A composite material propeller blade and its preparation method

By employing a mechanical 'interlocking' structure and continuous carbon fiber prepreg layup in the composite propeller blades, the problem of insufficient connection strength at the mold closing position was solved, achieving high strength and tear resistance.

CN117698992BActive Publication Date: 2026-11-10HUNAN BOOM NEW MATERIALS
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311473531.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-07
Publication Date
2026-11-10
Estimated Expiration
2043-11-07

AI Technical Summary

Technical Problem

The existing composite propeller blades have insufficient connection strength at the mold closing position, making them prone to cracking under aerodynamic loads.

Method used

The composite blades and metal blade roots form a mechanical 'interlocking' structure, and the main load-bearing beam and skin layer are formed by interleaved layers of carbon fiber prepreg, combined with lightweight core material to improve interlayer connectivity and tear resistance.

Benefits of technology

It improves the connection strength and tear resistance of propeller blades while maintaining lightweight properties, meeting performance requirements under extreme operating conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117698992B_ABST
    Figure CN117698992B_ABST
Patent Text Reader

Abstract

This invention discloses a composite material propeller blade and its manufacturing method. The blade comprises a metal root and an embedded composite material blade. Along the blade's cross-section are a D-shaped main load-bearing beam, a lightweight core material, and a carbon fiber filler. The outer surface of the blade is fully covered with a skin. The metal root includes an inner root sleeve and an outer root sleeve, which are connected to the outer root sleeve by bolts and / or adhesive. An inverted wedge structure is provided between the inner and outer root sleeves. The composite layer formed by the D-shaped main load-bearing beam and the skin extends and fills the double inverted wedge structure. The root of the blade forms a mechanical interlocking structure with the blade root, effectively dispersing the influence of lateral tensile force on the blade skin material. The manufacturing method provided by this invention uses a prepreg layer-by-layer staggered layup to form an integrated structure, effectively improving the load-bearing beam's withstand threshold for centrifugal force and aerodynamic bending moment during rotation, effectively meeting the propeller's performance requirements for the main load-bearing beam under extreme operating conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a propeller blade, specifically a composite material propeller blade and its preparation method, belonging to the field of aircraft propeller manufacturing technology. Background Technology

[0002] Composite materials are lightweight and high-strength. Using composite materials to manufacture propeller blades can effectively reduce the propeller's weight, improve the aircraft's range and payload capacity, and also reduce vibration and noise. They are considered the best materials for manufacturing propeller blades.

[0003] Currently, most composite propeller blades are formed using a compression molding process. This process involves laying prepreg in upper and lower molds to form composite structural layers, with a lightweight core material encased within these layers. After the molds are closed, the blades are pressed together using a hot press. Because the molds are closed at the leading and trailing edges of the blade, the composite structural layers at these points are discontinuous, relying solely on resin bonding for adhesion. This weak connection makes the leading edge of the blade prone to cracking under aerodynamic loads. Summary of the Invention

[0004] To address the problems existing in the prior art, the first objective of this invention is to provide a composite material propeller blade, which includes a composite material blade and a metal root. The root of the composite material blade is entirely embedded in the double inverted wedge cavity of the metal root, forming a mechanical "interlocking" structure with the metal root, which can effectively improve the connection strength between the blade and the root.

[0005] The second objective of this invention is to provide a method for preparing composite material propeller blades. In this method, the propeller blades are manufactured using a carbon fiber prepreg layup hot-pressing process. The composite material structural layers of the blade include a main load-bearing beam and a skin layer. The main load-bearing beam is a continuous unidirectional carbon fiber strip laminated into an integral structure, filled with a lightweight core material. The skin is a laminated carbon fiber fabric that fully encloses the load-bearing beam. The lightweight core material layer, load-bearing beam, and skin shell are combined using a layer-by-layer layup structure, resulting in good overall integrity and high reliability. Furthermore, without increasing the blade weight, by increasing the width of the lower skin and decreasing the width of the upper skin, and by folding the lower skin and staggering its overlap with the upper skin, the interlayer connectivity of the blade's leading edge can be effectively improved. Simultaneously, because the overlap position is staggered from the mold closing position, the tear resistance of the blade's leading edge is improved.

[0006] To achieve the above technical objectives, the present invention provides a composite material propeller blade. The composite material propeller blade consists of a D-shaped main load-bearing beam, a lightweight core material, and a carbon fiber filler along its cross-section. The outer surface of the propeller blade is fully covered with a skin. The D-shaped main load-bearing beam has a hollow structure filled with the lightweight core material. The metal propeller root includes an inner propeller root sleeve and an outer propeller root sleeve, which are connected to the outer propeller root sleeve by bolts and / or adhesives. A double inverted wedge structure is provided between the inner propeller root sleeve and the outer propeller root sleeve. The composite layer formed by the D-shaped main load-bearing beam and the skin extends and fills the double inverted wedge structure.

[0007] As a preferred embodiment, the inner sleeve of the propeller root has a cylindrical groove that is inserted into the lightweight core material inside the D-shaped main load-bearing beam of the propeller blade.

[0008] This invention also provides a method for preparing composite material propeller blades, comprising:

[0009] 1) Clean the upper and lower forming molds and cut the raw materials, including carbon fiber unidirectional tape, carbon fiber fabric and epoxy film;

[0010] 2) Lay the skin layer and the main load-bearing beam layer layer by layer in the upper and lower molds respectively. After every 3 to 10 layers, vacuum bag pressing is performed once to obtain the upper and lower mold parts;

[0011] 3) Insert the lightweight core material into the groove of the inner sleeve of the metal propeller root, place it on the lower mold, and fix it by vacuuming;

[0012] 4) After the upper and lower mold parts are joined together, they are placed on a hot press to solidify and form the final product.

[0013] As a preferred embodiment, the main load-bearing beam layer comprises a carbon fiber layer and a flame-retardant epoxy resin; the main load-bearing beam layer contains ≥30 carbon fiber layers.

[0014] As a preferred option, the main load-bearing beam layer uses T800 continuous carbon fiber.

[0015] As a preferred embodiment, the skin comprises carbon fiber fabric and flame-retardant epoxy resin.

[0016] As a preferred option, the skin is made of T300 carbon fiber fabric.

[0017] As a preferred embodiment, the vacuum bag pressing conditions are: temperature 10–60°C, vacuum degree 0.1–1 MPa, and time 10–20 min. More preferably, the vacuum bag pressing conditions are: 20±2°C, vacuum degree greater than 0.95 MPa, and time 10–20 min.

[0018] As a preferred embodiment, the vacuum fixing conditions for the lightweight core material are: temperature 10–60℃, vacuum degree 0.1–1 MPa, and time 20–60 min. More preferably, the vacuum fixing conditions for the lightweight core material are: 20±2℃, vacuum degree greater than 0.95 MPa, and time 30 min.

[0019] As a preferred embodiment, the lightweight core material is a high-strength, low-density foam material.

[0020] As a preferred embodiment, the high-strength, low-density foam material has a compressive strength ≥ 2 MPa and a density ≤ 0.75 kg / m³. 3 .

[0021] As a preferred embodiment, the skin layer area of ​​the lower mold part is larger than that of the upper mold part. When the upper and lower mold parts are closed, the skin layer of the lower mold part is folded over sequentially to the corresponding position of the skin layer of the upper mold part for connection. The folding method of the skin layer of the lower mold part and the skin layer of the upper mold part is to overlap layer by layer in a staggered manner, which aims to improve the integration of the joint.

[0022] As a preferred embodiment, the docking condition is as follows: for every 3 to 10 folds of the skin layer of the lower mold part and the skin layer of the upper mold part, a vacuum bag is applied once. More preferably, the docking condition is as follows: for every 1 to 2 folds of the skin layer of the lower mold part and the skin layer of the upper mold part, a vacuum bag is applied once.

[0023] The vacuum bag pressing conditions are: temperature 10–60℃, vacuum degree 0.1–1 MPa, and time 10–20 min. More preferably, the vacuum bag pressing conditions are: 20±2℃, vacuum degree greater than 0.95 MPa, and time 10–20 min.

[0024] As a preferred embodiment, the curing conditions are: temperature of 90–150°C, pressure of 3–6 MPa, and time of 1–4 hours.

[0025] The composite propeller blades provided by this invention are primarily laid up in the lower mold, specifically the lower skin shell, load-bearing beam, and part of the upper skin, as well as the placement of the lightweight core material. During layup, the width dimension of the lower skin prepreg is appropriately enlarged, while the corresponding dimensions of the upper skin prepreg are reduced by the same amount. This is to allow the excess lower skin prepreg to be folded over and aligned with the corresponding layup position of the upper skin when the upper skin is laid up, improving the interlayer connectivity at the blade edges and enhancing the stiffness and strength of the composite propeller blades without adding extra weight. The main load-bearing beam of the composite propeller provided by this invention uses a continuous carbon fiber prepreg layered staggered layup as an integral structure, effectively improving the structural stiffness of the blades. Furthermore, this invention employs a dual-force transmission path design at the junction of the composite blades and the metal root, combining adhesive bonding and mechanical interlocking, avoiding the complex strength design and verification work required for a single-force transmission path. This interlocking structure also boasts high reliability, with a failure probability that is "extremely unlikely."

[0026] Compared with the prior art, the beneficial technical effects of the present invention are as follows:

[0027] 1) The propeller blade root provided by this invention is entirely embedded in the double-wedge cavity of the metal blade root, forming a mechanical "interlocking" structure with the metal blade root, which can effectively improve the connection strength between the blade and the blade root. In addition, without increasing the weight of the blade, the width of the lower skin is increased and the width of the upper skin is reduced. The lower skin is folded over and overlapped with the upper skin in a staggered manner, which can effectively improve the interlayer connectivity of the blade leading edge. At the same time, because the overlap position is staggered from the mold closing position, the tear resistance of the blade leading edge is improved.

[0028] 2) In the preparation method provided by the present invention, the main load-bearing beam of the propeller adopts a continuous carbon fiber prepreg layer by layer as an integral structure, which can not only improve the overall consistency of the main load-bearing beam of the composite propeller and improve the load-bearing beam's threshold for centrifugal force and aerodynamic bending moment when the blade rotates, but also avoid the occurrence of layer gaps, effectively meeting the performance requirements of the propeller for the main load-bearing beam under extreme working conditions. Attached Figure Description

[0029] Figure 1 A cross-sectional schematic diagram of the blade provided by the present invention;

[0030] Among them, 1-main load-bearing beam, 2-skin, 3-lightweight core material, 4-carbon fiber filler;

[0031] Figure 2 A cross-sectional view of the paddle root provided by the present invention;

[0032] Among them, 1-propeller root outer sleeve, 2-sealing ring, 3-counterweight tube plug, 4-counterweight tube, 5-drive pin, 6-propeller root inner sleeve, 7-foaming adhesive;

[0033] Figure 3 This is a cross-sectional view of the paddle root provided in Comparative Example 2 of the present invention. Detailed Implementation

[0034] The specific implementation schemes of the present invention will be described in detail and clearly below with reference to the embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.

[0035] Example 1

[0036] In this embodiment, the propeller root outer sleeve and inner sleeve are made of 2A11 aluminum alloy. The blade skin is made of 3kT300 carbon fiber fabric, the D-shaped load-bearing beam is made of 12kT800 carbon fiber unidirectional tape, and the lightweight core material is PMI foam. The composite blade consists of a lightweight core material, a D-shaped load-bearing beam, and a skin along its cross-section from the inside out. The D-shaped load-bearing beam is a hollow integral structure filled with lightweight core material and wrapped with skin. The metal root includes an inner sleeve and an outer sleeve, which are connected to the outer sleeve by screws and / or adhesive. A double inverted wedge structure is provided between the inner sleeve and the outer sleeve. The composite material layer formed by the main load-bearing beam and the skin extends and is embedded in the cavity of the inverted wedge structure. The manufacturing process of this blade is as follows:

[0037] 1) Clean the molding die and cut the carbon fiber unidirectional tape, carbon fiber fabric, and epoxy film;

[0038] 2) Lay carbon fiber fabric, carbon fiber unidirectional tape, and epoxy film layer by layer in the lower mold to form the lower skin layer and the main load-bearing beam layer; the layup method is to vacuum bag press once for every 3 layers, and the vacuum bag pressing time is 15 minutes each time.

[0039] 3) Insert the lightweight core material into the groove of the inner sleeve of the metal paddle root at the designed angle, place it on the lower main load-bearing beam layer, and fix it by vacuuming for 20 minutes.

[0040] 4) Lay the upper main load-bearing beam layer and part of the skin layer, fold the excess part of the lower skin layer layer by layer, and overlap it with the upper skin layer in a staggered manner. After every 2 layers, vacuum bag press once, and the vacuum bag pressing time is 10 minutes each time.

[0041] 5) Lay the remaining skin layers one by one on the upper mold.

[0042] 5) Close the upper and lower molds and place them on a hot press to cure and form according to the curing process conditions. The curing process parameters are: temperature 100±5℃, pressure 6MPa, and time 1h.

[0043] The composite propeller blade provided in this embodiment has 27 layers of continuous carbon fiber prepreg in both the upper and lower sections of the main load-bearing beam, and 5 layers of carbon fiber fabric in both the upper and lower sections of the skin layer. The vacuum bag pressure temperature is 20±2℃, and the vacuum degree is greater than 0.95MPa. The layup is mainly completed in the lower mold. During layup, the lower skin prepreg is enlarged by 19.5mm in width along the layup direction at the leading edge, while the upper skin prepreg is reduced by 18.5mm at the corresponding position. The purpose is to allow the excess part of the lower skin prepreg to be folded over and aligned with the corresponding layup position of the upper skin when laying the upper skin, thereby improving the interlayer connectivity at the blade edge, increasing the stiffness and strength of the composite propeller blade, and without adding extra weight to the blade.

[0044] Example 2

[0045] The preparation process of this embodiment is exactly the same as that of Embodiment 1. The difference is that the width of the lower skin prepreg is increased by 21 mm in the leading edge lay-up direction, and the size of the upper skin prepreg at the corresponding position is reduced by 19 mm.

[0046] Example 3

[0047] The preparation process of this embodiment is exactly the same as that of Embodiment 1. The difference is that the lower skin prepreg is enlarged by 25 mm in width along the leading edge layup direction, and the upper skin prepreg at the corresponding position is reduced by 23 mm.

[0048] Comparative Example 1

[0049] The preparation process of this comparative example is exactly the same as that of Example 1, except that the dimensions of the lower skin and the upper skin are not proportionally enlarged and reduced, and are consistent.

[0050] Comparative Example 2

[0051] The preparation process of this comparative example is the same as that of Example 1, except for the structural differences, specifically: Figure 3 As shown, the metal propeller root is an integral structure, with a composite material layer wrapped around its surface.

[0052] Strength analysis was performed on Example 1, Comparative Example 1, and Comparative Example 2 after 125% overclocking. The maximum operating speed of the propeller was designed to be 2000 rpm. The blades were tested at 2500 rpm. The composite material was judged according to the maximum strain criterion. The results are shown in Tables 1 to 3. All metal materials used were 2A11 material with a yield strength of 321 MPa.

[0053] Table 1. Stress and strength verification of the composite material obtained in Example 1 under 125% blade overspin condition.

[0054]

[0055] Table 2 shows the stress and strength verification of the composite material under the 125% overspeed condition obtained in Comparative Example 1.

[0056]

[0057] Table 3 shows the stress and strength verification of the composite material under the 125% blade overspeed condition obtained in Comparative Example 2.

[0058]

[0059] As shown in Tables 1-3, the maximum tensile principal strain, maximum compressive principal strain, and maximum shear principal strain of the blade provided in Example 1 of this invention are all less than the fracture limit strain of T300 and T800 grade composite materials, and the safety factor is greater than 1, so the propeller does not fail even when over-rotating. However, the strain of the blade obtained in Comparative Example 2 is significantly increased compared to that in Example 1, but its safety factor is still greater than 1. This is because the lower skin layer and the upper skin layer are directly connected, resulting in no folding reinforcement. The skin edge has a poor force transmission effect. However, thanks to the double inverted wedge structure of the blade and the root, the propeller as a whole is still within the safe range. In Comparative Example 2, the safety factor is obviously less than 1 during the tensile process. This is because the skin material is wrapped around the surface of the root, making it difficult to quickly transmit centrifugal force during rotation. Moreover, once the end of the skin layer wrapped around the root lifts up, it is not only affected by centrifugal force but also by air resistance, further aggravating its fracture risk. Therefore, only with the combined effect of structure and method can the excellent technical effect of the blade be achieved.

Claims

1. A composite material propeller blade, characterized in that: The blade comprises a metal blade root and an embedded composite material blade. The composite material blade, along its cross-section, consists of a D-shaped main load-bearing beam, a lightweight core material, and a carbon fiber filler, with the outer surface of the blade covered by a fully enclosed skin. The D-shaped main load-bearing beam has a hollow internal structure filled with the lightweight core material. The metal blade root includes an inner blade root sleeve and an outer blade root sleeve, which are connected to the outer blade root sleeve by bolts and / or adhesive. A double inverted wedge structure is provided between the inner blade root sleeve and the outer blade root sleeve. The composite layer formed by the D-shaped main load-bearing beam and the skin extends and fills the double inverted wedge structure. The propeller blades are prepared as follows: 1) Clean the upper and lower forming molds and cut the raw materials including carbon fiber unidirectional belt, carbon fiber fabric and epoxy film; 2) Lay the skin layer and the main load-bearing beam layer layer by layer in the upper and lower molds respectively. After every 3 to 10 layers, vacuum bag pressing is performed once to obtain the upper and lower mold parts; 3) Insert the lightweight core material into the groove of the inner sleeve of the metal propeller root, place it on the lower mold, and fix it under vacuum; 4) After the upper and lower mold parts are joined together, they are placed on a hot press to solidify and form the final product; The skin layer area of ​​the lower mold part is larger than that of the upper mold part. When the upper and lower mold parts are closed, the skin layer of the lower mold part is folded over to the corresponding position of the skin layer of the upper mold part for docking.

2. The composite material propeller blade according to claim 1, characterized in that: The inner sleeve of the propeller root has a groove that is inserted into the lightweight core material inside the D-shaped main load-bearing beam of the propeller blade.

3. The composite material propeller blade according to claim 1, characterized in that: The main load-bearing beam layer includes a carbon fiber layer and flame-retardant epoxy resin; the main load-bearing beam layer has ≥30 carbon fiber layers; the carbon fiber used in the main load-bearing beam layer is T800 continuous carbon fiber.

4. The composite material propeller blade according to claim 1, characterized in that: The skin comprises carbon fiber fabric and flame-retardant epoxy resin; the carbon fiber fabric used in the skin is T300 carbon fiber fabric.

5. A composite material propeller blade according to claim 1, characterized in that: The vacuum bag pressing conditions are: temperature 10~60℃, vacuum degree 0.1~1MPa, and time 10~20min; the vacuum fixing conditions for the lightweight core material are: temperature 10~60℃, vacuum degree 0.1~1MPa, and time 20~60min.

6. A composite material propeller blade according to claim 1, characterized in that: The lightweight core material is a high-strength, low-density foam material; the high-strength, low-density foam material has a compressive strength ≥3MPa and a density ≤0.75kg / m³. 3 .

7. A composite material propeller blade according to claim 1, characterized in that: The docking conditions are as follows: the skin layer of the lower mold and the skin layer of the upper mold are folded 3 to 10 times, and vacuum bag pressing is performed once; the vacuum bag pressing conditions are: temperature 10 to 60°C, vacuum degree 0.1 to 1 MPa, and time 10 to 20 minutes.

8. A composite material propeller blade according to claim 1, characterized in that: The curing conditions are: temperature 90~150℃, pressure 3~6MPa, and time 1~4h.

Citation Information

Patent Citations

  • Composite propeller blade of propeller

    CN112429201A

  • Paddle forming process method and paddle root structure for improving paddle forming quality

    CN115431557A