Ultra-high strength marine engineering steel with high ductility and resistance to seawater corrosion fatigue and manufacturing method thereof

Through low C+Cr-Ni-Cu-Mo alloying and V-N micro-alloying and specific processing, the problems of insufficient corrosion fatigue resistance and high ductility of marine engineering steel in complex marine environments have been solved, and high strength, Marine steel plates with excellent resistance to seawater corrosion fatigue and low-temperature toughness improve the service safety of offshore engineering equipment.

CN117660837BActive Publication Date: 2024-10-22ANGANG STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311619970.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-30
Publication Date
2024-10-22
Estimated Expiration
2043-11-30

AI Technical Summary

Technical Problem

Existing steel for marine engineering has insufficient anti-corrosion fatigue performance and high ductility in complex marine environments, resulting in service safety and reliability problems. Especially in low temperature and seawater corrosive environments, materials are prone to failure, making it difficult to meet the needs of deep sea and offshore development.

Method used

The composition design of low C+Cr-Ni-Cu-Mo alloying and V-N micro-alloying is adopted, combined with secondary heating controlled rolling, DQ online quenching and induction high temperature tempering process, to control the microstructure and grain size of the steel plate. , forming a tempered martensite + ferrite structure to improve the seawater corrosion fatigue resistance and low-temperature toughness of the steel plate.

Benefits of technology

It achieves the high ductility, seawater corrosion fatigue resistance and low-temperature impact toughness of the steel plate. The yield strength is ≥690MPa, the tensile strength is 770~940MPa, the elongation after tensile fracture is ≥26%, the -40℃ impact energy is ≥150J, and the NDTT temperature is ≤ -50℃, significantly improving the service safety of offshore engineering equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117660837B_ABST
    Figure CN117660837B_ABST
Patent Text Reader

Abstract

The invention provides an ultra-high strength marine engineering steel with high ductility and seawater corrosion fatigue resistance and a manufacturing method thereof. The components of the marine engineering steel are as follows by weight percentage: C: 0.04% to 0.06%, Si: 0.15% to 0.25%, Mn: 1.00% to 1.20%, Cr: 2.50% to 3.50%, Ni: 0.90% to 1.30%, Cu: 0.80% to 1.20%, Mo: 0.40% to 0.60%, V: 0.045% to 0.065%, N: 0.017% to 0.025%, Ca: 0.002%~0.005%, P:≤0.01%, S:≤0.001%, Als:0.02%~0.05%, and the rest are Fe and inevitable impurities; the manufacturing method includes smelting, continuous casting, heating, primary heating, primary rolling, primary cooling, secondary heating, secondary rolling, secondary cooling and tempering; the yield strength of the marine engineering steel plate produced by the present invention is ≥690MPa, and the tensile strength is 770~940MPa; the tensile elongation after fracture is ≥26%, the -40℃ KV2 impact energy is ≥150J, and the NDTT temperature is ≤-50℃.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of metal materials, and in particular relates to ultra-high-strength marine engineering steel with high ductility and resistance to seawater corrosion fatigue and a manufacturing method thereof. Background Art

[0002] The particularity of the application environment of marine engineering has always placed high requirements on the service safety of marine equipment and structural materials. In recent years, as the offshore industry is gradually transforming and upgrading to the marine industry, the service environment of marine equipment has become increasingly complex and harsh. Corrosion fatigue resistance and elongation performance are key factors affecting the stability of long-term service of marine equipment and structures. Among them, the maximum loading stress amplitude of corrosion fatigue is often less than the yield limit of the material, and there is no sign before failure. In the process of corrosion fatigue, there are two basic damage modes, one is corrosion damage caused by corrosive media; the other is fatigue damage caused by alternating loads. These two material damage modes are not simply superimposed in this process, but there is an obvious coupling effect, which is the result of the combined action of corrosive environment, fatigue load and material factors. In particular, for marine engineering steel, it has been subjected to the alternating effects of low temperature, chloride ions, dry-wet cycles, wind and waves, and sea ice loads in the marine area for a long time in its service environment, which will lead to a sharp increase in the risk of failure due to corrosion fatigue in such harsh environments. Corrosion fatigue of high-strength steel for marine engineering has become one of the technical bottlenecks that seriously restrict the development of large-scale marine engineering technology and equipment, and its failure problem has seriously affected the reliability and safety of large-scale marine engineering equipment. On the other hand, improving the ductility of steel plates can help to cope with unexpected accidents and operational safety in severe sea conditions that ships and marine engineering equipment may encounter. The American ABS classification society has currently incorporated high ductility performance indicators into relevant specifications. Its purpose is to allow steel plates to absorb the energy of collision when ships, marine engineering equipment and structures collide, making it less likely for the structure to become unstable, thereby improving the service safety of the equipment.

[0003] At present, ultra-high strength steel represented by EH690 is widely used in marine engineering equipment. The higher the strength of steel, the greater its sensitivity to environmental fracture, which restricts its application in complex marine environments. With the deepening of my country's exploration of marine resources, marine engineering applications are developing towards deep sea and offshore. It is necessary to develop 690MPa E-grade marine steel with both corrosion fatigue resistance and high ductility and its manufacturing method to prepare technology for my country's future marine resource development needs.

[0004] Public reports of related patents:

[0005] The EH36 grade marine engineering steel disclosed in the invention "EH36 grade marine engineering steel with high ductility and its manufacturing method" (publication number CN114807761A) has a composition design of C: 0.05%~0.08%, Si: 0.10%~0.30%, Mn: 1.00%~1.50%, Nb: 0.01%~0.04%, V: 0.02%~0.05%, Ti: 0.005%~0.02%, P: ≤0.01%, S: ≤0.01%, Als: 0.01%~0.05%, and the rest is Fe and unavoidable impurities. The chemical composition of the invented steel does not add precious alloy elements such as Ni; by controlling the sulfur and phosphorus content, the microstructure and grain size of the steel plate are regulated by induction heating of the continuous casting billet, two-stage controlled rolling, relaxation and controlled cooling processes, and a steel plate with a high yield rate, stable strength and toughness, and especially high ductility is obtained; however, the shortcoming of this invention is that the strength level of the produced steel plate is not high, and the corrosion performance evaluation has not been carried out.

[0006] The invention "A high-ductility FH500 grade ship plate steel and its production method" (publication number CN108517463A) discloses that the ship plate steel composition is designed to be strengthened with Nb and V micro-alloys, and the controlled rolling and controlled cooling technology is used to obtain the soft phase ferrite and hard phase bainite structure. The controlled cooling stage adopts a three-stage cooling method of water cooling-air cooling-water cooling, and the first stage of cooling requires ultra-fast cooling of 100-150℃ / s. The process control is complex, and the requirements on the capacity of the controlled cooling equipment and the uniformity of the steel plate structure are high. At the same time, the corrosion performance of the steel plate was not evaluated.

[0007] The invention "Anti-corrosion fatigue steel for engineering and its preparation method" (publication number CN112899570A) discloses an anti-corrosion fatigue steel for engineering. Its composition design is based on the main elements of E690 steel (C 0.04-0.07%, Si 0.20-0.26%, Mn 1.45-1.60%, P≤0.01%, S≤0.015%, Cr 0.44-0.50%) to ensure the comprehensive mechanical performance requirements. The initiation and propagation of corrosion fatigue cracks are suppressed by adding and regulating the characteristic elements of Cu, Ni, and Sb to meet the requirements of anti-corrosion fatigue design for engineering steel. Its corrosion fatigue strength can be increased by 52%, but the low-temperature toughness of the steel is not evaluated. The evaluation index only stays at room temperature, which cannot meet the increasingly harsh use environment of marine engineering steel.

[0008] The invention "A high-strength steel for marine use that resists seawater corrosion fatigue and its manufacturing method" (publication number: CN114959418A) discloses a high-strength steel composition design that uses low carbon and adds alloy elements such as Cu, Ni, Cr, Sb, and Sn to improve the corrosion resistance of the steel, adds elements such as Si, Nb, and VN to improve the fatigue performance of the steel, and adds rare earth elements to improve the purity of the steel. Through the interaction between the elements, the initiation and expansion of steel corrosion fatigue cracks are suppressed, and the two-stage rolling process of low-speed and high-pressure reduction in the first stage and high-speed and high-pressure reduction in the second stage is combined. The process finally obtains a steel plate structure of refined equiaxed ferrite + granular bainite + a small amount of pearlite, the ferrite content is ≥85%, the grain size is 10-20μm, the steel plate has good seawater corrosion fatigue resistance, which is 1.5 times that of conventional steel plates, and the tensile elongation of the steel plate is in the range of 26% to 32%. The disadvantage is that this technology focuses on improving the corrosion resistance of steel by adding a large variety of corrosion-resistant characteristic elements and rare earth elements, which increases the difficulty and cost of smelting, and also has an adverse effect on the fatigue and elongation properties of steel.

[0009] The technical solution disclosed in the invention "A method for improving the production efficiency of thick plates in a single-stand rolling mill" (publication number CN111014292A) is mainly to directly cool the intermediate billet after the first heating and rolling, and then heat and roll it for the second time, and then directly roll it to the finished product thickness after the second heating to the target temperature. The method of directly cooling the intermediate billet and then heating and rolling it again eliminates the cooling time of the intermediate billet, which can significantly improve the efficiency of the rolling mill and thus greatly increase the hourly output of the rolling mill. The disadvantage is that this method increases the consumption of energy and industrial water due to the increase in the heating and cooling process in the process path, and the extent of the improvement in production efficiency remains to be discussed. Summary of the invention

[0010] The object of the present invention is to overcome the above problems and shortcomings and to provide an ultra-high strength marine engineering steel having high yield rate, stable strength and toughness, high ductility and resistance to seawater corrosion fatigue, and a method for manufacturing the same.

[0011] The object of the invention is achieved in this way:

[0012] The present invention adopts the composition design of low C + "Cr-Ni-Cu-Mo" alloying + VN microalloying, combines the secondary heating controlled rolling, DQ online quenching and induction high temperature tempering process to control the microstructure and grain size of the steel plate, and obtains a 690Mpa grade steel plate with high yield rate, stable strength and toughness, especially resistance to marine atmospheric corrosion and high ductility. Compared with the above-mentioned public invention, the present invention prepares an ultra-high strength steel plate with seawater corrosion fatigue resistance, high ductility and low temperature toughness suitable for the stress-bearing parts such as the boom, boom and base turntable in offshore lifting equipment. Its comprehensive performance can meet the long-term service conditions of marine engineering equipment, with a tensile elongation after fracture ≥26%, a -40℃ impact energy ≥150J, and a NDTT temperature ≤-50℃.

[0013] A high-ductility seawater corrosion fatigue-resistant ultra-high-strength marine engineering steel, the steel plate has the following components by weight percentage: C: 0.04%-0.06%, Si: 0.15%-0.25%, Mn: 1.00%-1.20%, Cr: 2.50%-3.50%, Ni: 0.90%-1.30%, Cu: 0.80%-1.20%, Mo: 0.40%-0.60%, V: 0.045%-0.065%, N: 0.017%-0.025%, Ca: 0.002%-0.005%, P: ≤0.01%, S: ≤0.001%, Als: 0.02%-0.05%, and the rest is Fe and unavoidable impurities.

[0014] The microstructure of the offshore steel plate is tempered martensite + ferrite, the average length of the tempered martensite lath is less than 15 μm, the volume fraction of ferrite is 7% to 12%, the morphology of the tempered carbonitride is short rod-shaped, and the average major axis size is less than 60 nm. The tempered carbonitride is V (C, N).

[0015] The offshore steel plate has a yield strength of ≥690MPa, a tensile strength of 770-940MPa, a tensile elongation of ≥26%, a -40°C KV2 impact energy of ≥150J, a NDTT temperature of ≤-50°C, and a steel plate thickness of 20-50mm.

[0016] The reasons for the composition design of the present invention are as follows:

[0017] The overall composition design concept of the present invention is embodied in three parts: first, low C and low Mn design is adopted to improve the high elongation performance of the steel plate under the premise of meeting the strength design requirement of 690MPa; second, the strength performance is guaranteed without losing the fatigue performance of the steel plate through the small-sized precipitation phases of V (C, N) and Cu; third, the corrosion resistance of the steel is improved as much as possible without adding too many alloy elements through the composite effect of Cr, Cu, Ni and Mo.

[0018] C: is an essential element to ensure the strength of steel materials. In the present invention, the role of C is mainly reflected in two points: one is to contribute strength in the form of solid solution strengthening, and the other is to contribute strength in the form of precipitation strengthening by cooperating with V and N elements. However, under the premise of meeting the strength design requirements of 690MPa level, from the perspective of high ductility and corrosion fatigue resistance of the steel of the present invention, it is necessary to reduce the C content as much as possible. The strength of the steel of the present invention mainly relies on the fine grain and precipitation strengthening mechanism brought about by the combination of the composition and the manufacturing method of the present invention, and does not rely on increasing the C content to achieve strength improvement. Therefore, after comprehensive consideration, a low C component design is adopted, and the C content is preferably controlled at C: 0.04% to 0.06%.

[0019] Si: It is the main deoxidizing component in the steelmaking process. Si in the form of solid solution will increase the strength while also increasing the ductile-brittle transition temperature, elastic limit and fatigue strength. In order to obtain a sufficient deoxidation effect, it must contain more than 0.10%. However, too high an upper limit will reduce the toughness of the base material and the weld, and have an adverse effect on the surface quality of the steel. The preferred Si content is 0.15% to 0.25%.

[0020] Mn: Mn is an essential element to ensure the strength and toughness of steel. With the increase of Mn content, the strength of steel increases significantly. 1% Mn can increase the tensile strength by about 100MPa. However, the Mn element is easy to segregate in steel, and it is easy to segregate at 1 / 4 and 1 / 2 thickness of medium and thick steel plates, which will cause a strong reduction in low-temperature toughness and even the phenomenon of impact fracture stratification. On the other hand, the present invention also adds Cr and Mo elements in the composition design and the manufacturing method involves tempering in the temperature range of 500 to 650°C. Under the premise of meeting the strength design requirements of 690MPa level, the low Mn design can effectively avoid segregation and the risk of second-type temper brittleness. In addition, reducing the Mn content is also beneficial to improving the corrosion resistance of the steel plate. Therefore, considering the material mechanics and corrosion resistance, it is preferred that the Mn content range is controlled within 1.00% to 1.20%.

[0021] Cr: Cr is an effective element to improve the corrosion resistance of steel. The addition of Cr in steel has a significant effect on the electrochemical process of steel. Cr can inhibit the anodic dissolution process in the electrochemical process, and the corrosion potential of the steel matrix shifts positively. The higher the amount of Cr added, the more obvious the inhibitory effect on the anodic process. On the one hand, Cr can form Cr2O3 and Cr(OH)3 products with better stability and corrosion resistance in the rust layer; on the other hand, Cr can promote the formation of α-FeOOH in the rust layer, and a part of it will be doped in α-FeOOH and Fe3O4 to form thermodynamically more stable α-(Fe,Cr)OOH and FeCr2O4. Under the combined effect of the two, the stability and protection of the rust layer of Cr-containing steel are greatly improved. The Cr-containing products in the rust layer can improve the original loose and porous network structure of the rust layer, provide more nucleation sites, and the rust particles gradually spheroidize and refine, which is conducive to the subsequent close agglomeration and fusion between particles, and the defects in the rust layer are reduced. With the extension of time, the structure of the rust layer gradually densifies, which can effectively hinder the penetration of corrosive Cl- ions in seawater. In addition, Cr is also an effective element for improving the strength of steel plates, but excessive Cr may cause a decrease in welding performance, so the present invention controls the Cr content to 2.5% to 3.5%.

[0022] Ni: Ni has a solid solution strengthening effect, which can improve the strength and toughness of steel. It has the characteristics of lowering the Ar3 point and minimizing the increase in carbon equivalent or cold crack sensitivity coefficient Pcm. Ni is also one of the key alloying elements for improving the corrosion resistance of steel plates. Adding Ni elements to steel can promote the formation of a stable, dense, chloride ion-resistant amorphous layer on the surface of the steel plate, inhibit the permeability of chloride ions and oxygen atoms, and improve the corrosion resistance of the steel plate. In addition, for the steel of the present invention, because a higher content of Cu elements is added to the steel by design, the addition of Ni elements can effectively inhibit the occurrence of cracks in Cu-containing steel during heating and hot rolling, but the cost of adding Ni elements is relatively high, so the present invention controls the Ni content range to 0.90% to 1.30%.

[0023] Cu: Cu is an essential element for resisting marine atmospheric corrosion. During the corrosion process of steel, it will be enriched in the inner rust layer in the form of CuO, which can well isolate corrosive media, reduce the promoting effect of chloride ions on corrosion, and increase the polarization resistance of steel, resulting in enhanced protectiveness of the rust layer, thereby improving the corrosion resistance of steel. On the other hand, in the present invention, the addition of Cu element is mainly to consider the precipitation strengthening effect of Cu in steel. During the tempering process of quenched steel, the lath substructure undergoes recovery recrystallization, and Cu forms small-sized precipitation phases at the dislocation line and lath boundary, producing strong precipitation strengthening. Especially under the induction high temperature tempering conditions with high heating rate, the precipitation phase nucleation speed is fast and not easy to coarsen, which is conducive to the formation of fine and dispersed Cu second phase, and its effect can reach the optimal value at 600-630°C. In addition, Cu can also effectively improve the welding performance of steel materials, reduce the cold cracking of steel, improve the forming performance and mechanical processing performance of steel, improve the anisotropy ratio of steel, reduce the work hardening index, and improve the fatigue resistance of steel. In order to avoid the hot brittleness of steel caused by Cu addition, the present invention adopts the method of adding Ni and Cu together and accurately controlling the composition, so that Cu can be uniformly dissolved to reduce the negative impact. Taking into account the material processing, mechanical and corrosion resistance, the preferred Cu content range is controlled within 0.80% to 1.20%.

[0024] Mo: Mo is a recognized local corrosion resistant element. Whether in the metallic state or in the oxidized state, Mo in the rust layer can increase the resistivity of the rust layer, the densification degree of the rust layer, and thus improve the protectiveness of the rust layer. Mo and Cr also have a certain synergistic effect, which can promote the transformation process of alloy elements in the rust layer into corrosion-resistant products. In addition, Mo can also improve the hardenability and fatigue properties of steel. The present invention controls the range of Mo to be 0.40% to 0.60%.

[0025] V: V has a strong affinity with both C and N. The fine V (C, N) particles dispersed in the ferrite are the main way of strengthening by vanadium microalloying. The V (C, N) precipitates in the ferrite conform to the BN orientation relationship with the ferrite matrix, and maintain a coherent relationship with the ferrite matrix in the initial stage of uniform precipitation in the ferrite. Compared with other microalloying elements such as Nb and Ti, the carbides and nitrides of V have the smallest mismatch with the ferrite matrix, and the coherent relationship between the carbides and nitrides of V and the ferrite matrix can be maintained to a larger particle size, which is beneficial to improve the resistance of steel to fatigue crack initiation and expansion, and also improve the yield strength ratio, low temperature toughness and welding performance of steel. However, the V content should not be too high, otherwise it will reduce the toughness of the steel and be detrimental to the creep performance of the steel. The V content of the present invention is controlled at 0.045% to 0.065%.

[0026] N: An important strengthening element of the present invention, N exists in steel mainly in two states: free state and compound. The existence of the former is not good for the toughness of the steel plate, while the existence of the latter has a positive effect on the comprehensive performance of the steel plate. For V-containing steel, when there is a lack of N in the steel, most of the V does not fully exert its precipitation strengthening effect. Whether in austenite or in ferrite, the solubility of VN is much lower than that of VC. That is to say, the precipitation of VN in austenite and ferrite always has a greater chemical driving force. Therefore, as long as there is enough N element in the matrix, the greater chemical driving force will cause N-rich V (C, N) to precipitate preferentially in ferrite or austenite. N-containing steel not only eliminates the cost increase caused by degassing and refining to remove N during the steelmaking process, but also the increase of N in the steel can give full play to the role of V microalloying elements, saving the amount of alloying elements, thereby reducing production costs. The N content in the steel affects both the interphase precipitation and random precipitation process of V(C,N) in ferrite. N-rich V(C,N) has a greater chemical driving force when precipitating, so its nucleation rate during precipitation increases significantly. As the N content increases, the interlayer spacing and precipitate size of V(C,N) interphase precipitation decrease, the density of random precipitated particles in ferrite increases, and the size of precipitated particles decreases. Considering that the corrosion fatigue performance requirements of the steel of the present invention should take into account both the size and density of the precipitates, the range of N is controlled to be 0.017% to 0.025%.

[0027] Ca: Ca treatment is performed on molten steel to purify the molten steel. The Ca element can spheroidize the MnS inclusions and disperse their size, preventing the MnS inclusions from forming long strip plastic shapes during the rolling process, and forming dispersed spherical shapes, and refining the size of sulfide inclusions, inhibiting the hot brittleness of S, improving the impact toughness and Z-direction performance of the steel plate, and improving the anisotropy of the impact toughness of the steel plate. The amount of Ca added depends on the S content in the steel. If the Ca addition is too low, the treatment effect is not great; if the Ca addition is too high, the size of Ca(O,S) is too large, the brittleness is also increased, and it can become the starting point of the fracture crack, reducing the low-temperature toughness of the steel, while also reducing the purity of the steel and polluting the molten steel. The present invention controls the Ca element content to 0.002% to 0.005%.

[0028] P: P can segregate in the center of the slab and gather at the grain boundaries, and is an element that has an adverse effect on the low-temperature toughness, ductility and weldability of the steel plate. Although P has the effect of improving the marine atmospheric corrosion resistance of the steel plate, considering the damage of P to the mechanical properties of the steel plate, P cannot be used to improve the marine atmospheric corrosion resistance of the steel plate. The present invention requires that the P content be controlled to be no higher than 0.01%.

[0029] S: S can combine with Mn in steel to form MnS inclusions. During hot rolling, MnS extends along the rolling direction to form a MnS inclusion band along the rolling direction, which becomes a crack source and seriously damages the transverse low-temperature impact toughness and Z-direction properties of the steel plate. The content of S in the material of the present invention is controlled to be no higher than 0.001%.

[0030] Als: As a deoxidation and grain refinement element that must be added in the present invention, the added content is above 0.01%, but when it exceeds 0.08%, hot cracks of the casting are likely to occur, and the toughness of the steel is reduced. The Als content is controlled at 0.01% to 0.05%.

[0031] The second technical solution of the present invention is to provide a method for manufacturing high-ductility seawater corrosion fatigue resistant ultra-high strength marine engineering steel, including smelting, heating, primary heating, primary rolling, primary quenching, secondary heating, secondary rolling, secondary quenching, and tempering;

[0032] (1) Smelting process:

[0033] a) During converter smelting, the contents of elements such as C, Si, Mn, P, and S are adjusted to be within the scope of the present invention, and other alloy components are added as required for smelting.

[0034] b) refining the molten steel and adjusting the contents of other alloy elements within the scope of the present invention.

[0035] c) subjecting the refined molten steel to RH treatment for a period of ≥30 min, and blowing nitrogen throughout the RH treatment to ensure that the final N content of the steel is within the range of the present invention, and controlling [H]≤2.0ppm and [O]≤18ppm in the steel.

[0036] (2) The molten steel obtained in step (1) is continuously cast to obtain the desired ingot. In order to improve the center segregation of the ingot, the superheat of the tundish is controlled to be ≤30°C. The pouring is protected throughout, and electromagnetic stirring and light pressure are applied. The electromagnetic stirring: I≥450A.

[0037] (3) One-time heating process: The ingot obtained in step (2) is heated to a temperature of 1180-1250°C. The steel of the present invention has a high alloy content and poor thermal conductivity. In order to control the heating quality of the continuous casting ingot, a segmented heating process is used for the first heating. Below 900°C, slow heating is used to relieve the thermal stress caused by thermal conductivity, and the heating rate is 8-12°C / min. Above 900°C, a rapid heating process is used to prevent abnormal growth of austenite grains, and the heating rate is 15-20°C / min, and the holding time is 2.0-3.5h.

[0038] (3) One-pass rolling process: The rolling temperature is in the austenite recrystallization temperature zone of 1080-1150℃, and the ingot is rolled to 1.5-2.0 times the finished product thickness. The first pass reduction is ≥50mm, and the average single pass reduction rate is above 15%. The purpose is to fully break up the austenite grains of the ingot, so that the dynamic recrystallization process of austenite can proceed fully, thereby refining the austenite grain size.

[0039] (3) Single quenching process: After the first rolling, the intermediate billet is subjected to DQ online quenching. The intermediate billet is rapidly cooled to below 120°C at an average cooling rate of 15-20°C / s and then air-cooled to room temperature. The pretreatment of the intermediate billet before secondary heating and austenitization is completed to obtain a martensitic structure.

[0040] (4) Secondary heating process: The secondary heated intermediate billet is heated to 900-950°C at a heating rate of 15-20°C / min to re-austenitize the intermediate billet. The pre-treated structure after one rolling and cooling is a fine martensite structure. This quenching non-steady-state supersaturated structure has a high internal energy storage. A large number of crystal defects such as dislocations and interfaces can provide a large number of recrystallization nucleation points during the secondary heating austenitization process, and a finer austenite structure can be obtained. The average equivalent diameter of the original austenite grains is ≤15μm. The morphology of the martensite structure after quenching will also be affected by the heredity of the structure. On the other hand, the secondary heating is equivalent to the normalizing treatment. Since the alloy component content of the steel of the present invention is relatively high, the secondary heating is beneficial to the uniform distribution of the alloy elements in the steel.

[0041] (5) Secondary rolling process: The secondary rolling temperature is 830-850℃, the average single-pass reduction rate is 15%-20%, and the final rolling temperature is 800-820℃. The purpose is to fully deform the austenite grains, provide energy storage and position for the phase deformation nuclei, increase the phase deformation nucleus rate, and achieve further grain refinement through dynamic recrystallization during secondary rolling.

[0042] (6) Straightening process: The steel plate must be straightened after rolling to improve the flatness of the steel plate and prevent problems such as warping of the steel plate during the cooling process.

[0043] (7) Secondary quenching process: The straightened steel plate immediately enters the DQ online quenching system at 770-790℃, and completes sub-temperature quenching at an average cooling rate of 15-20℃ / s. The final cooling temperature of the steel plate is less than 120℃, and then air-cooled to room temperature to form a martensite + undissolved ferrite structure. Due to the two austenitization and dynamic recrystallization processes, the martensite structure is subject to the genetic constraints of the organization, and the average length of the martensite lath is less than 15μm. The cooling temperature range of 770-790°C is in the two-phase region between the Ac1-Ac3 temperature of the steel of the present invention. The purpose of selecting this temperature range for sub-temperature quenching is to obtain a structure with dispersed ferrite (volume fraction 7-12%) retained on the martensite substrate. There are three reasons: first, the sub-temperature quenching temperature is low, and the refined undissolved ferrite can prevent grain growth, and finer austenite grains can be formed along the original austenite grain boundaries before quenching; second, after tempering, the undissolved ferrite is evenly distributed on the tempered bainite, dividing the tempered bainite matrix, making it difficult for cracks to expand at the junction of ferrite and tempered bainite. At the same time, during the crack expansion process, ferrite will also hinder the initiation and expansion of cracks through its own plastic deformation, which is conducive to improving the corrosion fatigue resistance of steel; third, the presence of undissolved ferrite can enrich the impurity elements that cause temper brittleness, reduce the chance of its segregation on the austenite grain boundary, and play a role in purifying the grain boundary. At the same time, due to the refinement of grains and the increase in grain boundaries, the content of harmful impurity elements per unit interface is reduced, which is beneficial to increase strength and toughness, reduce notch sensitivity and reduce brittleness.

[0044] (8) Induction high temperature tempering process: Electromagnetic induction heating is used to perform high temperature tempering on the steel plate after sub-temperature quenching. The purpose is to increase the heating rate of the tempering process so that the matrix retains a higher density of dislocations, which is conducive to reducing the nucleation work required for the formation of carbonitrides inside the supercooled structure after quenching. At the same time, the alloy elements diffuse rapidly in the channel, prompting the carbonitrides to disperse and precipitate in large quantities at the dislocations inside the lath. The steel plate is rapidly heated to 600-630℃ at an induction heating rate of 5-10℃ / s, kept at this temperature for 10-30min, and then air-cooled to room temperature. The reason for choosing high temperature tempering is that increasing the tempering temperature helps to shorten the nucleation time of tempered carbonitrides, and reducing the holding time can effectively prevent the coarsening and growth of tempered carbonitrides inside the lath, the original austenite grain boundary and the martensite lath boundary. After induction tempering, the carbonitride morphology is short rod-shaped with a long axis size of less than 60nm. The reason why induction tempering is used to control the size of carbonitrides is that the carbonitrides precipitated by tempering are prone to form incoherent interfaces with the matrix, and the vicinity of such interfaces will preferentially become crack sources during the service and loading process of the steel plate. Reducing the interface size of carbonitrides, that is, reducing the size of the incoherent interface to reduce the root cause of crack initiation, helps to improve the plasticity, toughness and fatigue resistance of high-strength grade steel plates.

[0045] The beneficial effects of the present invention are:

[0046] (1) The present invention improves the purity of steel by controlling the sulfur and phosphorus content in pure steel smelting, and improves the steel quality by treating spheroidized inclusions with Ca. The chemical composition of the steel plate is reasonably designed, and a low C and low Mn design is adopted, and Cr, Cu, Ni, and Mo corrosion-resistant characteristic elements are added in combination with VN microalloying to improve the seawater corrosion fatigue resistance of the steel, wherein Cr, Cu, Ni, and Mo improve the corrosion resistance of the steel, and Si and VN microalloying improve the fatigue resistance of the steel. Through the synergistic effect of each element, the initiation and expansion of steel corrosion fatigue cracks are suppressed, so that the steel plate has excellent seawater corrosion fatigue resistance, elongation performance, and low-temperature impact performance.

[0047] (2) The innovative process of secondary heating rolling + DQ online quenching + induction high temperature tempering is adopted. The intermediate billet is heated again after the first quenching. The non-steady-state structure with high energy storage provides energy release and a large number of nucleation positions during the re-austenitization process of the secondary heating, which refines the austenite grain size of the intermediate billet and is conducive to the good organization and composition uniformity of the second stage rolled steel plate. The sub-temperature quenching is adopted to obtain the organization with dispersed ferrite on the martensite substrate, which improves the plasticity, toughness and fatigue resistance of the steel plate. The steel plate after sub-temperature quenching is tempered at high temperature by electromagnetic induction heating. The high heating rate during the tempering process makes the matrix retain a high density of dislocations, which is conducive to reducing the nucleation work required for the formation of the second phase inside the supercooled organization after quenching. At the same time, the alloy elements diffuse rapidly in the channel, which promotes the large-scale dispersion and precipitation of carbonitrides in the dislocations inside the lath, the original austenite grain boundaries and the boundaries of the martensite lath. This process route is conducive to improving the comprehensive performance of the product, achieving the matching of strength, plasticity and toughness, and can provide a guarantee for the safety of the steel plate in long-term service in marine engineering.

[0048] (3) The steel plate structure prepared by the present invention is tempered martensite + ferrite, and the microstructure characteristics are: the average equivalent diameter of the original austenite grains is ≤15μm; the average length of the martensite lath is <15μm; the volume fraction of undissolved ferrite is 7-12%; the tempered carbonitride morphology is short rod-shaped, and the average major axis size is <60nm.

[0049] (4) The steel plate prepared by the present invention has seawater corrosion fatigue resistance (corrosion fatigue life is more than 2.5 times that of conventional steel plates), ultra-high strength (yield strength ≥690MPa, tensile strength 770-940MPa), high ductility (tensile elongation after fracture ≥26%) and low-temperature impact toughness (-40℃ impact energy ≥150J), good fracture toughness (NDTT temperature ≤-50℃), and the product thickness ranges from 20 to 50mm. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] Figure 1 This is a metallographic microstructure diagram of Example 1 of the present invention.

[0051] Figure 2This is the SEM morphology of the impact fracture of Example 1 of the present invention. DETAILED DESCRIPTION

[0052] The present invention will be further described below by way of examples.

[0053] The embodiment of the present invention performs smelting, continuous casting, heating, primary heating, primary rolling, primary quenching, secondary heating, secondary rolling, secondary quenching, and tempering according to the component ratio of the technical solution.

[0054] Primary heating: billet heating temperature 1180~1250℃,

[0055] One-pass rolling: The rolling temperature is 1080-1150℃, and the ingot is rolled to 1.5-2.0 times the thickness of the finished product; the first pass reduction is ≥50mm, and the average single pass reduction rate is above 15%;

[0056] Primary quenching: After the primary rolling, the intermediate billet is subjected to DQ online quenching, and the intermediate billet is rapidly cooled to below 120°C at an average cooling rate of 15-20°C / s and then air-cooled to room temperature;

[0057] Secondary heating: heating to 900-950℃ at a heating rate of 15-20℃ / min; the average equivalent diameter of the original austenite grains is ≤15μm,

[0058] Secondary rolling: the secondary rolling temperature is 830-850℃, the average single-pass reduction rate reaches 15-20%, and the final rolling temperature is 800-820℃;

[0059] Secondary quenching: The steel plate enters the DQ online quenching system immediately at 770-790℃, and completes the sub-temperature quenching at an average cooling rate of 15-20℃ / s. The final cooling temperature of the steel plate is less than 120℃, and then air-cooled to room temperature to form a martensite + undissolved ferrite structure.

[0060] Tempering: The induction high temperature tempering process is adopted to perform high temperature tempering on the steel plate after sub-temperature quenching by electromagnetic induction heating. The steel plate is rapidly heated to 600-630℃ at an induction heating rate of 5-10℃ / s, kept at this temperature for 10-30min, and then air-cooled to room temperature.

[0061] Further; the smelting process:

[0062] a) During converter smelting, the contents of elements such as C, Si, Mn, P, and S are adjusted to be within the scope of the present invention, and other alloy components are added as required for smelting.

[0063] b) refining the molten steel and adjusting the contents of other alloy elements within the scope of the present invention.

[0064] c) subjecting the refined molten steel to RH treatment for a period of ≥30 min, and blowing nitrogen throughout the RH treatment to ensure that the final N content of the steel is within the range of the present invention, and controlling [H]≤2.0ppm and [O]≤18ppm in the steel.

[0065] Furthermore, the continuous casting is to control the superheat of the tundish to ≤30°C; the pouring is protected throughout the whole process, and electromagnetic stirring and light pressure are put into use, and the electromagnetic stirring: I≥450A.

[0066] Furthermore, the primary heating adopts a segmented heating process, when the billet temperature is below 900°C, slow heating is adopted with a heating rate of 8 to 12°C / min; when the billet temperature is greater than 900°C, a rapid heating process is adopted with a heating rate of 15 to 20°C / min and a holding time of 2.0 to 3.5h.

[0067] Furthermore, after the first quenching is completed, the microstructure of the intermediate billet is a martensitic structure.

[0068] The composition of the steel of the present invention and the comparative steel is shown in Table 1. The main process parameters of smelting and heating of the steel of the present invention are shown in Table 2. The main process parameters of rolling and quenching and tempering of the steel of the present invention are shown in Table 3. The microstructure of the steel of the present invention is shown in Table 4. The properties and NDTT temperature of the steel of the present invention are shown in Table 5. The corrosion fatigue properties of the steel of the present invention and the comparative steel are shown in Table 6.

[0069] Table 1 Composition (wt%) of the steel of the present invention and the comparative example

[0070]

[0071] Note: P: ≤0.01%, S: ≤0.001%

[0072] Table 2 Main process parameters for steel smelting and heating in the embodiment of the present invention

[0073]

[0074] Table 3 Main process parameters of rolling and tempering of steel in the embodiment of the present invention

[0075]

[0076]

[0077] Table 4 Microstructure of steel according to the present invention

[0078]

[0079] Table 5 Properties and NDTT temperature of steel in the examples of the present invention

[0080]

[0081] Table 6 Corrosion fatigue properties of the steels of the embodiments of the present invention and the comparative examples

[0082]

[0083]

[0084] Note: The anti-seawater corrosion fatigue performance test refers to ISO 11782-Ⅰ-2017 "Corrosion of Metals and Alloys - Corrosion Fatigue Test Part 1 Cyclic Failure Test", and the axial stress control method is used to determine the corrosion fatigue life curve. Stress ratio -1, peak stress 450MPa, loading frequency 1HZ. The corrosion fatigue corrosion solution is configured according to ASTM D1141-98 standard to simulate seawater, the pH value is adjusted with a dilute NaOH solution, and a 40mm thick EH690 steel plate is introduced as a comparative example. The corrosion fatigue performance of the embodiments of the present invention and the comparative example is tested to evaluate the anti-seawater corrosion fatigue performance of the steel plate.

[0085] 4. The marine steel plate produced by the present invention has a yield strength of ≥690MPa, a tensile strength of 770-940MPa, a tensile elongation of ≥26%, a -40°C KV2 impact energy of ≥150J, a NDTT temperature of ≤-50°C, a steel plate thickness of 20-50mm, and a stress ratio of -1, a peak stress of 450MPa, and a corrosion solution configured according to ASTM D1141-98 standard to simulate the corrosion fatigue conditions of seawater, the corrosion fatigue life of the steel plate is 63000-68000N.

[0086] In order to describe the present invention, the present invention is appropriately and fully illustrated by the examples in the above. The above implementation modes are only used to illustrate the present invention, but not to limit the present invention. Ordinary technicians in the relevant technical field can make various changes and modifications without departing from the spirit and scope of the present invention. Any modifications, equivalent substitutions, improvements, etc. made should be included in the protection scope of the present invention. The patent protection scope of the present invention should be defined by the claims.

Claims

1. An ultra-high strength marine engineering steel with high ductility and resistance to seawater corrosion fatigue, characterized in that: The composition of the marine engineering steel is as follows by weight percentage: C: 0.04%~0.06%, Si: 0.15%~0.25%, Mn: 1.00%~1.20%, Cr: 2.50%~3.50%, Ni: 0.90%~1.30%, Cu: 0.80%~1.20%, Mo: 0.40%~0.60%, V: 0.045%~0.065%, N: 0.017%~0.025%, Ca: 0.002%~0.005%, P: ≤0.01%, S: ≤0.001%, Als: 0.02%~0.05%, and the rest is Fe and unavoidable impurities; The method for manufacturing the ultra-high strength marine engineering steel with high ductility and seawater corrosion fatigue resistance comprises smelting, continuous casting, heating, primary heating, primary rolling, primary quenching, secondary heating, secondary rolling, secondary quenching, and tempering; Primary heating: billet heating temperature 1180~1250℃, holding time 2.0~3.5h; One-pass rolling: The rolling temperature is 1080~1150℃, and the ingot is rolled to 1.5~2.0 times the thickness of the finished product; the first pass reduction is ≥50mm, and the average single pass reduction rate is above 15%; One-time quenching: After one rolling, the intermediate billet is quenched online, and the intermediate billet is rapidly cooled to below 120 °C at an average cooling rate of 15-20 °C / s and then air-cooled to room temperature; Secondary heating: heating to 900~950℃ at a heating rate of 15~20℃ / min; the average equivalent diameter of the original austenite grains is ≤15μm, Secondary rolling: The secondary rolling temperature is 830~850℃, the average single-pass reduction rate reaches 15%~20%, and the final rolling temperature is 800~820℃; Secondary quenching: The steel plate is immediately quenched at 770~790 ℃, and the sub-temperature quenching is completed at an average cooling rate of 15~20 ℃ / s. The final cooling temperature of the steel plate is less than 120 ℃; Tempering: The induction high temperature tempering process is adopted to perform high temperature tempering on the steel plate after sub-temperature quenching by electromagnetic induction heating. The steel plate is rapidly heated to 600~630℃ at an induction heating rate of 5~10℃ / s, kept at this temperature for 10~30 min, and then air-cooled to room temperature.

2. The ultra-high strength marine engineering steel with high ductility and seawater corrosion fatigue resistance according to claim 1, characterized in that: The microstructure of the marine engineering steel plate is tempered martensite + ferrite, the average length of the tempered martensite lath is less than 15 μm; the volume fraction of ferrite is 7% to 12%; the morphology of the tempered carbonitride is short rod-shaped, and the average major axis size is less than 60 nm.

3. The ultra-high strength marine engineering steel with high ductility and seawater corrosion fatigue resistance according to claim 2, characterized in that: The tempered carbonitride is V(C,N).

4. The ultra-high strength marine engineering steel with high ductility and seawater corrosion fatigue resistance according to claim 1, characterized in that: The yield strength of the offshore steel plate is ≥690 MPa, the tensile strength is 770~940 MPa, the tensile elongation after break is ≥26%, the -40°C KV2 impact energy is ≥150 J, the NDTT temperature is ≤-50°C, and the steel plate thickness is 20~50 mm.

5. The ultra-high strength marine engineering steel with high ductility and seawater corrosion fatigue resistance according to claim 1, characterized in that: The continuous casting is to control the superheat of the tundish to be ≤30°C; protect the pouring throughout the whole process, and put into electromagnetic stirring and light pressure, and the electromagnetic stirring: I≥450A.

6. The ultra-high strength marine engineering steel with high ductility and seawater corrosion fatigue resistance according to claim 1, characterized in that: The primary heating adopts a segmented heating process. When the billet temperature is below 900°C, slow heating is adopted with a heating rate of 8-12°C / min. When the billet temperature is greater than 900°C, a rapid heating process is adopted with a heating rate of 15-20°C / min.

7. The ultra-high strength marine engineering steel with high ductility and seawater corrosion fatigue resistance according to claim 1, characterized in that: After the first quenching is completed, the microstructure of the intermediate billet is a martensite structure.