublayer, thus obtaining the perovskite layer.
17. The method for preparing a perovskite solar cell according to claim 16, characterized in that: The solution method includes any one of spin coating, blade coating, spray coating, or slot coating; and / or, The lead halide framework layer is prepared by a dual-source co-evaporation process using lead iodide and cesium bromide, wherein the evaporation rate ratio of lead iodide to cesium bromide is 5:1 to 10:1; and / or, Methods for applying the cationic solution include spin coating and slot coating; and / or, In the step of preparing the first perovskite sublayer, the annealing treatment is either direct annealing or antisolvent engineering combined with thermal annealing. In the direct annealing, the annealing temperature is 80℃~150℃ and the annealing time is 10 min~30 min. In the antisolvent engineering combined with thermal annealing, the antisolvent includes one or more of diethyl ether, toluene, ethyl acetate, chlorobenzene and chloroform, and the thermal annealing temperature is 100℃~150℃ and the thermal annealing time is 10 min~30 min. In the step of preparing the second perovskite sublayer, the annealing treatment is carried out at a humidity of 5%RH~60%RH, with an inert gas stream blowing through the surface of the lead halide framework layer after coating with the cationic solution, and annealing at 80℃~100℃ for 15 min~30 min.
18. The method for preparing a perovskite solar cell according to claim 16, characterized in that: The perovskite solar cell is a perovskite-silicon tandem solar cell, and the preparation method of the perovskite solar cell further includes the following steps: Preparation of the substrate: A texturized silicon substrate cell is provided, a composite layer is prepared on the texturized silicon substrate cell, and a first transport layer is prepared on the composite layer; Preparation of the perovskite layer: The perovskite layer is prepared on the substrate, and the perovskite layer is stacked on the surface of the first transport layer; Fabrication of a second transport layer: A second transport layer is fabricated on the perovskite layer, wherein one of the first transport layer and the second transport layer is an electron transport layer and the other is a hole transport layer; Fabrication of a transparent electrode layer: The transparent electrode layer is fabricated on the second transport layer; A positive electrode and a negative electrode are prepared to obtain the perovskite solar cell.
19. The method for preparing a perovskite solar cell according to claim 18, characterized in that: The composite layer is prepared by magnetron sputtering; and / or, the hole transport layer is prepared by physical vapor deposition or evaporation; and / or, the electron transport layer is prepared by evaporation; and / or, the transparent electrode layer is prepared by magnetron sputtering and the positive electrode is prepared by evaporation; and / or, the negative electrode is prepared by evaporation.
20. The method for preparing a perovskite solar cell according to claim 18, characterized in that: A passivation layer is further prepared between the perovskite layer and the electron transport layer, the passivation layer being prepared by vapor deposition; and / or, an antireflection layer is prepared on the side of the transparent electrode layer away from the texturized silicon substrate, the antireflection layer being prepared by vapor deposition.
21. The method for preparing a perovskite solar cell according to claim 16, characterized in that: The perovskite solar cell is a single-junction perovskite solar cell, and the preparation method of the perovskite solar cell further includes the following steps: Preparation of the substrate: A textured transparent electrode layer is provided, and a first transport layer is prepared on the textured transparent electrode layer; Preparation of the perovskite layer: The perovskite layer is prepared on the substrate, and the perovskite layer is stacked on the surface of the first transport layer; Fabrication of a second transport layer: A second transport layer is fabricated on the perovskite layer, wherein one of the first transport layer and the second transport layer is an electron transport layer and the other is a hole transport layer; A positive electrode and a negative electrode are prepared to obtain the perovskite solar cell.
22. A photovoltaic module, characterized in that, This includes the perovskite solar cell according to any one of claims 1-15 or the perovskite solar cell prepared by any one of claims 16-21.
Citation Information
Patent Citations
Perovskite-silicon-based laminated solar cell and manufacturing method thereof
CN116133448A
Perovskite thin film layer and preparation method thereof, perovskite crystalline silicon laminated cell and preparation method thereof
CN116709886A