Silicon carbide MOSFET device and self-aligned manufacturing method thereof
By adopting two self-alignment processes and the use of a T-type dielectric layer in the SiC MOSFET device, the precise alignment of the JFET area is achieved, the problem of increased resistance in the JFET area is solved, and the conduction characteristics and process of the device are improved. accuracy.
Patent Information
- Application Number
- CN202311741411.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-18
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-12-18
AI Technical Summary
The JFET area resistance of SiC MOSFET devices accounts for an increasing proportion of the total resistance. The existing technology can easily cause unnecessary injection damage and photolithography accuracy problems when reducing the JFET area resistance, and it is difficult to effectively reduce the on-resistance of the device.
Two self-alignment processes are used to achieve self-alignment of the second conductivity type well region and the first conductivity type source region, and the second conductivity type well region and the first conductivity type first injection region, respectively, through the T-type dielectric layer Precise alignment of conductive type ranges reduces photolithography registration errors and avoids injection damage, thereby reducing JFET resistance.
The JFET resistance is significantly reduced, the forward conduction characteristics of the device are improved, unnecessary ion implantation damage and photolithography errors are avoided, and the process accuracy and device performance are improved.
Smart Images

Figure CN117711946B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of semiconductor devices, and in particular relates to a silicon carbide MOSFET device and a self-alignment manufacturing method thereof. Background Art
[0002] Among SiC power devices, Metal Oxide Semiconductor Field Effect Transistor (MOSFET) has considerable application prospects in new energy vehicles, rail transportation, aerospace systems, military electronic communication systems and other fields due to its advantages such as simple gate drive and unipolar conduction mechanism.
[0003] The key parameters of SiC MOSFET devices include breakdown voltage, threshold voltage, on-resistance, etc. How to reduce the on-resistance of the device is a core issue for domestic and foreign research institutions and companies. The on-resistance of SiC MOSFET devices includes substrate resistance, drift region resistance, JFET region resistance, channel resistance, and ohmic contact resistance. As the cell size decreases, the width of the JFET region becomes smaller and smaller, and the resistance of this region accounts for an increasing proportion of the total resistance. At present, there are two main solutions in the industry to reduce the resistance of the JFET region. One is to dope the entire active area, but this will cause unnecessary injection damage; the other is to dope the JFET region, but due to the limitations of lithography accuracy, there are problems such as asymmetric injection and channel damage. Summary of the invention
[0004] In view of the above-mentioned deficiencies of SiC MOSFET devices, the present invention provides a silicon carbide MOSFET device and a self-aligned manufacturing method thereof.
[0005] A self-aligned manufacturing method for a silicon carbide MOSFET device comprises the following steps:
[0006] S1. forming a first conductivity type epitaxial layer on a first conductivity type substrate;
[0007] S2. forming a first mask layer and a barrier layer on the surface of the first conductivity type epitaxial layer;
[0008] S3. forming a second conductivity type well region in the first conductivity type epitaxial layer;
[0009] S4. forming sidewalls on the barrier layer and on both sides of the first mask layer;
[0010] S5. forming a first conductive type source region in the second conductive type well region; achieving self-alignment of the second conductive type well region and the first conductive type source region through the sidewalls;
[0011] S6. After removing the sidewalls, a thickened dielectric layer is formed on both sides and above the first mask layer;
[0012] S7. Etching the thickened dielectric layer to form a T-shaped dielectric layer;
[0013] S8. removing the first mask layer and retaining the T-type dielectric layer;
[0014] S9. forming a first conductivity type first injection region and a first conductivity type second injection region located between the first conductivity type first injection regions in the first conductivity type epitaxial layer through a T-type dielectric layer; achieving self-alignment of the second conductivity type well region and the first conductivity type first injection region through the T-type dielectric layer, and removing the T-type dielectric layer;
[0015] S10. forming a gate dielectric layer on the surface of the device, forming a gate electrode on the gate dielectric layer, and forming an isolation dielectric layer on both sides and on the gate electrode;
[0016] S11. Form a source ohmic contact on the surfaces of the first conductive type source region and the second conductive type well region, form a drain ohmic contact on the back side of the first conductive type substrate, form a source electrode on the surface of the source ohmic contact, and form a drain electrode on the surface of the drain ohmic contact.
[0017] Beneficial effects of the present invention:
[0018] The present invention realizes self-alignment of the second conductivity type well region with the first conductivity type source region, and the second conductivity type well region with the first conductivity type first injection region, respectively, through two self-alignment processes, thereby significantly reducing the photolithography registration error in the entire process flow, and effectively reducing the JFET resistance while avoiding unnecessary ion implantation damage or JFET region injection damage to the channel, thereby improving the forward conduction characteristics of the device. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a process flow chart of a self-aligned manufacturing method for a silicon carbide MOSFET device according to Example 1.
[0020] Figure 2~Figure 13 This is a specific flow chart of the self-alignment process for silicon carbide MOSFET devices described in Example 1.
[0021] Explanation of the accompanying drawings: 1. drain electrode; 2. first conductive type substrate; 3. first conductive type epitaxial layer; 4. second conductive type well region; 5. first conductive type source region; 6-1. first conductive type first injection region; 6-2. first conductive type second injection region; 7. gate dielectric layer; 8. gate electrode; 9. isolation dielectric layer; 10. source electrode; 100. first mask layer; 101. blocking layer; 102. side wall; 103. thickened dielectric layer; 104. T-type dielectric layer; 104-1. first component of T-type dielectric layer; 104-2. second component of T-type dielectric layer. DETAILED DESCRIPTION
[0022] The present invention is further described below in conjunction with examples. The examples are only used to illustrate the present invention and do not constitute a limitation on the scope of the claims. Other alternative means that can be thought of by those skilled in the art are all within the scope of the claims of the present invention.
[0023] In addition, in the description of the present invention, it should be noted that the terms "central", "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc., indicating the orientation or position relationship, are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the invention. In addition, the terms "first", "second", and "third" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance. Example 1
[0024] A self-aligned manufacturing method for a silicon carbide MOSFET device, the process flow chart is as follows Figure 1 As shown, the following will be combined Figure 2~Figure 13 The specific process steps are described. The manufacturing method comprises the following steps:
[0025] S1. Figure 2 , Figure 3 As shown, a first conductive type epitaxial layer 3 is formed on a first conductive type substrate 2 by epitaxial growth, the first conductive type substrate 2 is a first conductive type silicon carbide substrate, and the first conductive type epitaxial layer 3 is a first conductive type silicon carbide epitaxial layer; the first conductive type substrate 2 and the first conductive type epitaxial layer 3 are made of 3C-SiC, 4H-SiC, 6H-SiC or 15R-SiC, the first conductive type substrate 2 has a thickness ranging from 10µm to 1000µm, and a doping concentration of 1e18cm -3 ~5e19cm -3 The first conductive type silicon carbide epitaxial layer 3 has a thickness of 8µm~200µm and a doping concentration of 1e14cm -3~5e16cm -3 , preferably 1e14cm -3 ~1e16cm -3 ;
[0026] S2. Figure 4 As shown, a first mask layer material is grown on the surface of the first conductive type epitaxial layer 3 by an LPCVD process, and then a patterned first mask layer 100 is formed by photolithography and etching processes. The thickness of the first mask layer 100 is in the range of 1µm to 10µm, and the material of the first mask layer 100 is Si3N4; a barrier layer 101 is formed on the first conductive type epitaxial layer 3 and the first mask layer 100 by an LPCVD process, and the thickness of the barrier layer is 100Å to 1000Å, and the material of the barrier layer 101 is SiO2; wherein LPCVD is Low Pressure Chemical Vapor Deposition, i.e., low pressure chemical vapor deposition;
[0027] S3. Figure 5 As shown, through the ion implantation process, a second conductive type well region 4 is formed in the first conductive type epitaxial layer 3, the depth of the second conductive type well region 4 ranges from 0.5µm to 1.5µm, and the doping concentration is 5e16cm -3 ~5e17cm -3 ;
[0028] S4. Figure 6 As shown, a sidewall 102 is formed on the surface of the device obtained in S3 by an LPCVD process. The sidewall 102 is located on both sides of the protrusion of the barrier layer 101. The sidewall material is polysilicon. The thickness of the sidewall is in the range of 0.2µm to 1.0µm, and the width is in the range of 0.1µm to 1.0µm.
[0029] S5. Figure 7 As shown, by ion implantation, a first conductive type source region 5 is formed in the second conductive type well region 4. The depth of the first conductive type source region 5 is in the range of 0.1µm to 0.5µm, and the doping concentration is 1e19cm -3 ~2e20cm -3 The sidewall 102 is used to achieve self-alignment between the second conductivity type well region 4 and the first conductivity type source region 5;
[0030] S6. Figure 8 As shown, the sidewall 102 is dry-etched, and the etching gas can be one or more combinations of gases such as Cl2, HBr, and HeO2. After the sidewall 102 is etched away, a thickened dielectric layer 103 is formed on the device surface through the LPCVD process. The material of the thickened dielectric layer 103 is SiO2. The top of the thickened dielectric layer 103 can be flush or not flush according to the actual process conditions.
[0031] S7. Fig. 9 As shown, the thickened dielectric layer 103 is etched by photolithography and etching to form a T-shaped dielectric layer 104, and the material of the T-shaped dielectric layer 104 is SiO2. The T-shaped dielectric layer 104 is arranged on the top of the device, and the T-shaped dielectric layer 104 covers the top of the first conductive type source region 5, the top of the second conductive type well region 4, the sidewall of the first mask layer 100, and the top of part of the first mask layer 100. The width of the first mask layer 100 not covered by the T-shaped dielectric layer 104 ranges from 0.5µm to 3.0µm;
[0032] The T-type dielectric layer is composed of a first T-type dielectric layer component 104-1 and a second T-type dielectric layer component 104-2. The first T-type dielectric layer component 104-1 covers the top of the first mask layer 100, and the second T-type dielectric layer component 104-2 covers the sidewall of the first mask layer 100, the top of the first conductive type source region 5, and the top of the second conductive type well region 4.
[0033] The width of the first T-shaped dielectric layer component 104 - 1 is in the range of 0.1µm to 1.0µm, and the thickness is in the range of 0.1µm to 1.0µm. The width of the second T-shaped dielectric layer component 104 - 2 is in the range of 0.5µm to 10.0µm, and the thickness is in the range of 1.0µm to 5.0µm.
[0034] S8. Fig.10 As shown, the first mask layer 100 is removed by a wet etching process, and the T-shaped dielectric layer 104 is retained. Phosphoric acid reagent may be used for the wet etching.
[0035] S9. Fig.11 As shown, with the T-type dielectric layer 104 as a mask, an ion implantation process is performed to form a first conductive type first implantation region 6-1 and a first conductive type second implantation region 6-2 located between the first conductive type first implantation region 6-1 in the first conductive type epitaxial layer 3. The depth of the first conductive type first implantation region 6-1 is in the range of 0.1µm to 1.0µm, the width of the first conductive type first implantation region 6-1 is the same as the width of the first component 104-1 of the T-type dielectric layer, the depth of the first conductive type second implantation region 6-2 is in the range of 0.5µm to 4.0µm, and the width is in the range of 0.5µm to 3.0µm. The depth of the first conductive type first implantation region 6-1 is less than the depth of the first conductive type second implantation region 6-2, and the difference between the two is not less than 0.2µm. The concentration of the first conductive type second implantation region 6-2 is substantially the same as the doping concentration of the first conductive type first implantation region 6-1, which is 1e16cm -3 ~5e17cm -3 , the difference between the two does not exceed 1e16cm -3, then remove the T-type dielectric layer 104, and then activate and anneal the device at a temperature of 1400°C~2200°C for 2min~30min; in this step, the first conductivity type first injection region 6-1 is formed by using the T-type dielectric layer 104 as a mask to achieve self-alignment of the second conductivity type well region and the first conductivity type first injection region. As the second self-alignment process in the self-alignment method, the two self-alignment processes significantly reduce the lithography registration error in the entire process flow, while avoiding unnecessary ion implantation damage or JFET region injection damage to the channel, effectively reducing the JFET resistance, thereby improving the forward conduction characteristics of the device.
[0036] S10. Fig.12 As shown, a gate dielectric layer 7 is formed by an oxidation process or an LPCVD process or an ALD (Atomic Layer Deposition) process, and the gate dielectric layer 7 covers the top of the first conductive type second injection region 6-2, the top of the first conductive type first injection region 6-1, the top of the second conductive type well region 4 and the top of part of the first conductive type source region 5; the material of the gate dielectric layer 7 is selected from SiO2, Si3N4 or Al2O3. Then, the quality of the gate dielectric layer 7 is improved by a high-temperature annealing process, and the annealing gas can be one or more combinations of gases such as NO, N2O, H2, NH3, etc., and the annealing temperature is 900°C to 1300°C. A gate electrode 8 is formed by atomic layer deposition, chemical vapor deposition, plasma enhanced chemical vapor deposition or sputtering, and the gate electrode 8 is located on the gate dielectric layer 7; the gate electrode material can be polycrystalline silicon, amorphous silicon or amorphous silicon, and the doping impurities can be impurities such as Al, N, P, B, etc. Polysilicon is injected and the polysilicon surface is flattened by CMP process, and then activated annealing is performed, and a patterned isolation dielectric layer 9 is formed by LPCVD process, photolithography and etching process, and the isolation dielectric layer 9 wraps the top and side wall of the gate electrode 8; the material of the isolation dielectric layer can be silicon dioxide, or nitride, or a composite of silicon dioxide and nitride. The thickness of the isolation dielectric layer 9 ranges from 0.5µm to 5µm to form a source window;
[0037] S11. Fig.13 As shown, a metal is formed by evaporation, sputtering or electroplating of the source window, and a Ti / Al alloy is selected as the metal, and then annealed at 300°C to 1100°C to form a source ohmic contact. A drain ohmic contact is formed on the bottom layer of the first conductive type substrate 2, a source electrode 10 is formed on the surface of the source ohmic contact, and a drain electrode 1 is formed on the surface of the drain ohmic contact. The metal material can be one or more combinations of materials such as Al, Ti, Ag, Ni, Pt, and Cu.
[0038] This embodiment also provides a silicon carbide MOSFET device, which is obtained by the self-aligned manufacturing method of the silicon carbide MOSFET device described above, comprising:
[0039] Drain electrode 1;
[0040] A first conductive type substrate 2 located on the drain electrode 1;
[0041] A first conductivity type epitaxial layer 3 located on the first conductivity type substrate 2;
[0042] A second conductivity type well region 4 located in the first conductivity type epitaxial layer 3;
[0043] a first conductivity type source region 5 located in the second conductivity type well region 4;
[0044] a first conductivity type first implantation region 6 - 1 located in the first conductivity type epitaxial layer 3 and between the second conductivity type well regions 4 ;
[0045] a first conductivity type second injection region 6 - 2 located between the first conductivity type first injection regions 6 - 1;
[0046] a gate dielectric layer 7 located on the first conductivity type epitaxial layer 3;
[0047] a gate electrode 8 located on the gate dielectric layer 7;
[0048] An isolation dielectric layer 9 located on both sides and above the gate electrode 8;
[0049] A source electrode 10 is located on the surfaces of the first conductivity type source region 5 and the second conductivity type well region 4 .
[0050] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.
Claims
1. A self-aligned manufacturing method for a silicon carbide MOSFET device, characterized in that: The following steps are involved: S1. forming an epitaxial layer of a first conductivity type on a substrate of a first conductivity type; S2. forming a first mask layer and a barrier layer on the surface of the first conductivity type epitaxial layer; S3. forming a second conductivity type well region in the first conductivity type epitaxial layer; S4. forming sidewalls on the barrier layer and on both sides of the first mask layer; S5. forming a first conductive type source region in the second conductive type well region; achieving self-alignment of the second conductive type well region and the first conductive type source region through the sidewalls; S6. After removing the sidewalls, a thickened dielectric layer is formed on both sides and above the first mask layer; S7. Etching the thickened dielectric layer to form a T-shaped dielectric layer; the T-shaped dielectric layer comprises a first T-shaped dielectric layer component and a second T-shaped dielectric layer component, the first T-shaped dielectric layer component covers the top of the first mask layer, and the second T-shaped dielectric layer component covers the sidewall of the first mask layer, the top of the first conductive type source region, and the top of the second conductive type well region; the first T-shaped dielectric layer component has a width range of 0.1µm~1.0µm and a thickness range of 0.1µm~1.0µm, and the second T-shaped dielectric layer component has a width range of 0.5µm~10.0µm and a thickness range of 1.0µm~5.0µm; S8. removing the first mask layer and retaining the T-type dielectric layer; S9. forming a first conductivity type first injection region and a first conductivity type second injection region located between the first conductivity type first injection regions in the first conductivity type epitaxial layer through a T-type dielectric layer; achieving self-alignment of the second conductivity type well region and the first conductivity type first injection region through the T-type dielectric layer, and removing the T-type dielectric layer; the depth of the first conductivity type first injection region is less than the depth of the first conductivity type second injection region, and the difference between the two is not less than 0.2µm; S10. forming a gate dielectric layer on the surface of the device, forming a gate electrode on the gate dielectric layer, and forming an isolation dielectric layer on both sides and on the gate electrode; S11. Form a source ohmic contact on the surfaces of the first conductive type source region and the second conductive type well region, form a drain ohmic contact on the back side of the first conductive type substrate, form a source electrode on the surface of the source ohmic contact, and form a drain electrode on the surface of the drain ohmic contact.
2. A self-aligned manufacturing method for a silicon carbide MOSFET device according to claim 1, characterized in that: In step S7 and step S8, a patterned thickened dielectric layer is formed by photolithography and etching processes, and then the first mask layer is removed by a wet etching process to retain the patterned thickened dielectric layer to form a T-shaped dielectric layer.
3. A self-aligned manufacturing method for a silicon carbide MOSFET device according to claim 2, characterized in that: The depth of the first conductive type first injection region ranges from 0.1µm to 1.0µm, the width of the first conductive type first injection region is the same as the width of the first component of the T-type dielectric layer, and the depth of the first conductive type second injection region ranges from 0.5µm to 4.0µm.
4. The self-aligned manufacturing method of a silicon carbide MOSFET device according to claim 1, characterized in that: The concentration of the first conductivity type second injection region is substantially the same as the doping concentration of the first conductivity type first injection region, which is 1e16 cm -3 ~5e17cm -3 , the difference between the two does not exceed 1e16cm -3 .
5. The self-aligned manufacturing method of a silicon carbide MOSFET device according to claim 1, characterized in that: The thickness of the barrier layer ranges from 100Å to 1000Å, and the thickness of the sidewall ranges from 0.2µm to 1.0µm.
6. A silicon carbide MOSFET device, obtained by a self-aligned manufacturing method of a silicon carbide MOSFET device according to any one of claims 1 to 5, characterized in that: include, drain electrode; a first conductive type substrate located above the drain electrode; an epitaxial layer of the first conductivity type located on the substrate of the first conductivity type; a second conductivity type well region located in the first conductivity type epitaxial layer; a first conductivity type source region located in the second conductivity type well region; a first conductive type first implantation region located in the first conductive type epitaxial layer and between second conductive type well regions; a second implantation region of the first conductivity type located between the first implantation regions of the first conductivity type; a gate dielectric layer located on the first conductivity type epitaxial layer; a gate electrode located on the gate dielectric layer; an isolation dielectric layer located on both sides and above the gate electrode; A source electrode is located on the surface of the first conductive type source region and the second conductive type well region.