A GH4099 high-temperature alloy active cooling leading edge component and its manufacturing method

By using selective laser melting and femtosecond laser processing to prepare leading edge components of GH4099 high-temperature alloy, the problem of flow channel control was solved, a highly efficient thermal protection effect was achieved, and the preparation process was simplified.

CN117733180BActive Publication Date: 2026-11-17BEIJING HANGXING MACHINERY MFG CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202311802981.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-26
Publication Date
2026-11-17
Estimated Expiration
2043-12-26

AI Technical Summary

Technical Problem

Existing processing methods for sweating-type active cooling multi-stage flow channel structures cannot effectively control the flow channel distribution and size, resulting in difficulties in transporting the cooling medium and poor thermal protection.

Method used

A three-layer leading edge component was prepared by using GH4099 high-temperature alloy powder through a combination of selective laser melting and femtosecond laser processing. The component consists of an inner dense layer, an intermediate porous material layer, and a surface sweating structure layer. Conventional fractal channels, three-dimensional void channels, and microscale sweating channels are respectively set, and the channels are interconnected.

Benefits of technology

It achieves high precision in flow channel dimensions, smooth transport of cooling medium, avoids blockage, improves thermal protection effect, and simplifies the preparation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117733180B_ABST
    Figure CN117733180B_ABST
Patent Text Reader

Abstract

This invention relates to an actively cooled leading-edge component of GH4099 high-temperature alloy and its manufacturing method, belonging to the field of aircraft thermal protection technology. The manufacturing method includes powder pretreatment; selective laser melting (SLM) based on a leading-edge component model to obtain a blank; heat treatment of the blank; and two processing operations using a femtosecond laser on the surface sweating structure layer of the blank to obtain the leading-edge component. The leading-edge component consists of an inner dense layer, an intermediate porous material layer, and a surface sweating structure layer, from the inside out. The inner dense layer contains conventional fractal channels with a pore size ≥1mm; the intermediate porous material layer contains three-dimensional void channels with a diameter of 60μm-200μm; and the surface sweating structure layer contains microscale sweating channels with a pore size of 30-50μm. The cooling medium is uniformly spread on the surface of the leading-edge component, achieving self-driven thermal protection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of aircraft thermal protection technology, and in particular to a GH4099 high-temperature alloy active cooling leading edge component and its manufacturing method. Background Technology

[0002] Hypersonic vehicles generate enormous aerodynamic heat due to air friction during supersonic flight, potentially exceeding 10 MW / m². 2 The extreme heat flux density poses a significant challenge to the safe flight of hypersonic vehicles. To enable the vehicle to be used repeatedly for extended periods, non-ablative thermal protection methods must be employed to ensure the safety and reliability of the vehicle's leading edge.

[0003] Self-extraction sweating cooling is a highly efficient and promising active cooling thermal protection method for the leading edge. Its mechanism involves the cooling medium undergoing transport, heat exchange, and phase change processes through a multi-stage flow channel structure driven by capillary force, forming a protective gas film layer on the component surface to isolate the ultra-high temperature heat flow generated by friction between the air and the component. The sweating cooling thermal protection scheme has two main advantages: 1) stronger cooling capacity, primarily because liquids with high specific heat capacity (such as water) are generally chosen as the cooling medium, allowing it to absorb more heat during phase change; 2) the sweating cooling thermal protection uses a multi-stage transport channel similar to a leaf, enabling autonomous transport of the cooling medium under capillary force without the need for an additional power unit, further reducing weight. However, in practical applications, the sweating active cooling thermal protection scheme has not achieved ideal results. Related research has found that the main reason for the reduced thermal protection effect is the immaturity of the multi-stage flow channel structure design and fabrication technology, and the low controllability of the flow channel distribution and dimensions, leading to difficulties in transporting the cooling medium.

[0004] Currently, the processing methods for sweating-type active cooling multi-stage flow channel structures are powder sintering and layer etching. Powder sintering prepares porous media by sintering spherical metal powders or composite materials, but the flow channel distribution and size cannot be controlled. Layer etching etches flow channels on a thin plate and then diffuses and welds them layer by layer. The flow channels are controllable, but the design and processing of complex flow channels results in poor performance and high cost.

[0005] Therefore, there is an urgent need for a sweating-type active cooling thermal protection component with high thermal protection effect and a composite manufacturing method. Summary of the Invention

[0006] Based on the above analysis, the present invention aims to provide a GH4099 high-temperature alloy active cooling leading edge component and its manufacturing method, in order to solve the problem of poor thermal protection effect of existing leading edge components.

[0007] On one hand, the present invention provides a method for manufacturing an actively cooled leading edge component of GH4099 high-temperature alloy, comprising the following steps:

[0008] S1: Powder pretreatment, high-temperature alloy powder is subjected to vacuum low-temperature drying treatment;

[0009] The alloying elements and their mass fractions in the high-temperature alloy powder are as follows: C: ≤0.08wt.%, Cr: 17-20wt.%, W: 5-7wt.%, Mo: 3.5-4.5wt.%, Al: 1.7-2.4wt.%, Co: 5-8wt.%, Ti: 1-1.5wt.%, Fe: ≤2wt.%, B: ≤0.005wt.%, Mg: ≤0.01wt.%, Ce: ≤0.02wt.%, Mn: ≤0.4wt.%, Si: ≤0.5wt.%, P: ≤0.015wt.%, S: ≤0.015wt.%, with the balance being Ni;

[0010] S2: Selective laser melting. Based on the structural characteristics of the leading edge component model, the sample is sliced ​​to obtain an additive manufacturing sample model. Then, based on the leading edge component model, selective laser melting is performed on the high-temperature alloy powder. By controlling the process parameters and scanning strategy, a blank consisting of an internal dense layer, a middle porous material layer, and a surface sweating structure layer is obtained from the inside out.

[0011] S3: Heat treatment, subjecting the blank to heat treatment; the heat treatment includes solution treatment and aging or stress relief treatment and aging.

[0012] S4: Microscale sweating channels are processed on the surface sweating structure layer of the blank by two femtosecond laser processing operations, namely femtosecond laser drilling and femtosecond laser surface microstructure processing, to obtain a three-layer three-channel leading edge component.

[0013] The leading edge component consists of an inner dense layer, an intermediate porous material layer, and a surface sweating structure layer from the inside out. The inner dense layer contains conventional fractal channels with a pore size ≥ 1 mm. The intermediate porous material layer contains three-dimensional void channels with a diameter of 60 μm-200 μm. The surface sweating structure layer contains microscale sweating channels with a pore size of 30-50 μm.

[0014] Furthermore, the flowability of the dried high-temperature alloy powder is ≤17s / 50g.

[0015] Furthermore, the high-temperature alloy powder has a D10 of 15–20 μm, a D50 of 30–35 μm, and a D90 of 45–50 μm.

[0016] Furthermore, in step S2, when preparing the internal dense layer and the surface sweating structure layer, the parameters for laser selective melting are: laser power of 250-350W, scanning speed of 800-1000mm / s, overlap distance of 40-60μm, powder layer thickness of 40-60μm, and rotation of 67° layer by layer.

[0017] Furthermore, the density of the inner dense layer and the surface sweating structure layer is 99%, the thickness of the surface sweating structure layer is 500-800 μm, and the thickness of the inner dense layer is 10-15 mm.

[0018] Furthermore, in step S2, when preparing the intermediate porous material layer, the parameters for laser selective melting are: laser power of 150-200W, scanning speed of 1000-1200mm / s, overlap distance of 70-80μm, powder thickness of 40-60μm, reciprocating scanning, and no rotation.

[0019] Furthermore, the porosity of the intermediate porous material layer is 30-50%, and the thickness of the intermediate porous material layer is 5-10 mm.

[0020] Furthermore, in step S4, the process parameters for femtosecond laser drilling are as follows: laser spot diameter 10-20μm; laser pulse width 600-800fs; laser wavelength 1030nm; single pulse energy 30-40μJ; repetition frequency 500-700kHz; and scanning rate 200-400mm / s.

[0021] Further, in step S4, the femtosecond laser surface microstructure processing parameters are: laser spot diameter 60-70μm; pulse width 100-300fs; laser wavelength 1030nm; single pulse energy 20-30μJ; repetition frequency 1-3kHz; and scanning rate 5-10mm / s.

[0022] On the other hand, the present invention provides an active cooling leading edge component of GH4099 high-temperature alloy. The leading edge component has a three-layer, three-channel structure. The three-layer structure consists of an inner dense layer, an intermediate porous material layer, and a surface sweating structure layer from the inside out. The inner dense layer contains conventional fractal channels with a pore size ≥1mm; the intermediate porous material layer contains three-dimensional void channels with a pore size of 60-200μm; and the surface sweating structure layer contains microscale sweating channels with a pore size of 30-50μm. The channels are interconnected.

[0023] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:

[0024] 1. This invention provides a method for manufacturing a sweating active cooling edge component, which is used to prepare a leading edge component made of GH4099 high-temperature alloy. By combining additive manufacturing and femtosecond laser processing, a leading edge component with a surface sweating structure layer, a middle porous material layer and an internal dense layer can be prepared. The three layers are metallurgically bonded, and each of the three layers contains a conventional fractal flow channel, a three-dimensional void flow channel and a microscale sweating flow channel, and the flow channels are interconnected. The dimensional accuracy is high. In addition, the preparation method is relatively simple and easy to control.

[0025] 2. In this invention, by designing the model and controlling the process parameters and scanning strategy in the additive manufacturing process, it is possible to form three-dimensional void channels with a diameter of 60-200 μm and conventional fractal channels with a pore size of ≥1 mm in the middle porous material layer and the inner dense layer, respectively. Finally, microscale sweating channels with a pore size of 30-50 μm are processed on the surface sweating structure layer by femtosecond laser, resulting in high forming efficiency.

[0026] In this invention, the above-described technical solutions can be combined with each other to achieve more preferred combinations. Other features and advantages of this invention will be set forth in the following description, and some advantages may become apparent from the description or be learned by practicing the invention. The objects and other advantages of this invention can be realized and obtained from what is particularly pointed out in the description and drawings. Attached Figure Description

[0027] The accompanying drawings are for illustrative purposes only and are not intended to limit the invention. Throughout the drawings, the same reference numerals denote the same parts.

[0028] Figure 1 This is a schematic diagram of the leading edge component of a certain type of aircraft.

[0029] Figure 2 This is a schematic cross-sectional view of a leading-edge component of a certain type of aircraft.

[0030] Figure 3 Microscale sweating pathway diagram using femtosecond laser;

[0031] Figure 4 This is a diagram of the porous material layer structure in the middle;

[0032] In the figure, 1. Surface sweating structure layer; 2. Middle porous material layer; 3. Internal dense layer; 4. Microscale sweating channel; 5. Three-dimensional void channel; 6. Conventional fractal channel; 7. Cooling medium. Detailed Implementation

[0033] The preferred embodiments of the present invention will now be described in detail with reference to the accompanying drawings, which constitute a part of the present invention and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not intended to limit the scope of the present invention.

[0034] Leading-edge components are critical structural parts in aircraft, facing severe thermal protection challenges during high Mach number flight. Self-suction active cooling allows the leading edge to achieve autonomous cooling without power, enabling it to operate at higher temperatures. Currently, the main fabrication processes for leading-edge components include powder sintering, lamination etching, and additive manufacturing. However, existing processes suffer from poor stability, high control difficulty, and low forming accuracy, making it impossible to fabricate complex flow channels and potentially clogging the sweating channels, thus affecting the cooling effect.

[0035] Therefore, the present invention provides a method for manufacturing an actively cooled leading edge component of GH4099 high-temperature alloy, comprising the following steps:

[0036] S1: Powder pretreatment, high-temperature alloy powder is subjected to vacuum low-temperature drying treatment;

[0037] The alloying elements and their mass fractions in the high-temperature alloy powder are as follows: C: ≤0.08wt.%, Cr: 17-20wt.%, W: 5-7wt.%, Mo: 3.5-4.5wt.%, Al: 1.7-2.4wt.%, Co: 5-8wt.%, Ti: 1-1.5wt.%, Fe: ≤2wt.%, B: ≤0.005wt.%, Mg: ≤0.01wt.%, Ce: ≤0.02wt.%, Mn: ≤0.4wt.%, Si: ≤0.5wt.%, P: ≤0.015wt.%, S: ≤0.015wt.%, with the balance being Ni.

[0038] S2: Selective laser melting. Based on the structural characteristics of the leading edge component model, the sample is sliced ​​to obtain an additive manufacturing sample model. Then, based on the leading edge component model, selective laser melting is performed on the high-temperature alloy powder. By controlling the process parameters and scanning strategy, a blank consisting of an internal dense layer, a middle porous material layer, and a surface sweating structure layer is obtained from the inside out.

[0039] S3: Heat treatment, subjecting the blank to heat treatment; the heat treatment includes solution treatment and aging or stress relief treatment and aging.

[0040] S4: Microscale sweating channels are processed on the surface sweating structure layer of the blank using two femtosecond laser processing operations, namely femtosecond laser drilling and femtosecond laser surface microstructure processing, to obtain a three-layer, three-channel leading edge component.

[0041] The leading edge component consists of an inner dense layer, an intermediate porous material layer, and a surface sweating structure layer from the inside out. The inner dense layer contains conventional fractal channels with a pore size ≥ 1 mm. The intermediate porous material layer contains three-dimensional void channels with a diameter of 60 μm-200 μm. The surface sweating structure layer contains microscale sweating channels with a pore size of 30-50 μm.

[0042] Compared with existing technologies, the preparation method provided by this invention, through the combination of additive manufacturing and femtosecond laser processing, can fabricate a leading edge component with a three-layer structure, consisting of a surface sweating structure layer 1, a middle porous material layer 2, and an inner dense layer 3, from the outside to the inside. Furthermore, microscale sweating channels 4, three-dimensional void channels 5, and conventional fractal channels 6 are respectively fabricated on the three-layer structure, and these channels are interconnected. Cooling medium 7 sequentially flows through the conventional fractal channel 6, the three-dimensional void channel 5, and the microscale sweating channel 4. Under capillary action, the cooling medium 7 seeps out from the microscale sweating channel 4, undergoing a phase change and absorbing heat; and a gas film is formed on the leading edge surface, thereby achieving the purpose of cooling. The leading edge component obtained by this invention has high channel dimensional accuracy, does not have the problem of channel blockage, and the preparation method is relatively simple and easy to control.

[0043] Specifically, in step S1, the flowability of the dried high-temperature alloy powder is ≤17s / 50g.

[0044] It should be noted that in this invention, the raw material powder is the initial material for preparing the leading edge component, and its properties directly affect the quality of the leading edge component. Therefore, the GH4099 high-temperature alloy powder needs to be dried to control its flowability to ≤17s / 50g (Hall flow rate), which facilitates the subsequent preparation of the leading edge component and ensures the formation and precision of the flow channel.

[0045] Specifically, in step S1, the loose packing density of the dried GH4099 high-temperature alloy powder is ≥4.6 g / cm³. 3 .

[0046] It should be noted that in this invention, the loose packing density has a significant impact on the density of the additive material. A lower loose packing density is prone to generating incomplete fusion defects inside the material, which can seriously affect the formation of the flow channel.

[0047] Specifically, in step S1, the high-temperature alloy powder has a D10 of 15-20 μm, a D50 of 30-35 μm, and a D90 of 45-50 μm.

[0048] It should be noted that, in this invention, uniformly distributed powder can improve the stability of powder spreading, resulting in a defect-free leading edge component and ensuring the forming and precision of the flow channel.

[0049] It should be noted that in this invention, the additive sample model is divided from the inside to the surface into an internal dense layer, an intermediate porous material layer, and a surface sweating structure layer of different thicknesses. During the additive manufacturing process, a layer of GH4099 high-temperature alloy powder is uniformly spread on the substrate, and different process parameters are set according to the internal dense layer, the intermediate porous material layer, and the surface sweating structure layer. After the first layer of GH4099 high-temperature alloy powder is formed, powder is spread again on the basis of the first layer, and the above process is repeated to obtain a blank with a three-layer structure.

[0050] Preferably, the substrate is made of a nickel-based high-temperature alloy.

[0051] It should be noted that in this invention, GH4099 high-temperature alloy blanks are prepared using selective laser melting. In order to ensure the density of the internal dense layer, the surface sweating structure layer and the middle porous material layer, as well as to facilitate subsequent femtosecond laser processing and channel precision, the preparation parameters for each layer are different.

[0052] Specifically, in step S2, when preparing the internal dense layer and the surface sweating structure layer, the parameters for laser selective melting are: laser power of 250-350W, scanning speed of 800-1000mm / s, overlap distance of 40-60μm, powder layer thickness of 40-60μm, and rotation of 67° layer by layer.

[0053] With the above-mentioned process parameters, a high-density internal dense layer and a surface sweating structure layer were obtained, both with a density exceeding 99% and exhibiting high strength. During service, the surface sweating structure layer of the leading edge component is in direct contact with the air and bears the highest heat; its primary function is protection. Therefore, the thickness of the surface sweating structure layer in the fabricated leading edge component is above 500 μm. However, as its thickness gradually increases to above 800 μm, it becomes difficult to prepare subsequent microscale sweating channels. Therefore, the thickness of the surface sweating structure layer is controlled at 500-800 μm, and the thickness of the internal dense layer is 10-15 mm.

[0054] Specifically, in step S2, when preparing the intermediate porous material layer, the parameters for laser selective melting are: laser power of 150-200W, scanning speed of 1000-1200mm / s, overlap distance of 70-80μm, powder thickness of 40-60μm, reciprocating scanning, and no rotation.

[0055] With the above process parameters, the porosity of the resulting intermediate porous material layer is 30-50%, and its thickness is 5-10 mm. Located between the surface sweating structure layer and the inner dense layer, this intermediate porous material layer is a transitional layer. The cooling medium in the leading edge component diffuses and permeates from the inner dense layer to the surface sweating structure layer. To avoid hindering the diffusion of the cooling medium, the porosity of the intermediate porous material layer is 30-50%. When the porosity of the intermediate porous material layer is greater than 50%, the overall strength of the leading edge component decreases; when the porosity is less than 30%, it hinders the diffusion and permeation of the cooling medium, resulting in a low diffusion rate and inability to form effective protection on the surface sweating structure layer.

[0056] Specifically, in step S3, a blank is obtained by additive manufacturing. The blank needs to be heat-treated to ensure that microscale sweating channels are formed on the surface of the blank using a femtosecond laser.

[0057] Specifically, heat treatment can combine solution treatment and aging treatment. Solution treatment is performed at 1100-1200℃ for 1-2 hours, while aging treatment is performed at 700-850℃ for 16 hours. Alternatively, stress relief treatment and aging treatment can be used. Stress relief treatment involves heating at 500-550℃ and holding for 1.5-2.5 hours. Aging treatment requires a higher initial holding temperature than the second holding temperature. The initial holding temperature is 800-850℃ for 1-2 hours, and the second holding temperature is 700-750℃ for 3-4 hours.

[0058] The leading edge component mainly cools itself through the principle of sweating. A three-layer structure blank is obtained by additive manufacturing. The three layers are, from the inside to the outside, an inner dense layer, an intermediate porous material layer, and a surface sweating structure layer. Conventional fractal flow channels and three-dimensional void flow channels are respectively set in the inner dense layer and the intermediate porous material layer, and the two are interconnected. The pore diameter of the conventional fractal flow channel is ≥1mm; the pore diameter of the three-dimensional void flow channel is 60~200μm.

[0059] To achieve the sweating cooling of the aforementioned leading edge component, a microscale sweating channel with a pore size of 30–50 μm was prepared on the surface sweating structure layer using a femtosecond laser. The resulting channel has high precision and does not have a clogging problem, thus ensuring the sweating cooling effect of the leading edge component.

[0060] Specifically, the femtosecond laser processing includes the following steps:

[0061] T1: Fix the blank and set parameters;

[0062] T2: Femtosecond laser drilling: Using a femtosecond laser to perform laser drilling on the sweating structure layer on the surface of the blank, ensuring that the laser beam is perpendicular to the surface of the blank;

[0063] T3: Femtosecond laser surface microstructure processing: Femtosecond laser is used to process the surface of components to form hydrophilic microstructures, which facilitates the spread of cooling media.

[0064] It should be noted that a series of regularly arranged microchannels with apertures ≤50μm are prepared on the surface of the component using femtosecond lasers; at the same time, the surface is modified using femtosecond lasers to improve the wettability of the material on the surface of the component, obtain sufficiently high capillary pressure, overcome the effect of gravity, and realize the self-suction of the cooling medium.

[0065] Specifically, in step S4, the femtosecond laser drilling process parameters are: laser spot diameter 10-20μm; laser pulse width 600-800fs; laser wavelength 1030nm; single pulse energy 30-40μJ; repetition frequency 500-700kHz; and scanning rate 200-400mm / s.

[0066] Specifically, in step S4, the femtosecond laser surface microstructure processing parameters are: laser spot diameter 60-70μm; pulse width 100-300fs; laser wavelength 1030nm; single pulse energy 20-30μJ; repetition frequency 1-3kHz; and scanning rate 5-10mm / s.

[0067] By using a femtosecond laser to drill holes in the surface sweating structure layer, ensuring that the laser beam is perpendicular to the surface sweating structure layer of the blank, it can directly penetrate the surface sweating structure layer and connect with the middle porous material layer. This allows the cooling medium to diffuse directly from the inner dense layer to the surface sweating structure layer through conventional fractal channels, three-dimensional void channels, and microscale sweating channels in sequence, forming a protective layer around the surface sweating structure layer and achieving self-driven thermal protection.

[0068] The resulting leading edge component is a three-layer, three-channel structure. From the inside out, the three layers are: an inner dense layer, a middle porous material layer, and a surface sweating structure layer. The density of the inner dense layer and the surface sweating structure layer is above 99%. The thickness of the surface sweating structure layer is 500-800 μm, and the thickness of the inner dense layer is 10-15 mm. The porosity of the middle porous material layer is 30-50%, and its thickness is 5-10 mm. The inner dense layer contains conventional fractal channels with a pore size ≥1 mm. The middle porous material layer contains three-dimensional void channels with a pore size of 60-200 μm, and the surface sweating structure layer contains microscale sweating channels with a pore size of 30-50 μm. The conventional fractal channels, the three-dimensional void channels, and the microscale sweating channels are interconnected.

[0069] To more clearly describe the present invention, the following embodiments and comparative examples are provided for further illustration.

[0070] Example 1

[0071] This embodiment provides a method for manufacturing an actively cooled leading edge component of GH4099 high-temperature alloy, including the following steps:

[0072] S1: Powder pretreatment, vacuum low-temperature drying treatment (100-120℃, 1-2h) of high-temperature alloy powder to improve the fluidity of raw materials;

[0073] The mass percentage of GH4099 high-temperature alloy powder is as follows: C: 0.039 wt.%, Cr: 18.81 wt.%, W: 6.10 wt.%, Mo: 4.19 wt.%, Co: 6.56 wt.%, Al: 2.07 wt.%, Ti: 1.28 wt.%, Fe: 1.05 wt.%, B: 0.002 wt.%, Mg: 0.007 wt.%, Ce: 0.015 wt.%, Mn: 0.02 wt.%, Si: 0.31 wt.%, P: 0.004 wt.%, S: 0.005 wt.%, with the balance being Ni.

[0074] The GH4099 high-temperature alloy powder has a D10 of 19 μm, a D50 of 34 μm, a D90 of 49 μm, a flowability (Hall flow rate) of 15.64 s / 50 g, and a loose packing density of 4.6 g / cm³. 3 ;

[0075] S2: Additive manufacturing. Based on the structural characteristics of the leading edge component model, slicing is performed to prepare an additive sample model. The additive sample model is then split from the inside to the surface into an internal dense layer, an intermediate porous material layer, and a surface sweating structure layer of different thicknesses. During the additive manufacturing process, a layer of GH4099 high-temperature alloy powder is uniformly spread on a nickel-based high-temperature alloy substrate. Different process parameters are set according to the internal dense layer, the intermediate porous material layer, and the surface sweating structure layer. After the first layer of GH4099 high-temperature alloy powder is formed, powder is spread again on the basis of the first layer, and the above process is repeated to obtain a blank with a three-layer structure.

[0076] Powder was prepared into a blank by selective laser melting. When preparing the internal dense layer and the surface sweating structure layer, the laser power of selective laser melting was 300W, the scanning speed was 960mm / s, the overlap distance was 50μm, the powder thickness was 40μm, and the layer was rotated 67° layer by layer.

[0077] The process parameters for laser selective melting in preparing the intermediate porous material layer are as follows: laser power is 200W, scanning speed is 1200mm / s, overlap distance is 80μm, powder thickness is 40μm, reciprocating scanning, no rotation;

[0078] S3: Heat treatment, the blank is heat treated by solution treatment and aging, the solution treatment temperature is 1150℃ and the holding time is 2h; the aging temperature is 750℃ and the holding time is 16h, followed by air cooling.

[0079] S4: After heat treatment, the blank is cleaned of sintered powder and impurities, then processed. A femtosecond laser is then used to process the surface of the processed blank (on the surface sweating structure layer) to create microscale sweating channels, including:

[0080] T1: Fix the processed blank and then set the operating parameters of the femtosecond laser;

[0081] T2: Femtosecond laser drilling: Laser drilling is performed on the surface sweating structure layer of the blank using a femtosecond laser, ensuring that the laser beam is perpendicular to the surface of the blank. The aperture of the microscale sweating channel is 30-50μm, penetrating the surface sweating structure layer.

[0082] The laser spot diameter is 20μm, the laser pulse width is 800fs, the laser wavelength is 1030nm, the single pulse energy is 40μJ, the repetition frequency is 600kHz, and the scanning rate is 400mm / s.

[0083] T3: Surface microstructure processing: The surface of the component is processed using a femtosecond laser to form a hydrophilic microstructure, which facilitates the spread of the cooling medium. The laser spot diameter is 70μm; the pulse width is 300fs; the laser wavelength is 1030nm; the single pulse energy is 30μJ; the repetition frequency is 3kHz; and the scanning rate is 10mm / s to obtain the leading edge component.

[0084] Reference Figure 1-4 The leading edge component is conical and consists of a three-layer structure: an inner dense layer, a middle porous material layer, and a surface sweating structure layer, with thicknesses of 10 mm, 5 mm, and 0.5 mm, respectively. The inner dense layer contains conventional fractal channels with pore sizes ≥ 1 mm; the middle porous material layer contains three-dimensional void channels with pore sizes of 60-200 μm; and the surface sweating structure layer contains microscale sweating channels with pore sizes of 30-50 μm (see reference). Figure 3 ).

[0085] Example 2

[0086] The preparation process of Example 2 is largely the same as that of Example 1, except that the laser selective melting process in Example 2 is different from that in Example 1.

[0087] S1: Powder pretreatment, vacuum low-temperature drying treatment (100-120℃, 1-2h) of high-temperature alloy powder to improve the fluidity of raw materials;

[0088] The mass percentage of GH4099 high-temperature alloy powder is as follows: C: 0.027 wt.%, Cr: 19.35 wt.%, W: 6.78 wt.%, Mo: 3.73 wt.%, Co: 7.64 wt.%, Al: 1.83 wt.%, Ti: 1.08 wt.%, Fe: 1.93 wt.%, B: 0.004 wt.%, Mg: 0.005 wt.%, Ce: 0.015 wt.%, Mn: 0.31 wt.%, Si: 0.46 wt.%, P: 0.003 wt.%, S: 0.002 wt.%, with the balance being Ni.

[0089] The GH4099 high-temperature alloy powder has a D10 of 16 μm, a D50 of 33 μm, a D90 of 46 μm, a flowability (Hall flow rate) of 16.69 s / 50 g, and a loose packing density of 4.7 g / cm³. 3 ;

[0090] S2: Additive manufacturing. Based on the structural characteristics of the leading edge component model, slicing is performed to prepare an additive sample model. The additive sample model is then split from the inside to the surface into an internal dense layer, an intermediate porous material layer, and a surface sweating structure layer of different thicknesses. During the additive manufacturing process, a layer of GH4099 high-temperature alloy powder is uniformly spread on a nickel-based high-temperature alloy substrate. Different process parameters are set according to the internal dense layer, the intermediate porous material layer, and the surface sweating structure layer. After the first layer of GH4099 high-temperature alloy powder is formed, powder is spread again on the basis of the first layer, and the above process is repeated to obtain a blank with a three-layer structure.

[0091] Powder was prepared into a blank by selective laser melting. When preparing the internal dense layer and the surface sweating structure layer, the laser power of selective laser melting was 350W, the scanning speed was 1000mm / s, the overlap distance was 40μm, the powder thickness was 40μm, and the layer was rotated 67° layer by layer.

[0092] The process parameters for laser selective melting in preparing the intermediate porous material layer are as follows: laser power is 150W, scanning speed is 1000mm / s, overlap distance is 90μm, powder thickness is 40μm, reciprocating scanning, no rotation;

[0093] S3: Heat treatment, the blank is heat treated by solution treatment and aging, the solution treatment temperature is 1150℃ and the holding time is 2h; the aging temperature is 750℃ and the holding time is 16h, followed by air cooling.

[0094] S4: After heat treatment, the blank is cleaned of sintered powder and impurities, then processed. A femtosecond laser is then used to process the surface of the processed blank (on the surface sweating structure layer) to create microscale sweating channels, including:

[0095] T1: Fix the processed blank and then set the operating parameters of the femtosecond laser;

[0096] T2: Femtosecond laser drilling: Laser drilling is performed on the surface sweating structure layer of the blank using a femtosecond laser, ensuring that the laser beam is perpendicular to the surface of the blank. The aperture of the microscale sweating channel is 30-50μm, penetrating the surface sweating structure layer.

[0097] The laser spot diameter is 20μm, the laser pulse width is 800fs, the laser wavelength is 1030nm, the single pulse energy is 40μJ, the repetition frequency is 600kHz, and the scanning rate is 400mm / s.

[0098] T3: Surface microstructure processing: The surface of the component is processed using a femtosecond laser to form a hydrophilic microstructure, which facilitates the spread of the cooling medium. The laser spot diameter is 70μm; the pulse width is 300fs; the laser wavelength is 1030nm; the single pulse energy is 30μJ; the repetition frequency is 3kHz; and the scanning rate is 10mm / s to obtain the leading edge component.

[0099] Reference Figure 1 and Figure 2 The leading edge component is conical and consists of three layers: an inner dense layer, an intermediate porous material layer, and a surface sweating structure layer, from the inside out. The inner dense layer contains conventional fractal channels with a pore size ≥1mm; the intermediate porous material layer contains three-dimensional void channels with a pore size of 60-200μm; and the surface sweating structure layer contains microscale sweating channels with a pore size of 30-50μm.

[0100] Example 3

[0101] The preparation process of Example 3 is largely the same as that of Example 1, except that the femtosecond laser processing technology in Example 3 is different from that in Example 1.

[0102] S1: Powder pretreatment, vacuum low-temperature drying treatment (100-120℃, 1-2h) of high-temperature alloy powder to improve the fluidity of raw materials;

[0103] The mass percentage of GH4099 high-temperature alloy powder is as follows: C: 0.06 wt.%, Cr: 17.96 wt.%, W: 5.97 wt.%, Mo: 4.41 wt.%, Co: 5.61 wt.%, Al: 2.37 wt.%, Ti: 1.46 wt.%, Fe: 1.57 wt.%, B: 0.003 wt.%, Mg: 0.004 wt.%, Ce: 0.011 wt.%, Mn: 0.39 wt.%, Si: 0.39 wt.%, P: 0.007 wt.%, S: 0.003 wt.%, with the balance being Ni.

[0104] The GH4099 high-temperature alloy powder has a D10 of 17 μm, a D50 of 34 μm, a D90 of 49 μm, a flowability (Hall flow rate) of 15.13 s / 50 g, and a loose packing density of 4.6 g / cm³. 3 ;

[0105] S2: Additive manufacturing. Based on the structural characteristics of the leading edge component model, slicing is performed to prepare an additive sample model. The additive sample model is then split from the inside to the surface into an internal dense layer, an intermediate porous material layer, and a surface sweating structure layer of different thicknesses. During the additive manufacturing process, a layer of GH4099 high-temperature alloy powder is uniformly spread on a nickel-based high-temperature alloy substrate. Different process parameters are set according to the internal dense layer, the intermediate porous material layer, and the surface sweating structure layer. After the first layer of GH4099 high-temperature alloy powder is formed, powder is spread again on the basis of the first layer, and the above process is repeated to obtain a blank with a three-layer structure.

[0106] Powder was prepared into a blank by selective laser melting. When preparing the internal dense layer and the surface sweating structure layer, the laser power of selective laser melting was 300W, the scanning speed was 960mm / s, the overlap distance was 50μm, the powder thickness was 40μm, and the layer was rotated 67° layer by layer.

[0107] The process parameters for laser selective melting in preparing the intermediate porous material layer are as follows: laser power is 200W, scanning speed is 1200mm / s, overlap distance is 80μm, powder thickness is 40μm, reciprocating scanning, no rotation;

[0108] S3: Heat treatment, the blank is heat treated by solution treatment and aging, the solution treatment temperature is 1150℃ and the holding time is 2h; the aging temperature is 750℃ and the holding time is 16h, followed by air cooling.

[0109] S4: After heat treatment, the blank is cleaned of sintered powder and impurities, then processed. A femtosecond laser is then used to process the surface of the processed blank (on the surface sweating structure layer) to create microscale sweating channels, including:

[0110] T1: Fix the processed blank and then set the operating parameters of the femtosecond laser;

[0111] T2: Femtosecond laser drilling: Laser drilling is performed on the surface sweating structure layer of the blank using a femtosecond laser, ensuring that the laser beam is perpendicular to the surface of the blank. The aperture of the microscale sweating channel is 30-50μm, penetrating the surface sweating structure layer.

[0112] The laser spot diameter is 10 μm, the laser pulse width is 600 fs, the laser wavelength is 1030 nm, the single pulse energy is 40 μJ, the repetition frequency is 500 kHz, and the scanning rate is 400 mm / s.

[0113] T3: Surface microstructure processing: The surface of the component is processed using a femtosecond laser to form a hydrophilic microstructure, which facilitates the spread of the cooling medium. The laser spot diameter is 70μm; the pulse width is 200fs; the laser wavelength is 1030nm; the single pulse energy is 30μJ; the repetition frequency is 2kHz; and the scanning rate is 7mm / s to obtain the leading edge component.

[0114] Reference Figure 1 and Figure 2 The leading edge component is conical and consists of three layers: an inner dense layer, an intermediate porous material layer, and a surface sweating structure layer, from the inside out. The inner dense layer contains conventional fractal channels with a pore size ≥1mm; the intermediate porous material layer contains three-dimensional void channels with a pore size of 60-200μm; and the surface sweating structure layer contains microscale sweating channels with a pore size of 30-50μm.

[0115] Example 4

[0116] The preparation process of Example 4 is largely the same as that of Example 1, except that the heat treatment in Example 4 is different from that in Example 1.

[0117] In step S3, the heat treatment can also be stress relief treatment and aging treatment. The stress relief treatment is heated to 530°C and held for 1 hour, then cooled to room temperature in the furnace. The aging treatment is heated to a higher temperature for the first holding than for the second holding. The blank is heated to 830°C for the first holding and held for 1.5 hours. The second holding is heated to 730°C for 3 hours.

[0118] Example 5

[0119] The preparation process of Example 5 is largely the same as that of Example 4, except that the heat treatment in Example 5 is different from that in Example 4.

[0120] In step S3, the heat treatment can also be stress relief treatment and aging treatment. The stress relief treatment is heated to 500°C and held for 2 hours, and then cooled to room temperature in the furnace. The aging treatment is heated to a higher temperature for the first holding than for the second holding. The blank is heated to 800°C for the first holding and held for 2 hours. The second holding is heated to 700°C for 4 hours.

[0121] Example 6

[0122] The preparation process of Example 6 is largely the same as that of Example 4, except that the heat treatment in Example 6 is different from that in Example 4.

[0123] In step S3, the heat treatment can also be stress relief treatment and aging treatment. The stress relief treatment is heated to 520°C and held for 2 hours, then cooled to room temperature in the furnace. The aging treatment is heated to a higher temperature for the first holding than for the second holding. The blank is heated to 820°C for the first holding and held for 1.5 hours. The second holding is heated to 720°C for 3 hours.

[0124] Example 7

[0125] The preparation process of Example 7 is largely the same as that of Example 4, except that the heat treatment in Example 7 is different from that in Example 4.

[0126] In step S3, the heat treatment can also be stress relief treatment and aging treatment. The stress relief treatment is heated to 550°C and held for 1.5 hours, then cooled to room temperature in the furnace. The aging treatment is heated to a higher temperature for the first holding than for the second holding. The blank is heated to 850°C for the first holding and held for 1 hour. The second holding is heated to 750°C for 3 hours.

[0127] Comparative Example 1

[0128] This comparative example provides a sintering manufacturing method for a sweating active cooling leading edge component, including the following steps:

[0129] S1: Sieving Process: Based on the service conditions, spherical high-temperature alloy powder materials with the required particle diameter are selected using a vibrating screen. Urea (CO(NH2)2) pore-forming agent is selected, and urea is ground into powders of different particle diameters, which are then sieved to separate urea with the required particle diameter.

[0130] S2: Powder mixing treatment: The high-temperature alloy powder obtained in S1 is combined with urea in different proportions and mechanically dry-mixed in a ball mill for 4 hours to make the material evenly distributed.

[0131] S3: Compression Molding: Before molding, to improve the strength of the compact and prevent segregation of the powder mixture, an appropriate amount of liquid polyvinyl alcohol is added to the powder as a molding agent and ground evenly. The ground powder is then introduced into the leading edge mold and pressed into a conical porous media leading edge blank under static pressure in a large hydraulic press.

[0132] S4: Sintering and Shaping: First, slowly heat from room temperature to 180℃ to fully decompose the pore-forming agent in the porous blank; then heat to 600℃ and hold for 30-60 minutes to completely reduce the surface oxides of the powder particles, forming sintering necks at the particle interfaces; next, heat to the sintering temperature of 1250℃ and hold for 100-150 minutes to allow sintering to proceed fully and near completion. Finally, reduce the temperature to 500℃ and allow it to cool naturally to room temperature.

[0133] Comparative Example 2

[0134] This comparative example provides a method for etching a layer to manufacture a sweating active cooling leading edge component, including the following steps:

[0135] S1: Plate preparation: First, use organic solvents to clean the surface of the high-temperature alloy sheet to remove surface oil, impurities, etc.

[0136] S2: Plate fixing: Fix the high-temperature alloy sheet on the processing platform to ensure that the high-temperature alloy sheet will not move during the micro-groove processing;

[0137] S3: Parameter Settings: Set all operating parameters for the photolithography or chemical etching equipment;

[0138] S4: Flow channel processing: Using photolithography or chemical etching equipment to process at fixed positions on the surface of a high-temperature alloy thin plate to obtain complex internal flow channels.

[0139] S5: Cleaning: Clean the grooves on the surface of the high-temperature alloy sheet to ensure the wettability of the groove walls and the flow performance of the cooling medium. After cleaning, perform drying.

[0140] S6: Welding: Welding metal plates processed by photolithography or chemical etching to form a layer plate leading edge structure, thereby obtaining a layer plate etching leading edge component.

[0141] Comparative Example 3

[0142] This comparative example provides a laser additive manufacturing method for a sweating-type actively cooled leading edge component, including the following steps:

[0143] S1: Powder pretreatment: Vacuum low-temperature drying treatment of raw materials (100-120℃, 1-2h) to improve the flowability of raw materials;

[0144] In this embodiment, the raw material is GH4099 high-temperature alloy powder, with the following mass percentages: 18.81 wt.% Cr, 6.10 wt.% W, 4.19 wt.% Mo, 6.56 wt.% Co, <0.02 wt.% Mn, 2.07 wt.% Al, 1.28 wt.% Ti, 0.039 wt.% C, and the balance being Ni.

[0145] The GH4099 high-temperature alloy powder has a D10 of 15–20 μm, a D50 of 30–35 μm, a D90 of 45–50 μm, a flowability (Hall flow rate) of 17 s / 50 g, and a loose packing density of 4.6 g / cm³. 3 ;

[0146] S2: Model Design: Based on the structural characteristics of the leading edge component, slice the model to prepare the additive prototype model;

[0147] S3: Additive Manufacturing: Based on the sliced ​​model, the leading edge component is formed by selective laser melting. The laser power of selective laser melting additive manufacturing is 300W, the scanning speed is 960mm / s, the overlap distance is 50μm, the powder thickness is 40μm, and the layer-by-layer rotation is 67°.

[0148] S4: Heat treatment: Anneal the blank in a vacuum environment at a temperature of 1200℃ for 2 hours.

[0149] S5: Machining: Remove sintered powder and impurities from the surface of the annealed blank, and then process it; finally obtain the laser additive manufacturing sweating active cooling leading edge component.

[0150] Performance testing

[0151] The leading edge components obtained in Examples 1-7 and Comparative Examples 1-3 were tested. The leading edge components were directly injected with an oxyacetylene flame at a temperature of 1700K and a heat flux density of 0.32. The temperatures of the inner and outer surfaces of the leading edge components before and after the coolant was introduced were measured. The test results are shown in Table 1 (each group was tested three times and the average value was taken).

[0152] Table 1 Test Results

[0153]

[0154]

[0155] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for manufacturing a GH4099 high-temperature alloy actively cooled leading-edge component, characterized in that, Includes the following steps: S1: Powder pretreatment, high-temperature alloy powder is subjected to vacuum low-temperature drying treatment; The alloying elements and their mass fractions in the high-temperature alloy powder are as follows: C: ≤0.08wt.%, Cr: 17-20wt.%, W: 5-7wt.%, Mo: 3.5-4.5wt.%, Al: 1.7-2.4wt.%, Co: 5-8wt.%, Ti: 1-1.5wt.%, Fe: ≤2wt.%, B: ≤0.005wt.%, Mg: ≤0.01wt.%, Ce: ≤0.02wt.%, Mn: ≤0.4wt.%, Si: ≤0.5wt.%, P: ≤0.015wt.%, S: ≤0.015wt.%, with the balance being Ni; S2: Selective laser melting. Based on the structural characteristics of the leading edge component model, the sample is sliced ​​to obtain an additive manufacturing sample model. Then, based on the leading edge component model, selective laser melting is performed on the high-temperature alloy powder. By controlling the process parameters and scanning strategy, a blank consisting of an internal dense layer, a middle porous material layer, and a surface sweating structure layer is obtained from the inside out. The density of the inner dense layer and the surface sweating structure layer is 99%, the thickness of the surface sweating structure layer is 500-800µm, the thickness of the inner dense layer is 10-15mm, and the porosity of the intermediate porous material layer is 30-50%, with a thickness of 5-10mm. S3: Heat treatment, subjecting the blank to heat treatment; the heat treatment includes solution treatment and aging or stress relief treatment and aging. S4: Microscale sweating channels are processed on the surface sweating structure layer of the blank by two femtosecond laser processing operations, namely femtosecond laser drilling and femtosecond laser surface microstructure processing, to obtain a three-layer three-channel leading edge component. The internal dense layer contains conventional fractal channels with a pore size ≥ 1 mm; the intermediate porous material layer contains three-dimensional void channels with a pore size of 60-200 µm; and the surface sweating structure layer contains microscale sweating channels with a pore size of 30-50 µm. The conventional fractal channels, the three-dimensional void channels, and the microscale sweating channels are interconnected.

2. The manufacturing method of the GH4099 high-temperature alloy active cooling leading edge component according to claim 1, characterized in that, In step S1, the flowability of the dried high-temperature alloy powder is ≤17s / 50g.

3. The manufacturing method of the GH4099 high-temperature alloy active cooling leading edge component according to claim 1, characterized in that, In step S1, the high-temperature alloy powder has a D10 of 15~20µm, a D50 of 30~35µm, and a D90 of 45~50µm.

4. The manufacturing method of the GH4099 high-temperature alloy active cooling leading edge component according to claim 1, characterized in that, In step S2, when preparing the internal dense layer and the surface sweating structure layer, the parameters for laser selective melting are: laser power of 250-350W, scanning speed of 800-1000mm / s, overlap distance of 40-60µm, powder layer thickness of 40-60µm, and rotation of 67° layer by layer.

5. The manufacturing method of the GH4099 high-temperature alloy active cooling leading edge component according to claim 1, characterized in that, In step S2, when preparing the intermediate porous material layer, the parameters for laser selective melting are: laser power of 150-200W, scanning speed of 1000-1200mm / s, overlap distance of 70-80µm, powder thickness of 40-60µm, reciprocating scanning, and no rotation.

6. The manufacturing method of the GH4099 high-temperature alloy active cooling leading edge component according to claim 1, characterized in that, In step S4, the femtosecond laser drilling process parameters are as follows: laser spot diameter 10-20μm; laser pulse width 600-800fs; laser wavelength 1030nm; single pulse energy 30-40µJ; repetition frequency 500-700kHz; and scanning rate 200-400mm / s.

7. The manufacturing method of the GH4099 high-temperature alloy active cooling leading edge component according to claim 1, characterized in that, In step S4, the femtosecond laser surface microstructure processing parameters are as follows: laser spot diameter 60-70μm; pulse width 100-300fs; laser wavelength 1030nm; single pulse energy 20-30µJ; repetition frequency 1-3kHz; and scanning rate 5-10mm / s.

8. A GH4099 high-temperature alloy actively cooled leading edge component, characterized in that, Prepared by the manufacturing method according to any one of claims 1-7.

Citation Information

Patent Citations

  • Ultra-high speed aircraft thermal protection and drag reduction method and system

    CN104608942A

  • Aircraft and shell assembly thereof

    CN109835466A

  • Selective laser melting forming process for GH4099 nickel-based alloy element

    CN112589115A

  • Preparation method of micro-structure reinforced surface and plate-type evaporator of micro-structure reinforced surface

    CN115464272A