A polylactic acid film with high puncture resistance and preparation method thereof
By adding raw materials such as polypropylene carbonate, bacterial cellulose and hydrophobic modified graphene oxide to the polylactic acid film, the problem of insufficient toughness of the polylactic acid film is solved, its puncture resistance and barrier properties are improved, and better Packaging performance and industrial productivity.
Patent Information
- Application Number
- CN202311656103.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-05
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-12-05
AI Technical Summary
Polylactic acid film has poor toughness, lacks elasticity and flexibility, making it easy to puncture when packaging items with spikes, and its puncture resistance is insufficient.
By adding raw materials such as polypropylene carbonate, bacterial cellulose and hydrophobic modified graphene oxide, the toughness and barrier properties of the polylactic acid film are improved, its tensile strength and elastic modulus are increased, and the brittleness is reduced, and through specific preparation methods Such as spray drying and melt extrusion technology to improve the dispersion and interface compatibility of materials.
It significantly improves the puncture resistance and barrier properties of the polylactic acid film, enhances its oxygen and water vapor barrier capabilities, and at the same time improves the antibacterial performance and the feasibility of industrial production.
Smart Images

Figure BDA0004588963780000081 
Figure BDA0004588963780000121
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of polymer materials, and more specifically, to a polylactic acid film with high puncture resistance and a preparation method thereof. Background Art
[0002] Biodegradable plastics can be decomposed under natural conditions, thereby reducing pollution to the environment and reducing the impact of plastic waste on the ecosystem. Biodegradable plastics can be produced from natural resources such as biomass and plant starch. Starch has been studied in depth due to its cheap price and wide sources, and a variety of daily necessities and industrial products such as starch-based films and starch tableware have been prepared through modification and compounding. However, starch has its natural defects. Its mechanical properties are poor and its performance is unstable. It can only be used in fields with low requirements for mechanical properties. The emergence of polylactic acid has changed this situation. Polylactic acid (PLA) is an aliphatic polyester with lactic acid (2-hydroxypropionic acid) as the basic structural unit. PLA can be made by fermenting natural raw materials such as corn, or by polycondensation of lactic acid.
[0003] Polylactic acid has good biocompatibility, environmental safety, no toxicity, good mechanical properties and light transparency, and good processing performance. It can be used for a variety of packaging materials such as ground film, food packaging bags, and medicines. However, polylactic acid has poor toughness, lacks elasticity and flexibility, and has a hard and brittle texture. When used as a food packaging bag for contents with sharp thorns (such as lobsters, shellfish, bones, and skewers with bamboo sticks), it will be pierced or punctured due to the lack of toughness of the material. Summary of the invention
[0004] In order to improve the toughness and flexibility of a polylactic acid film, reduce its brittleness, and improve its puncture resistance, the present application provides a polylactic acid film with high puncture resistance and a preparation method thereof.
[0005] In the first aspect, the present application provides a polylactic acid film with high puncture resistance, which adopts the following technical solution:
[0006] A high puncture resistance polylactic acid film comprises the following raw materials in parts by weight: 60-70 parts of a polylactic acid base material, 30-40 parts of polypropylene carbonate, 1.5-2.5 parts of hydrophobically modified graphene oxide, 1-2 parts of bacterial cellulose, 0.1-0.5 parts of a toughening agent, 0.02-0.1 parts of a compatibilizer, 0.25-2.5 parts of a lubricant, and 0.25-1.5 parts of an antioxidant.
[0007] By adopting the above technical scheme, in order to improve the toughness of polylactic acid, a certain amount of polycarbonate propylene is added. Polycarbonate propylene is an aliphatic polycarbonate polymerized by carbon dioxide and propylene oxide under the action of a catalyst. It has excellent oxygen barrier properties, biodegradability and good flexibility. In addition, polycarbonate propylene has good compatibility with polylactic acid, so it can effectively improve the tensile strength and elastic modulus of the polylactic acid film, enhance toughness and reduce brittleness. In addition, a certain amount of bacterial cellulose is added. Bacterial cellulose is a three-dimensional network structure with a high degree of polymerization and significant tensile properties formed by a large number of D-glucose monomers connected by β-1,40 glycosidic bonds. It has high safety, low cost, high flexibility, transparency and biodegradability. Excellent physical and chemical properties, such as high safety, low cost, high flexibility, transparency and biodegradability, the hydroxyl group on the bacterial cellulose can hydrogen bond with the carbonyl group on the polylactic acid base material, thereby enhancing the interaction between the bacterial fiber and the polylactic acid base material, improving the tensile strength of the polylactic acid film, and the bacterial cellulose It has high porosity, high crystallinity and high specific surface area. In the polylactic acid film, when oxygen passes through, the porous structure prolongs the oxygen permeation path, thereby improving the oxygen barrier of the polylactic acid film. The hydrophobically modified graphene oxide is prepared by hydrophobically modifying graphene oxide, which weakens its surface polarity and enhances its non-polarity, and improves its interfacial compatibility with the polylactic acid base material and polypropylene carbonate, thereby increasing the elastic modulus of the polylactic acid film, enhancing its toughness, maintaining high tensile strength, elastic modulus and elongation at break. Moreover, graphene oxide with reduced surface polar groups can also increase the crystallization of polylactic acid, reduce the crystal size of polylactic acid, significantly improve the crystallinity of polylactic acid, and increase the compactness of the molecular chain arrangement inside the film, making it difficult for small molecules to pass through. In addition, graphene oxide has a layered structure. Graphene oxide evenly dispersed in the mixture of polylactic acid base material and polypropylene carbonate allows water vapor and oxygen to pass through a more tortuous path, thereby blocking water molecules and oxygen, further enhancing the barrier effect of the polylactic acid film.
[0008] Preferably, the hydrophobically modified graphene oxide comprises graphene oxide and tert-butyldimethylchlorosilane in a mass ratio of 1:0.3-0.5.
[0009] By adopting the above technical scheme, tert-butyldimethylchlorosilane is used to hydrophobically modify graphene oxide, and the methylsilane in the tert-butyldimethylchlorosilane can be grafted with the hydroxyl groups contained in the graphene oxide, thereby reducing the content of polar groups on the surface of the graphene oxide, and improving the compatibility of the graphene oxide with the polylactic acid base material and polypropylene carbonate. In addition, the hydrophobically modified graphene oxide acts as a crystal nucleus in the blend, and plays a heterogeneous nucleation role in the crystallization of the polylactic acid base material, so that the crystallinity is improved, the mobility between the molecular chains is enhanced, the molecular chains are arranged in order, the crystallization ability is enhanced, the crystal size is reduced, the tensile strength and elastic modulus of the polylactic acid film are improved, and the compactness of the polylactic acid molecular chain is improved, thereby improving the barrier property of the polylactic acid film to water vapor and oxygen.
[0010] Preferably, the preparation method of the hydrophobically modified graphene oxide is as follows:
[0011] Disperse graphene oxide in deionized water, add imidazole catalyst and tert-butyldimethylsilyl chloride, stir at room temperature for 10-12 hours, vacuum dry, disperse in dichloromethane, and ultrasonicate for 20-30 minutes to prepare a dispersion;
[0012] Adding polylactic acid resin into dichloromethane, stirring and dissolving, to obtain polylactic acid emulsion, wherein the mass ratio of polylactic acid to graphene oxide is 1:0.05-0.1;
[0013] The dispersion and the polylactic acid emulsion are mixed and spray-dried to prepare hybrid nanoparticles;
[0014] The mixed nanoparticles and polylactic acid resin are mixed, melted and extruded at a mass ratio of 0.1-0.2:1 to obtain hydrophobically modified graphene oxide.
[0015] By adopting the above technical scheme, the surface polar groups of graphene oxide grafted with methylsilane are reduced, and it is insoluble in dichloromethane and exists in the form of a suspension. After mixing it with a polylactic acid emulsion, the graphene oxide grafted with methylsilane can achieve good dispersion in the polylactic acid resin through a spray drying method. The graphene oxide grafted with methylsilane is frozen in the dispersion and the polylactic acid emulsion, thereby maintaining the same dispersion as the original mixed solution. In addition, spray drying can obtain smaller and finer solid mixed nanoparticles, which can be melt-coated with the polylactic acid resin. During mixing, the methylsilane-grafted graphene oxide is easier to be evenly dispersed in the polylactic acid resin, so that there is more interface area between the polylactic acid resin and the polylactic acid resin, which can improve the load transfer efficiency. The mixed nanoparticles can be completely dispersed with the polylactic acid resin through melt blending and extrusion to prevent the mixed nanoparticles from agglomerating and affecting the transparency and flexibility of the polylactic acid film. The mixed nanoparticles are separated from the interface of the polylactic acid resin matrix to form a large number of micro-voids, which are helpful for stress absorption, thereby making the tensile fracture surface of the material rough, and significantly improving the tensile properties of the material.
[0016] Preferably, the melt index of the polylactic acid base material and the polylactic acid resin is 5-8 g / 10 min, and the density is 1.4-2 g / cm 3 .
[0017] By adopting the above technical scheme, when preparing hydrophobically modified graphene oxide, using a polylactic acid resin with a melt index and density similar to those of the polylactic acid base material, the dispersion uniformity of the hydrophobically modified graphene oxide and the polylactic acid base material can be further improved, and the tensile strength, elastic modulus and other mechanical properties of the polylactic acid film can be improved.
[0018] Preferably, the bacterial cellulose is pretreated as follows:
[0019] Add polyvinyl alcohol to N,N-dimethylformamide, stir and dissolve to obtain a PVA solution with a concentration of 3-5wt%, add lactic acid-citric acid copolymer, stir and dissolve to obtain an impregnation solution, and the mass ratio of polyvinyl alcohol to lactic acid-citric acid copolymer is 1:0.1-0.3;
[0020] The bacterial cellulose is added to the impregnation solution, impregnated at -(0.01-0.03) MPa for 48-50 hours, and allowed to stand and dry. The mass ratio of the bacterial cellulose to the polyvinyl alcohol is 0.2-0.7:1.
[0021] By adopting the above technical scheme, bacterial cellulose contains a large number of hydrophilic hydroxyl groups, and has a large moisture permeability in a humid environment. Its barrier capacity for water vapor needs to be improved. Therefore, polyvinyl alcohol is impregnated with an impregnation solution containing polyvinyl alcohol and lactic acid-citric acid copolymer under negative pressure. The bacterial cellulose has a large porosity. Polyvinyl alcohol is impregnated under negative pressure and can fill the pores of the bacterial cellulose. The hydroxyl groups on the bacterial cellulose form a large number of hydrogen bonds with the hydroxyl groups on the polyvinyl alcohol, which enhances the interaction between the bacterial cellulose and the polyvinyl alcohol and reduces the content of hydrophilic hydroxyl groups on the bacterial cellulose. In addition, polyvinyl alcohol has excellent gas barrier properties, so it can enhance the water vapor barrier capacity of bacterial cellulose. The lactic acid-citric acid copolymer is made by copolymerization of lactic acid and citric acid. Due to the introduction of carboxyl groups on the molecular chain, reactive sites are introduced on the polylactic acid molecular chain. When subjected to When the pretreated bacterial cellulose is mixed with a polylactic acid base material, on the one hand, due to the presence of carboxyl groups on the lactic acid-citric acid copolymer, hydrogen bonds can be formed with hydroxyl groups on polyvinyl alcohol and carbonyl groups on the polylactic acid base material. On the other hand, due to the presence of polylactic acid segments in the lactic acid-citric acid copolymer, the bacterial cellulose has good compatibility with the polylactic acid base material. Therefore, it can be used as a compatibilizer between the polylactic acid base material and the polyvinyl alcohol on the surface of the bacterial cellulose, thereby improving the compatibility between the polylactic acid base material and the bacterial cellulose, thereby further improving the mechanical properties of the polylactic acid film, such as puncture resistance and tensile strength. In addition, the hydroxyl groups on the polyvinyl alcohol can also form hydrogen bonds with the carbonyl groups on the polylactic acid base material, and can also form hydrogen bonds with the carboxyl groups on the lactic acid-citric acid copolymer. Therefore, the hydroxyl content on the polyvinyl alcohol can be reduced, thereby reducing the hydrophilicity of the polyvinyl alcohol, thereby further improving the barrier ability of the bacterial cellulose to water vapor.
[0022] Preferably, the bacterial cellulose is subjected to the following treatment before being added to the impregnation solution:
[0023] The bacterial cellulose is placed in a sodium hydroxide solution with a concentration of 4-5wt%, boiled for 1-1.5h, cooled and dried, and then placed in a nano zinc oxide dispersion with a concentration of 4-8wt%, immersed for 2-3h at -(0.05-0.08)MPa, filtered, washed with deionized water, and vacuum dried.
[0024] By adopting the above technical scheme, the bacterial cellulose is first subjected to negative pressure impregnation treatment with a dispersion containing nano zinc oxide before being treated with an impregnation solution, and nano zinc oxide is loaded on the porous bacterial cellulose, so that the bacterial cellulose has an antibacterial effect. Moreover, nano zinc oxide, as an inorganic antibacterial agent, not only has excellent antibacterial properties, but can also effectively eliminate Gram-positive bacteria and Gram-negative bacteria, inhibit fungal growth, and impart antibacterial properties to bacterial cellulose, thereby improving the antibacterial ability of polylactic acid film. Moreover, it has good heat resistance, and when bacterial cellulose is hot-melted with polylactic acid base material, thermal decomposition is not easy to occur, and the antibacterial ability of the polylactic acid film will not be reduced. In addition, the addition of nano zinc oxide can further improve the tensile strength of bacterial cellulose and enhance its mechanical strength.
[0025] Preferably, the nano zinc oxide dispersion is prepared by mixing nano zinc oxide, gelatin, distilled water and sodium dodecylbenzene sulfonate and grinding for 20-30 minutes, the amount of sodium dodecylbenzene sulfonate added is 0.01-0.1 of the mass of nano zinc oxide, and the amount of gelatin added is 0.1-0.2 of the mass of nano zinc oxide.
[0026] By adopting the above technical scheme, sodium dodecyl sulfate, as an anionic surfactant, can ionize dodecylbenzenesulfonate ions and sodium ions. The dodecylsulfonate ions are adsorbed on the positively charged positions on the surface of the chemical particles you apply through electrostatic attraction and diffusion. Due to the hydrophobic effect between the hydrocarbon chains of the adsorbed dodecylbenzenesulfonate ions and the hydrocarbon chains of sodium dodecylbenzenesulfonate or dodecylbenzenesulfonate ions in the solution, the nano zinc oxide is evenly dispersed in the distilled water with good stability. The nano zinc oxide can be firmly bonded to the surface of bacterial cellulose through the greater adhesion of gelatin and will not fall off due to mechanical shearing, thereby extending the antibacterial durability.
[0027] Preferably, the toughening agent comprises phenyl silicone resin, PBS and hydroxylated PCL in a mass ratio of 0.3-0.5:0.1-0.3:1.
[0028] By adopting the above technical scheme, polybutylene succinate is a biodegradable material with high tension, strong toughness and excellent biocompatibility. As a toughening agent, it can effectively improve the brittleness of polylactic acid. PCL is poly-ε-caprolactone, which is a semi-crystalline polyester with good toughness and high elongation at break. It can effectively improve the mechanical properties of polylactic acid. Moreover, after hydroxylation, it can easily hydrogen bond with the carbonyl group on the polylactic acid base material to improve the mechanical strength. The phenyl group in the phenyl silicone resin can be grafted with the polylactic acid base material through a compatibilizer, thereby improving the interfacial adhesion, improving the toughness of the polylactic acid film, and enhancing its puncture resistance.
[0029] Preferably, the compatibilizer comprises epoxy soybean oil and lysine diisocyanate in a mass ratio of 1:0.5-1.
[0030] By adopting the above technical scheme, the isocyanate group of lysine diisocyanate reacts with the carboxyl group and hydroxyl group on the polymer to generate a graft copolymer, which is distributed at the interface between the two phases, thereby improving the interfacial adhesion, playing a significant volume-increasing role, and improving the tensile strength and toughness of the polylactic acid film. During the hot-melt blending process, the epoxy group in the epoxy soybean oil undergoes a ring-opening reaction with the terminal hydroxyl group / terminal carboxyl group of the polylactic acid and PBS and the phenyl group on the phenyl silicone resin to generate a graft copolymer, which is distributed at the phase interface to improve the dispersion of PBS and the phenyl silicone resin in the polylactic acid base material and the interfacial adhesion. In addition, the epoxy soybean oil is a small molecule, has a plasticizing effect, and can also improve the toughness of the polylactic acid. Therefore, using epoxy soybean oil and lysine diisocyanate as a compatibilizer can improve the compatibility and interfacial effect of the polylactic acid base material and the toughening agent, and enhance the tensile strength and toughness of the blend.
[0031] In a second aspect, the present application provides a method for preparing a polylactic acid film with high puncture resistance, using the following technical solution:
[0032] A method for preparing a polylactic acid film with high puncture resistance comprises the following steps:
[0033] The polylactic acid base material, polypropylene carbonate, hydrophobically modified graphene oxide, bacterial cellulose, a toughening agent, a compatibilizer, an antioxidant and a lubricant are uniformly mixed to prepare a mixture;
[0034] The mixed material is melted, extruded, cast and stretched to obtain a polylactic acid film.
[0035] By adopting the above technical scheme, the raw materials are blended and then hot-melted, extruded, cast and stretched to prepare a polylactic acid film. The preparation method is simple and easy to realize industrial production.
[0036] In summary, this application has the following beneficial effects:
[0037] 1. Since the present application adopts raw materials such as polypropylene carbonate, hydrophobically modified graphene oxide, bacterial cellulose, and toughening agents to improve the toughness and barrier properties of polylactic acid films, and since the graphene oxide is hydrophobically modified, it is evenly dispersed with the polylactic acid base material, polypropylene carbonate has good compatibility with polylactic acid and high toughness, and the hydroxyl groups on the bacterial cellulose can hydrogen bond with the carbonyl groups on the polylactic acid base material to increase the strength of the force, thereby further improving the toughness of the polylactic acid film and improving the puncture resistance. In addition, the layer structure of the hydrophobic graphene oxide is distributed in the polylactic acid film, and the porous structure of the bacterial cellulose can extend the gas permeation path and improve the barrier capacity of the polylactic acid film.
[0038] 2. In the present application, it is preferred to graft methylsilane on the surface of graphene oxide, form a dispersion with dichloromethane, mix it with polylactic acid emulsion, make mixed nanoparticles, and then blend and extrude with polylactic acid resin, so as to improve the compatibility of hydrophobic graphene oxide and polylactic acid base material, and improve the tensile strength, elastic modulus and puncture resistance of polylactic acid film.
[0039] 3. In the present application, it is preferred to use an impregnation solution formed by polyvinyl alcohol and lactic acid-citric acid copolymer to perform negative pressure impregnation pretreatment on bacterial cellulose, thereby reducing the hydroxyl content on the surface of bacterial cellulose and increasing the compatibility of bacterial fiber with polylactic acid base material, improving the mechanical properties and barrier properties of polylactic acid film, and loading nano zinc oxide on bacterial cellulose to make the bacterial cellulose have an antibacterial effect, thereby making the polylactic acid film have better antibacterial effect. DETAILED DESCRIPTION
[0040] The following examples further illustrate the present application in detail.
[0041] Preparation Examples 1-6 of Hydrophobically Modified Graphene Oxide
[0042] Preparation Example 1: (1) 10 g of graphene oxide was dispersed in 90 g of deionized water, 5 g of imidazole catalyst and 5 g of tert-butyldimethylsilyl chloride were added, stirred at room temperature for 12 h, vacuum dried at 50 ° C for 4 h, dispersed in 90 g of dichloromethane, and ultrasonicated for 30 min to prepare a dispersion. The graphene oxide was selected from Nanjing Jicang Nano Technology, model JCGO-1-35, and imidazole was selected from Jingmen Dongxin Biotechnology Co., Ltd.;
[0043] (2) Add 100 g of polylactic acid resin to 900 g of dichloromethane and stir to dissolve to obtain a polylactic acid emulsion. The melt index of the polylactic acid resin is 5 g / 10 min and the density is 2 g / cm 3 , selected from Total L130 in Thailand;
[0044] (3) mixing the dispersion and the polylactic acid emulsion, spray drying, and preparing mixed nanoparticles, wherein the inlet air temperature during spray drying is 40° C., the outlet air temperature is 30° C., and the flow rate is 5 ml / min;
[0045] (4) 10 g of the mixed nanoparticles prepared in step (3) were mixed with 100 g of polylactic acid resin in a mass ratio of 0.1:1, melted, extruded, and granulated at 210° C. to obtain hydrophobically modified graphene oxide. The polylactic acid resin had a melt index of 5 g / 10 min and a density of 2 g / cm 3 , selected from Thailand Total L130.
[0046] Preparation Example 2: (1) Disperse 10 g of graphene oxide in 90 g of deionized water, add 3 g of imidazole catalyst and 3 g of tert-butyldimethylsilyl chloride, stir at room temperature for 10 h, and vacuum dry at 50 ° C for 4 h to obtain hydrophobically modified graphene oxide, the graphene oxide is selected from Nanjing Jicang Nano Technology, model JCGO-1-35, and imidazole is selected from Jingmen Dongxin Biotechnology Co., Ltd.;
[0047] (2) Add 200 g of polylactic acid resin into 1800 g of dichloromethane and stir to dissolve to obtain a polylactic acid emulsion. The melt index of the polylactic acid resin is 8 g / 10 min and the density is 1.24 g / cm 3 , selected from Thailand Total LX175;
[0048] (3) mixing the dispersion and the polylactic acid emulsion, spray drying, and preparing mixed nanoparticles, wherein the inlet air temperature during spray drying is 40° C., the outlet air temperature is 30° C., and the flow rate is 5 ml / min;
[0049] (4) 20 g of the mixed nanoparticles prepared in step (3) were mixed with 100 g of polylactic acid resin at a mass ratio of 0.2:1, melted, extruded, and granulated at 210° C. to obtain hydrophobically modified graphene oxide. The polylactic acid resin had a melt index of 8 g / 10 min and a density of 1.24 g / cm 3 , selected from Thailand Total LX175.
[0050] Preparation Example 3: (1) 10 g of graphene oxide was dispersed in 90 g of deionized water, 5 g of imidazole catalyst and 5 g of tert-butyldimethylsilyl chloride were added, stirred at room temperature for 12 h, and vacuum dried at 50 ° C for 4 h. The graphene oxide was selected from Nanjing Jicang Nano Technology, model JCGO-1-35, and imidazole was selected from Jingmen Dongxin Biotechnology Co., Ltd.;
[0051] (2) The product obtained in step (1) was mixed with 200 g of polylactic acid resin, melted, extruded and granulated at 210° C. The melt index of the polylactic acid resin was 5 g / 10 min and the density was 2 g / cm 3 , selected from Thailand Total L130.
[0052] Preparation Example 4: (1) 10 g of graphene oxide was dispersed in 90 g of deionized water, 5 g of imidazole catalyst and 5 g of tert-butyldimethylsilyl chloride were added, stirred at room temperature for 12 h, and vacuum dried at 50 ° C for 4 h. The graphene oxide was selected from Nanjing Jicang Nano Technology, model JCGO-1-35, and imidazole was selected from Jingmen Dongxin Biotechnology Co., Ltd.;
[0053] (2) The product obtained in step (1) was mixed with 100 g of polylactic acid resin, melted, extruded and granulated at 210° C. to obtain mixed nanoparticles. The polylactic acid resin had a melt index of 5 g / 10 min and a density of 2 g / cm 3 , selected from Total L130 in Thailand;
[0054] (3) 10 g of the mixed nanoparticles prepared in step (3) were mixed with 100 g of polylactic acid resin in a mass ratio of 0.1:1, melted, extruded, and granulated at 210° C. to obtain hydrophobically modified graphene oxide. The polylactic acid resin had a melt index of 5 g / 10 min and a density of 2 g / cm 3 , selected from Thailand Total L130.
[0055] Preparation Example 5: (1) Disperse 10 g of graphene oxide in 90 g of deionized water, add 5 g of imidazole catalyst and 5 g of tert-butyldimethylsilyl chloride, stir at room temperature for 12 h, and vacuum dry at 50 ° C for 4 h. The graphene oxide is selected from Nanjing Jicang Nano Technology, model JCGO-1-35, and the imidazole is selected from Jingmen Dongxin Biotechnology Co., Ltd.;
[0056] (2) Add 100 g of polylactic acid resin to 900 g of dichloromethane and stir to dissolve to obtain a polylactic acid emulsion. The melt index of the polylactic acid resin is 5 g / 10 min and the density is 2 g / cm 3 , selected from Total L130 in Thailand;
[0057] (3) adding the product obtained in step (1) to the polylactic acid emulsion, stirring evenly, and spray drying; during the spray drying, the air inlet temperature is 40° C., the air outlet temperature is 30° C., and the fluid rate is 5 ml / min.
[0058] Preparation Example 6: Disperse 10 g of graphene oxide in 90 g of deionized water, add 5 g of imidazole catalyst and 5 g of tert-butyldimethylchlorosilane, stir at room temperature for 12 h, vacuum dry at 50 ° C for 4 h, disperse in 90 g of dichloromethane, ultrasonicate for 30 min to make a dispersion, graphene oxide is selected from Nanjing Jichang Nano Technology, model JCGO-1-35, imidazole is selected from Jingmen Dongxin Biotechnology Co., Ltd.
[0059] Preparation Example 7 of Bacterial Cellulose
[0060] Preparation Example 7: Inoculate 6% of Xylella fastidiosa into the seed culture medium, activate and culture at 30°C and 150r / min for 48h, inoculate the activated seed liquid into the fermentation medium at a volume fraction of 6%, and mix thoroughly. Subsequently, pour the inoculated culture medium evenly into a large culture dish, culture it at a constant temperature of 30°C for 10d to obtain film-like bacterial cellulose, wash it repeatedly with a large amount of deionized water to remove the residual culture medium on the surface, and then place it in a 0.1mol / l sodium hydroxide solution, water bath it at 100°C for 1h, further remove the residual culture medium and residual bacteria, wash it repeatedly with deionized water until it is neutral, and crush it to make bacterial cellulose with a length of 5μm.
[0061] Preparation Example 8 of Lactic Acid-Citric Acid Copolymer
[0062] Preparation Example 8: An aqueous L-lactic acid solution with a concentration of 88% and citric acid were mixed in a molar ratio of 12:1, dehydrated at 150°C under normal pressure for 2 hours, reduced pressure to 100 mmHg and reacted for 2 hours, and finally reacted at 30 mmHg for 4 hours to obtain L-lactic acid and citric acid copolymers. A 100-mL three-necked flask was equipped with a mechanical stirring system and a vacuum reflux system connected to an air condenser, the air condenser was filled with 3A molecular sieves, the above-mentioned L-lactic acid and citric acid copolymers were added, heated to 100°C, gradually reduced pressure to 5 mmHg, reacted for 8 hours, cooled to room temperature, dissolved in acetone, and then the product was precipitated with a large amount of distilled water, filtered under reduced pressure, and vacuum dried at 40°C for 48 hours.
[0063] Example
[0064] Example 1: A polylactic acid film with high puncture resistance, the raw material dosage is shown in Table 1, wherein the melt index of the polylactic acid base material is 5g / 10min, and the density is 2g / cm 3 , selected from Thailand Total L130, polypropylene carbonate selected from Dongguan Mingxun New Materials, model 8825, hydrophobically modified graphene oxide is prepared by Preparation Example 1, bacterial cellulose is prepared by Preparation Example 7, the toughening agent includes phenyl silicone resin, PBS and hydroxylated PCL in a mass ratio of 0.5:0.3:1, the phenyl silicone resin model is N9810, the hydroxylated PCL is selected from Chuangsai Youxuan, the article number is PE03153, PBS is selected from Thailand PPT Chemical Co., Ltd., model FD92PB, the compatibilizer includes epoxy soybean oil and lysine diisocyanate in a mass ratio of 1:1, the epoxy soybean oil model is E8088, the epoxy value is 6.5%, lysine diisocyanate is selected from Huateng Pharmaceutical, the article number is 101051, the antioxidant is antioxidant 1010, and the lubricant is zinc stearate.
[0065] The method for preparing the above-mentioned polylactic acid film with high puncture resistance comprises the following steps:
[0066] S1, uniformly mixing polylactic acid base material, polypropylene carbonate, hydrophobically modified graphene oxide, bacterial cellulose, toughening agent, compatibilizer, antioxidant and lubricant to prepare a mixture;
[0067] S2. The mixture was melted, extruded and cast at 210°C to form a film with a thickness of 450 μm. The film was preheated at 70°C for 12 seconds and biaxially stretched at a speed of 65 mm / s with a stretching ratio of 4×4 to obtain a polylactic acid film with a thickness of 35 μm.
[0068] Table 1 Amount of raw materials used for high puncture resistance polylactic acid film in Examples 1-4
[0069]
[0070]
[0071] Example 2: A polylactic acid film with high puncture resistance, the raw material dosage is shown in Table 1, wherein the polylactic acid base material has a melt index of 8 g / 10 min and a density of 1.24 g / cm 3 , selected from Thailand Total LX175, polypropylene carbonate selected from Dongguan Mingxun New Materials, model 8825, hydrophobically modified graphene oxide is prepared by Preparation Example 2, bacterial cellulose is prepared by Preparation Example 7, the toughening agent includes phenyl silicone resin, PBS and hydroxylated PCL in a mass ratio of 0.3:0.1:1, the phenyl silicone resin model is N9810, the hydroxylated PCL is selected from Chuangsai Youxuan, the article number is PE03153, PBS is selected from Thailand PPT Chemical Co., Ltd., model FD92PB, the compatibilizer includes epoxy soybean oil and lysine diisocyanate in a mass ratio of 1:0.5, the epoxy soybean oil model is E8088, the epoxy value is 6.5%, lysine diisocyanate is selected from Huateng Pharmaceutical, the article number is 101051, the antioxidant is antioxidant 1010, and the lubricant is zinc stearate.
[0072] The method for preparing the above-mentioned polylactic acid film with high puncture resistance comprises the following steps:
[0073] S1, uniformly mixing polylactic acid base material, polypropylene carbonate, hydrophobically modified graphene oxide, bacterial cellulose, toughening agent, compatibilizer, antioxidant and lubricant to prepare a mixture;
[0074] S2. The mixture was melted, extruded and cast at 200°C to form a film with a thickness of 400 μm. The film was preheated at 75°C for 10 seconds and biaxially stretched at a speed of 65 mm / s with a stretching ratio of 4×4 to obtain a polylactic acid film with a thickness of 35 μm.
[0075] Example 3-4: A polylactic acid film with high puncture resistance, which is different from Example 1 in that the amounts of raw materials used are as shown in Table 1.
[0076] Example 5: A polylactic acid film with high puncture resistance, which is different from Example 1 in that the toughening agent includes PBS and hydroxylated PCL in a mass ratio of 0.3:1.
[0077] Example 6: A polylactic acid film with high puncture resistance, which is different from Example 1 in that the toughening agent is hydroxylated PCL.
[0078] Example 7: A polylactic acid film with high puncture resistance. The difference from Example 1 is that no phenyl silicone resin and hydroxylated PCL are added to the toughening agent, and both are PBS.
[0079] Example 8: A polylactic acid film with high puncture resistance, which is different from Example 1 in that the toughening agent includes phenyl silicone resin and PBS in a mass ratio of 0.5:0.3.
[0080] Example 9: A polylactic acid film with high puncture resistance, which is different from Example 1 in that the bacterial cellulose is pretreated as follows:
[0081] 100g of polyvinyl alcohol was added to N,N-dimethylformamide, stirred and dissolved to obtain a PVA solution with a concentration of 5wt%, and 30g of lactic acid-citric acid copolymer was added and stirred and dissolved to obtain an impregnation solution, wherein the polyvinyl alcohol was 1799 and had a molecular weight of 440,500, and the lactic acid-citric acid copolymer was prepared by Preparation Example 8;
[0082] The bacterial cellulose was added to the impregnation solution, impregnated at -0.03 MPa for 48 hours, and allowed to stand and dry. The mass ratio of the bacterial cellulose to the polyvinyl alcohol was 0.7:1.
[0083] Example 10: A polylactic acid film with high puncture resistance, which is different from Example 1 in that the bacterial cellulose is pretreated as follows:
[0084] 100g of polyvinyl alcohol was added to N,N-dimethylformamide, stirred and dissolved to obtain a PVA solution with a concentration of 3wt%, and 10g of lactic acid-citric acid copolymer was added and stirred and dissolved to obtain an impregnation solution, wherein the polyvinyl alcohol was 1799 and had a molecular weight of 440,500, and the lactic acid-citric acid copolymer was prepared by Preparation Example 8;
[0085] The bacterial cellulose was added into the impregnation solution, impregnated at -0.01 MPa for 50 h, and allowed to stand and dry. The mass ratio of the bacterial cellulose to the polyvinyl alcohol was 0.2:1.
[0086] Example 11: A polylactic acid film with high puncture resistance, which is different from Example 1 in that the bacterial cellulose is pretreated as follows:
[0087] Add 100g of polyvinyl alcohol to N,N-dimethylformamide, stir and dissolve, and prepare a 5wt% PVA solution as the impregnation solution. The polyvinyl alcohol is 1799 and the molecular weight is 440,500.
[0088] The bacterial cellulose was added into the impregnation solution, impregnated at -0.01 MPa for 50 h, and allowed to stand and dry. The mass ratio of the bacterial cellulose to the polyvinyl alcohol was 0.2:1.
[0089] Example 12: A polylactic acid film with high puncture resistance, which is different from Example 1 in that the bacterial cellulose is pretreated as follows:
[0090] 30 g of lactic acid-citric acid copolymer was added to 1900 g of N,N-dimethylformamide and stirred to dissolve to prepare an impregnation solution. The lactic acid-citric acid copolymer was prepared according to Preparation Example 8;
[0091] The bacterial cellulose was added into the impregnation solution, impregnated at -0.01 MPa for 50 hours, and allowed to stand and dry. The mass ratio of the bacterial cellulose to the lactic acid-citric acid copolymer was 0.7:0.3.
[0092] Example 13: A polylactic acid film with high puncture resistance, which is different from Example 9 in that the bacterial cellulose is subjected to the following treatment before being added to the impregnation solution:
[0093] The bacterial cellulose was placed in a 5wt% sodium hydroxide solution, boiled for 1.0h, cooled and dried, and then placed in an 8wt% nano zinc oxide dispersion, immersed at -0.08MPa for 2h, filtered, washed with deionized water, and vacuum dried. The nano zinc oxide dispersion was prepared by mixing 8g nano zinc oxide, 1.6g gelatin, 92g distilled water and 0.8g sodium dodecylbenzene sulfonate and grinding for 30min. The nano zinc oxide was selected from Darcynion, model XDN-GC30, with a particle size of 20nm.
[0094] Example 14: A polylactic acid film with high puncture resistance, which is different from Example 9 in that the bacterial cellulose is subjected to the following treatment before being added to the impregnation solution:
[0095] The bacterial cellulose was placed in a 4wt% sodium hydroxide solution, boiled for 1.5h, cooled and dried, and then immersed in a 4wt% nano zinc oxide dispersion at -0.05MPa for 3h, filtered, washed with deionized water, and vacuum dried. The nano zinc oxide dispersion was prepared by mixing 4g nano zinc oxide, 0.4g gelatin, 96g distilled water and 0.04g sodium dodecylbenzene sulfonate and grinding for 30min. The nano zinc oxide was selected from Darcynion, model XDN-GC30, with a particle size of 20nm.
[0096] Example 15: A polylactic acid film with high puncture resistance, which differs from Example 1 in that an equal amount of tea polyphenols is used instead of nano zinc oxide.
[0097] Comparative Example
[0098] Comparative Example 1: A polylactic acid film with high puncture resistance, which differs from Example 1 in that an equal amount of graphene oxide is used to replace the hydrophobically modified graphene oxide, and the graphene oxide is selected from Nanjing Jichang Nanotechnology, and the model is JCGO-1-35.
[0099] Comparative Example 2: A polylactic acid film with high puncture resistance, which differs from Example 1 in that no bacterial cellulose is added.
[0100] Comparative Example 3: A polylactic acid film with high puncture resistance, which differs from Example 1 in that polypropylene carbonate is not added.
[0101] Comparative Example 4: A processing technology for a biodegradable heat shrinkable film, comprising the following steps:
[0102] S1. Preparation of modified polylactic acid: 90 parts of polylactic acid, 10 parts of allyl (diisopropylamino) dimethyl silane and 1 part of benzoyl peroxide were mixed evenly, and then transferred to a twin-screw extruder for reaction. The screw speed was 100 rpm and the reaction temperature was 170°C. The product was cooled, pelletized and dried to obtain modified polylactic acid.
[0103] S2. Processing of heat shrinkable film: (1) 100 parts of modified polylactic acid, 1 part of fatty alcohol polyoxyethylene ether AEO-9, 1 part of ethylene bisstearamide, 1 part of antioxidant 1076, and 0.5 part of light stabilizer 944 are mixed uniformly, and dried to a water content of less than 100 ppm; (2) the mixture obtained in step (1) is transferred to a twin-screw extruder, melt-extruded at a melt extrusion temperature of 190°C, cast into a sheet at a die, wound around the sheet, biaxially stretched at a biaxial stretching temperature of 110°C, cooled and shaped, and rolled up to obtain a heat shrinkable film with a thickness of 35 μm.
[0104] Comparative Example 5: a commercially available polylactic acid film with a thickness of 35 μm.
[0105] Performance testing
[0106] The polylactic acid film was prepared according to the methods in the examples and comparative examples, and the properties of the polylactic acid film were tested according to the following methods. The test results are recorded in Table 2.
[0107] 1. Tensile strength and elastic modulus: The test is carried out in accordance with GB / T1040.3-2006 "Determination of tensile properties of plastics Part 3: Test conditions for films and sheets". The sample gauge length is 50mm, width is 10mm, and the tensile rate is 50mm / min.
[0108] 2. Puncture resistance: Test according to 37841-2019 "Test method for puncture resistance of plastic films and sheets".
[0109] 3. Oxygen permeability: Tested in accordance with GB / T1038-2000 "Plastic Film and Sheet Gas Permeability Test Method Pressure Difference Method", with the test humidity at 0% RH and the test temperature at 23°C.
[0110] 4. Water vapor transmission rate: Tested in accordance with GB / T1037-1988 "Test method for water vapor transmission of plastic film and sheet - Cup method", the test humidity is 90% RH, and the test temperature is 30℃.
[0111] 5. Antibacterial rate: GB / T31402-2015 "Test method for antibacterial properties of plastic surfaces" was used for testing, and Escherichia coli and Staphylococcus aureus were selected as test bacteria.
[0112] Table 2 Performance test of polylactic acid film
[0113]
[0114] It can be seen from the data in Table 2 that Examples 1 and 2 respectively use the hydrophobically modified graphene oxide prepared in Preparation Example 1 and Preparation Example 2, and Examples 3 and 4 undergo phase change with Example 1, with different amounts of raw materials used. The polylactic acid films prepared in Examples 1-4 have high tensile strength and elastic modulus, high puncture resistance, and strong barrier properties to water vapor and oxygen, indicating that the polylactic acid films prepared using raw materials such as hydrophobically modified graphene oxide, bacterial cellulose and polypropylene carbonate in this application have strong toughness and good barrier properties.
[0115] Compared with Example 1, Example 5 uses PBS and hydroxylated PCL as toughening agents, and no phenyl silicone resin is added. Compared with Example 1, Example 6 only uses hydroxylated PCL as a toughening agent. Table 2 shows that the tensile strength, elastic modulus and puncture resistance of the polylactic acid film prepared in Example 5 are lower than those in Example 1, and the toughness of the polylactic acid film prepared in Example 6 is lower than that in Example 5, indicating that the use of phenyl silicone resin, PBS and hydroxylated PCL as toughening agents can effectively improve the toughness of the polylactic acid film.
[0116] In Example 7, only PBS is used as a toughening agent, while in Example 8, phenyl silicone resin and PBS are used as toughening agents. The tensile strength and other mechanical properties of the polylactic acid film prepared in Example 8 are better than those in Example 7, but not as good as those in Example 5, indicating that the combination effect of phenyl silicone resin and hydroxylated PCL is better than that of phenyl silicone resin and PBS.
[0117] Compared with Example 1, Examples 9 and 10 use polyvinyl alcohol and lactic acid-citric acid copolymer to pretreat bacterial cellulose. As can be seen from Table 2, the polylactic acid films prepared in Examples 9 and 10 have significantly improved water vapor barrier properties, slightly improved oxygen barrier properties, and improved tensile strength, elastic modulus and puncture resistance of the polylactic acid films.
[0118] In Example 11, when pretreating bacterial cellulose, no lactic acid-citric acid copolymer was added. Compared with Example 9, the tensile strength, elastic modulus and puncture resistance of the polylactic acid film prepared in Example 11 were weakened, and the barrier ability to water vapor decreased.
[0119] In Example 12, when bacterial cellulose was pretreated, polyvinyl alcohol was not added. Compared with Example 9, the mechanical properties of the polylactic acid film prepared in Example 12, such as tensile strength, were weakened, the moisture permeability was increased, and the water vapor barrier effect was weakened.
[0120] Compared with Example 9, in Example 13 and Example 14, nano zinc oxide is loaded on the surface of bacterial cellulose before impregnating it in the impregnation solution, so that the mechanical strength of the polylactic acid film is improved to a certain extent and the antibacterial ability is significantly increased; while in Example 15, tea polyphenols are used instead of nano zinc oxide, and the antibacterial ability of the polylactic acid film prepared is not as good as that of Example 13 and Example 14.
[0121] In Comparative Example 1, graphene oxide was not hydrophobically modified. Compared with Example 1, the tensile strength, elastic modulus and puncture resistance of the polylactic acid film were significantly reduced, and the barrier effect against water vapor and oxygen was weakened.
[0122] Compared with Example 1, Comparative Example 2 did not add bacterial cellulose. Table 2 shows that the oxygen barrier property of the polylactic acid film is reduced, but the water barrier property is improved. This shows that although bacterial cellulose has a porous structure and can extend the oxygen permeation path, it is hydrophilic in itself, which will have a certain impact on the water barrier property of the polylactic acid film.
[0123] In Comparative Example 3, no polypropylene carbonate was added. Compared with Example 1, the tensile strength and elastic modulus of the polylactic acid film prepared in Comparative Example 3 decreased, and the anti-puncture effect was weakened.
[0124] Comparative Example 4 is a polylactic acid film prepared by the prior art. Although its mechanical properties such as puncture resistance and tensile strength are improved compared with those of commercially available polylactic acid films, they are still inferior to those of the present application, and its barrier properties to water vapor and oxygen are relatively poor.
[0125] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A polylactic acid film with high puncture resistance, characterized in that: The invention comprises the following raw materials in parts by weight: 60-70 parts of polylactic acid base material, 30-40 parts of polypropylene carbonate, 1.5-2.5 parts of hydrophobically modified graphene oxide, 1-2 parts of bacterial cellulose, 0.1-0.5 parts of toughening agent, 0.02-0.1 parts of compatibilizer, 0.25-2.5 parts of lubricant, and 0.25-1.5 parts of antioxidant; The preparation method of the hydrophobically modified graphene oxide is as follows: Disperse graphene oxide in deionized water, add imidazole catalyst and tert-butyldimethylsilyl chloride, stir at room temperature for 10-12 hours, vacuum dry, disperse in dichloromethane, and ultrasonicate for 20-30 minutes to prepare a dispersion; Adding polylactic acid resin into dichloromethane, stirring and dissolving, to obtain polylactic acid emulsion, wherein the mass ratio of polylactic acid resin to graphene oxide is 1:0.05-0.1; The dispersion and the polylactic acid emulsion are mixed and spray-dried to prepare hybrid nanoparticles; The mixed nanoparticles and polylactic acid resin are mixed in a mass ratio of 0.1-0.2:1, melted, and extruded to obtain hydrophobically modified graphene oxide; The bacterial cellulose is pretreated as follows: Add polyvinyl alcohol to N,N-dimethylformamide, stir and dissolve to obtain a PVA solution with a concentration of 3-5wt%, add lactic acid-citric acid copolymer, stir and dissolve to obtain an impregnation solution, and the mass ratio of polyvinyl alcohol to lactic acid-citric acid copolymer is 1:0.1-0.3; Add bacterial cellulose to the impregnation solution, soak for 48-50 hours at - (0.01-0.03) MPa, stand and dry, the mass ratio of bacterial cellulose to polyvinyl alcohol is 0.2-0.7:
1.
2. The polylactic acid film with high puncture resistance according to claim 1, characterized in that: The hydrophobically modified graphene oxide comprises graphene oxide and tert-butyldimethylchlorosilane in a mass ratio of 1:0.3-0.
5.
3. The polylactic acid film with high puncture resistance according to claim 1, characterized in that: The polylactic acid base material and polylactic acid resin have a melt index of 5-8 g / 10 min and a density of 1.4-2 g / cm 3 .
4. The polylactic acid film with high puncture resistance according to claim 1, characterized in that: Before the bacterial cellulose is added to the impregnation solution, the following treatment is first performed: The bacterial cellulose is placed in a sodium hydroxide solution with a concentration of 4-5wt%, boiled for 1-1.5h, cooled and dried, and then placed in a nano zinc oxide dispersion with a concentration of 4-8wt%, immersed for 2-3h at -(0.05~0.08)MPa, filtered, washed with deionized water, and vacuum dried.
5. The polylactic acid film with high puncture resistance according to claim 4, characterized in that: The nano zinc oxide dispersion is prepared by mixing nano zinc oxide, gelatin, distilled water and sodium dodecylbenzene sulfonate and grinding for 20-30 minutes. The amount of sodium dodecylbenzene sulfonate added is 0.01-0.1 of the mass of the nano zinc oxide, and the amount of gelatin added is 0.1-0.2 of the mass of the nano zinc oxide.
6. The polylactic acid film with high puncture resistance according to claim 1, characterized in that: The toughening agent includes phenyl silicone resin, PBS and hydroxylated PCL in a mass ratio of 0.3-0.5:0.1-0.3:
1.
7. The polylactic acid film with high puncture resistance according to claim 6, characterized in that: The compatibilizer comprises epoxy soybean oil and lysine diisocyanate in a mass ratio of 1:0.5-1.
8. The method for preparing the polylactic acid film with high puncture resistance according to any one of claims 1 to 7, characterized in that: The following steps are involved: The polylactic acid base material, polypropylene carbonate, hydrophobically modified graphene oxide, bacterial cellulose, a toughening agent, a compatibilizer, an antioxidant and a lubricant are uniformly mixed to prepare a mixture; The mixed material is melted, extruded, cast and stretched to obtain a polylactic acid film.
Citation Information
Patent Citations
Carbon nanofibers based on carbonized bacterial cellulose as well as composition and application of carbon nanofibers
CN104532407A
Polylactic acid-bacterial cellulose composite material and preparation method thereof
CN105237973A
Antibacterial PE film and preparation method thereof
CN112029171A
Polypropylene-polylactic acid mixed resin / graphene / natural fiber bionanocomposite and manufacturing method of thereof
KR1020130103154A
Degradable high-barrier composite film and preparation method therefor
WO2023115599A1