A hybrid membrane based on UiO66 modification, preparation method and application in flow battery

By mixing carbonized UiO-66 with SPEEK and modifying β-CD, hybrid films with good chemical stability under strong acid and strong oxidation conditions were prepared, which solved the poor circulation stability of existing proton exchange membranes in all vanadium flow batteries. The problem of improving battery efficiency and stability.

CN117747895BActive Publication Date: 2024-10-22NANJING TECH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311602980.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-27
Publication Date
2024-10-22
Estimated Expiration
2043-11-27

AI Technical Summary

Technical Problem

The existing proton exchange membranes have poor circulation stability in all vanadium flow batteries, especially under strong acid and strong oxidation conditions, and are costly and difficult to replace.

Method used

A hybrid film based on UiO66 was used to mix UiO-66 with SPEEK by carbonizing UiO-66, and optionally modifying β-CD, and prepared by casting method to form an S/β-CUiO-66-3% hybrid film.

Benefits of technology

The hybrid film has good chemical stability under strong acid and strong oxidation conditions, improves water absorption and tensile strength, reduces swelling, and shows higher battery efficiency and longer battery life in all vanadium flow batteries. Cyclic stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117747895B_ABST
    Figure CN117747895B_ABST
Patent Text Reader

Abstract

The present invention discloses a hybrid membrane based on UiO66 modification, a preparation method and an application in a flow battery; the matrix of the hybrid membrane is doped with carbonized UiO‑66; further, the surface of the carbonized UiO‑66 is also modified with β‑CD. The cross section of the hybrid membrane is dense and uniform, and has good chemical stability under strong acid and strong oxidation conditions. And the carbonized UiO‑66 is doped into the matrix after being modified with β‑CD, and due to the interaction between the carbonized UiO‑66 and the matrix, the water absorption rate and tensile strength of the hybrid membrane are greatly improved compared with the membrane, and the swelling rate is significantly reduced. In addition, the all-vanadium flow battery assembled using the hybrid membrane has higher VE and EE.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a hybrid membrane based on UiO66 modification, a preparation method and application in a flow battery, and belongs to the technical field of hybrid membranes. Background Art

[0002] In order to overcome the intermittent and uncontrollable nature of renewable energy use, it is imperative to develop advanced large-scale energy storage technologies. Vanadium flow batteries (VFBs) have attracted much attention in the field of energy storage due to their fast response speed, flexible design, and long cycle life. Proton exchange membranes (PEMs) are one of the main components of VFBs. While conducting protons to form internal circuits, they also play a role in blocking active ions, which directly determines the performance of the battery. Ideal PEMs should have low active ion permeability, high proton conductivity, and good chemical stability. Currently, the most commonly used PEM is perfluorosulfonic acid Nafion membrane, but its disadvantages such as poor ion selectivity and high cost have greatly limited its further development. Therefore, it is necessary to develop new low-cost alternative membrane materials.

[0003] Proton-conducting sulfonated polyetheretherketone (SPEEK) membrane with small water channels is the most promising proton exchange membrane material. Although SPEEK can reduce membrane costs, its easy degradation in strong oxidizing and acidic media leads to poor cyclic stability in VFB. Metal-organic framework (MOFs) materials with regular and adjustable pores and large specific surface area have been used to modify SPEEK membranes, but the stability of MOFs in acidic environments restricts their practical application. Summary of the invention

[0004] In order to solve the deficiencies of the prior art, the present invention provides a hybrid membrane based on UiO66 modification, a preparation method and an application in a flow battery. The hybrid membrane has good chemical stability under strong acid and strong oxidation conditions.

[0005] The technical solution adopted by the present invention is:

[0006] A hybrid membrane based on UiO66 modification, wherein the hybrid membrane mainly comprises a polymer matrix doped with carbonized UiO-66.

[0007] The polymer matrix is ​​SPEEK.

[0008] Preferably, the surface of the carbonized UiO-66 is also modified with β-CD.

[0009] The above-mentioned method for preparing the hybrid membrane based on UiO66 modification comprises the following steps:

[0010] S1: preparing UiO-66 and carbonizing UiO-66;

[0011] S2: The carbonized UiO-66 is mixed with SPEEK to prepare a casting solution, and a film is prepared by a casting method.

[0012] Preferably, after step S1 and before step S2, a step of modifying the surface of the carbonized UiO-66 with β-CD is further included.

[0013] Preferably, in step S1, UiO-66 is prepared by a hydrothermal synthesis method, specifically, the method is: dissolving ZrCl4, terephthalic acid and acetic acid in DMF, mixing them evenly and then subjecting them to hydrothermal treatment; cooling after completion, centrifuging, washing and drying to obtain UiO-66;

[0014] Among them, the ratio of ZrCl4, terephthalic acid and acetic acid is: (180-200) mg: (120-140) mg: (8-12) g.

[0015] Preferably, in step S1, the specific method of carbonizing UiO-66 is: placing UiO-66 in a tubular furnace, under an argon atmosphere, gradually heating and keeping the temperature until the temperature reaches 550-650°C, and then annealing for 4-6 hours and then cooling.

[0016] Preferably, the specific method of surface β-CD modification of carbonized UiO-66 is: dissolving the carbonized UiO-66 in DMF, adding β-CD, stirring and filtering, and drying the filter residue;

[0017] Among them, the mass ratio of β-CD to carbonized UiO-66 is 1:(0.8-1.2).

[0018] Preferably, in step S2, the casting solution is prepared by: dispersing carbonized UiO-66 and SPEEK in DMF, and then ball milling after ultrasonication;

[0019] The amount of carbonized UiO-66 added is 1-4% of the amount of SPEEK added.

[0020] Preferably, in step S2, the specific method of forming the film by the casting method is: after the film is scraped on the scraper, it is preformed at 55-75°C for 5-7h, then dried at 90-110°C in vacuum for 11-14h, and the film is peeled off after cooling.

[0021] Application of any of the above-mentioned hybrid membranes modified based on UiO66 in all-vanadium liquid flow batteries.

[0022] The beneficial effects of the present invention are:

[0023] (1) The hybrid membrane has a dense and uniform cross-section and has good chemical stability under strong acid and strong oxidizing conditions.

[0024] (2) The interaction between β-CUiO-66 and SPEEK greatly improves the water absorption and tensile strength of the SPEEK / β-CUiO-66 hybrid membrane compared with the SPEEK membrane, and significantly reduces the swelling rate. In addition, the performance of membranes with different β-CUiO-66 contents is better than that of the SPEEK / CUiO-66 hybrid membrane with the corresponding doping ratio.

[0025] (3) The all-vanadium redox flow battery assembled using the S / β-CUiO-66-3% hybrid membrane has higher VE and EE than that of the SPEEK membrane and the S / CUiO-66-3% hybrid membrane. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The SEM and TEM images of UiO-66 and CUiO-66. a) SEM image of UiO-66; b) SEM image of CUiO-66; c) TEM image of UiO-66; d) TEM image of CUiO-66;

[0027] Figure 2 a) XRD pattern of UiO-66; b) XRD pattern of CUiO-66;

[0028] Figure 3 a) Full XPS spectrum of CUiO-66; bd) High-resolution XPS scans of Zr3d, C1s and O1s;

[0029] Figure 4 BET test diagrams of UiO-66 and CUiO-66. a) N2 adsorption-desorption isotherm of UiO-66; b) Pore size distribution of UiO-66; c) N2 adsorption-desorption isotherm of CUiO-66; d) Pore size distribution of CUiO-66;

[0030] Figure 5 CUiO-66 in a) 3M H2SO4 and b) vanadium-containing acidic electrolyte solution (1.5M VO2 + +3M H2SO4) after two days of immersion;

[0031] Figure 6 a) Surface SEM image of S / CUiO-66-x% membrane; b) cross-sectional SEM image (x = 1, 2, 3, 4 wt%);

[0032] Figure 7 SEM image of the CMOF / polymer interface in the S / CUiO-66-3% membrane;

[0033] Figure 8a) SEM image of the cross section of the S / UiO-66-3% membrane after being immersed in the electrolyte solution for 2 days; bd) SEM image of the surface, cross section and local magnification of the S / CUiO-66-3% membrane after being immersed in the electrolyte solution for 14 days;

[0034] Fig. 9 The water absorption and swelling properties of SPEEK membrane and S / CUiO-66-x% membrane (x = 1, 2, 3, 4 wt%);

[0035] Fig.10 Mechanical properties of SPEEK membrane and S / CUiO-66-x% membrane (x = 1, 2, 3, 4wt%);

[0036] Fig.11 is the proton transfer efficiency of SPEEK membrane and S / CUiO-66-x% membrane (x=1, 2, 3, 4wt%);

[0037] Fig.12 a) vanadium ion permeability of SPEEK membrane and S / CUiO-66-x% membrane; b) ion selectivity (x=1, 2, 3, 4wt%);

[0038] Fig.13 20-100mA cm -2 Performance diagram of all-vanadium redox flow battery of Nafion 212 membrane, SPEEK membrane and S / CUiO-66-3% membrane under current density;

[0039] Fig.14 For S / CUiO-66-3% film at 100 mA cm -2 Long cycle battery efficiency at current density;

[0040] Fig.15 a) 100 mA cm -2 Capacity retention of SPEEK membrane and S / CUiO-66-3% membrane under different current densities; b) SEM image of the cross section of the membrane after 500 charge and discharge cycles;

[0041] Fig.16 is the general structure of cyclodextrin;

[0042] Fig.17 is the SEM image of β-CUiO-66;

[0043] Fig.18 a) N2 adsorption-desorption curve and b) pore size distribution diagram of β-CUiO-66;

[0044] Fig.19 This is the SEM image of β-CUiO-66 after being immersed in 3M H2SO4 solution for two days;

[0045] Fig. 20 a) Surface SEM image of the hybrid membrane; b) cross-sectional SEM image (x = 1, 2, 3, 4 wt%);

[0046] Fig.21 The SEM image of the filler / polymer interface in the S / β-CUiO-66-3% membrane;

[0047] Fig. 22 a) Surface, b) cross section and c) local magnified SEM images of the S / β-CUiO-66-3% membrane after immersion in the electrolyte solution for 14 days;

[0048] Fig.23 The water absorption and swelling properties of SPEEK membrane and S / β-CUiO-66-x% membrane (x=1, 2, 3, 4wt%);

[0049] Fig.24 Mechanical properties of SPEEK membrane and S / β-CUiO-66-x% membrane (x = 1, 2, 3, 4wt%);

[0050] Fig.25 20-100mA cm -2 Performance diagram of all-vanadium redox flow battery of Nafion 212 membrane, SPEEK membrane and S / β-CUiO-66-3% membrane under current density;

[0051] Fig.26 20-100mA cm -2 Performance comparison of all-vanadium liquid flow batteries under different current densities. DETAILED DESCRIPTION

[0052] The present invention will be specifically described below in conjunction with the accompanying drawings and embodiments.

[0053] Example 1

[0054] Preparation of UiO-66

[0055] UiO-66 was prepared by hydrothermal synthesis. The specific experimental steps are as follows: 81.7 mL of DMF was added to a 250 mL beaker, 190.3 mg of ZrCl4, 133 mg of terephthalic acid and 9.6 g of acetic acid were weighed and dissolved in the above solution, stirred continuously at room temperature for 4 hours, and ultrasonicated for 20 minutes. After complete mixing, it was transferred to a 100 mL reactor and hydrothermally treated at 120 ° C for 24 hours. After cooling naturally to room temperature, centrifugation (10000 r / min, 5 min) was performed to collect UiO-66 nanocrystals, and then washed with excess DMF and methanol several times in turn to collect the white product. Finally, it was dried in an oven at 60 ° C overnight, and the obtained sample was recorded as UiO-66.

[0056] Preparation of Carbonized UiO-66 (CUiO-66)

[0057] Weigh a certain amount of UiO-66 powder, put it into a crucible and send it into a handheld tube furnace for direct carbonization under argon atmosphere. The carbonization process is as follows: first, at 5℃min -1 The heating rate was from 20℃ to 200℃, and kept at this temperature for 1h; then it was raised to 400℃ at the same rate, and kept at this temperature for 1h; finally, it was heated at 3℃min -1 The heating rate was raised to 600°C. After reaching the target temperature, annealing was performed at the target temperature for 5 h, and finally the temperature was naturally lowered. The obtained black powder was recorded as CUiO-66.

[0058] Preparation of SPEEK / CUiO-66 hybrid membrane

[0059] SPEEK / CUiO-66 hybrid membrane was prepared by solution casting. A certain amount of CUiO-66 was dispersed in 10mL DMF, and then 1.5g SPEEK was added to the CUiO-66 / DMF mixed solution, ultrasonicated for 30min, and ball milled for 24h to obtain a uniform casting solution. The casting solution was allowed to stand for a few minutes before scraping. After scraping the film on the scraper, the glass plate was placed in a 60℃ forced air drying oven for 6h for preforming, and then transferred to a 100℃ vacuum drying oven for 12h. Finally, the glass plate was cooled naturally and immersed in deionized water to peel off the membrane. The prepared hybrid membrane was immersed in 1M H2SO4 solution for 24h for activation, and then the membrane was stored in fresh deionized water for standby use. The corresponding hybrid membrane is recorded as S / CUiO-66-x%, where S represents SPEEK and x% represents the mass ratio of CUiO-66 to SPEEK (1-4wt%).

[0060] Characterization of materials

[0061] Morphology analysis

[0062] The morphologies of UiO-66 and CUiO-66 were compared by SEM and TEM characterization. Figure 1 As shown. The obtained UiO-66 has a regular octahedral structure, a smooth surface, and a uniform particle size of about 500nm. The morphology of the sample did not change after high-temperature carbonization, maintaining a highly symmetrical geometric shape, and the average particle size was reduced to about 400nm ( Figure 1 b area).

[0063] XRD characterization

[0064] The phase structures of the prepared samples (UiO-66 and CUiO-66) were analyzed by XRD. Figure 2As shown. UiO-66 has obvious characteristic diffraction peaks, which are consistent with the simulation data, indicating that UiO-66 crystals have been successfully synthesized and have good crystallinity. After carbonization, its characteristic peaks completely disappeared. The XRD spectrum of CUiO-66 is consistent with the XRD spectrum of ZrO2, indicating that the main component of CUiO-66 is ZrO2. In addition, the XRD of CUiO-66 found the diffraction peak of carbon (002) at 2θ=24°, confirming that a stable carbon structure was formed during the carbonization process.

[0065] XPS characterization

[0066] Figure 3 Figure 1 is the XPS spectrum of CUiO-66. From the overall spectrum, it can be seen that CUiO-66 is composed of C, O and Zr elements. In the C1s spectrum, CC, CO and C-OH peaks are displayed. Figure 3 The high-resolution scanning image of Zr3d elements in the c region shows that Zr3d 5 / 2 、Zr3d 3 / 2 And the characteristic peaks of ZrO2. Figure 3 The d region is a high-resolution XPS spectrum of O1s, and the three valence bond structures of O, ZrO2, H2O and OC=O, correspond to characteristic peaks at 530.0, 532.2 and 533.3 eV, respectively. The spectra of Zr3d and O1s containing ZrO2 peaks both indicate that ZrO2 is formed after carbonization, which is consistent with the XRD analysis results.

[0067] BET characterization

[0068] BET specific surface area and pore size distribution of UiO-66 and CUiO-66 Figure 4 The N2 adsorption-desorption curve of UiO-66 belongs to type I isotherm, and its pore size distribution is below 2nm, showing obvious micropore characteristics and a high specific surface area (1295.1m 2 g -1 The N2 adsorption-desorption isotherm of the carbonized material CUiO-66 is type IV, with an H3 type hysteresis loop in the relative pressure range of 0.4-0.9, and the specific surface area is reduced to 132.4 m 2 g -1 From the pore size distribution of CUiO-66, it can be seen that the pore size of the material increases and the distribution becomes wider after carbonization, which indicates that the original microporous structure is transformed into a mesoporous structure through carbonization. The mesoporous structure is more conducive to the entry and exit of protons, which may be beneficial to improving the mobility of protons.

[0069] Stability analysis

[0070] CUiO-66 was added into 3M sulfuric acid solution and vanadium-containing acid electrolyte solution (1.5M VO 2++3M H2SO4) and stored at room temperature for several days to verify its acid stability, and the microscopic morphology changes were observed by scanning electron microscopy. Figure 5 It can be seen that due to the stable structure of CUiO-66, its shape and size did not change significantly after immersion compared with UiO-66. Although there was electrolyte residue on the surface of the particles after immersion in the electrolyte, an obvious octahedral structure was still observed, which proved that CUiO-66 has good chemical stability in an acidic environment and can be used in the VFB system.

[0071] Basic characterization of SPEEK / CUiO-66 hybrid membrane

[0072] Morphology analysis

[0073] The surface and cross-sectional morphology of the membrane were characterized by scanning electron microscopy, and the quality and internal microstructure of the membrane were investigated. Figure 6 a region and Figure 6 Region b shows the surface and cross-sectional SEM images of the hybrid membrane. From the surface image, it can be seen that the hybrid membrane is dense, and there are obvious bulges compared with the surface of the SPEEK membrane. In the cross-sectional image, when the doping amount of CUiO-66 is 1-3wt%, the particles are evenly distributed in the SPEEK matrix. Further magnification reveals a good filler / polymer interface ( Figure 7 ), indicating that CUiO-66 and SPEEK have good compatibility, which is beneficial to improve the mechanical strength and stability of the membrane. When the doping amount is greater than 3wt%, the dispersion uniformity of the particles in the membrane becomes worse and slight agglomeration occurs.

[0074] Chemical stability analysis

[0075] The two hybrid membranes containing 3 wt% UiO-66 and CUiO-66 particles were prepared in a vanadium-containing electrolyte solution (1.5 M VO 2+ / 3M H2SO4) for different time periods, and the chemical stability of the membrane was studied by observing the morphological changes of the membrane. Figure 8 As can be seen in area a, after immersion for 48 hours, a large number of small holes were observed on the cross section of the S / UiO-66-3% membrane due to the falling of MOF particles. In contrast, the S / CUiO-66-3% membrane showed excellent structural stability: after immersion for up to 14 days, there were no defects or damage on the membrane surface, and evenly distributed CMOF particles and a good filler / polymer interface were still observed on the cross section ( Figure 8 bd area), which shows that the addition of CUiO-66 can improve the acid and oxidation resistance of the basement membrane.

[0076] Physicochemical properties of SPEEK / CUiO-66 hybrid membranes

[0077] Water absorption and swelling

[0078] Fig. 9 The figure shows the changes in the water absorption and swelling rate of the hybrid membrane with the CUiO-66 content in the membrane. As can be seen from the figure, CUiO-66 can increase the water absorption of the membrane. With the increase of CUiO-66 content, the water absorption of the composite membrane first increases and then decreases, reaching a maximum value (39.4%) at S / CUiO-66-2%, which is about 11.5% higher than that of the SPEEK membrane. At the same time, the swelling rate of CUiO-66 is lower than that of the SPEEK membrane, which is attributed to its rigid skeleton structure, which can inhibit the swelling of the SPEEK polymer chain to a certain extent.

[0079] Mechanical properties

[0080] Fig.10 This is a comparison chart of the mechanical properties of SPEEK membrane and SPEEK / CUiO-66 hybrid membrane. As the doping amount increases, the tensile strength of the hybrid membrane is higher than that of the SPEEK membrane. This is because hydrogen bonds are formed between the -SO3H groups in SPEEK and the -OH groups in the inorganic particles, which increases the mechanical stability of the membrane and improves the tensile strength. The S / CUiO-66-3% membrane has the highest tensile strength of 26.6Mpa. Although the tensile strength decreases when the addition amount of CUiO-66 is 4wt%, it is still higher than that of the SPEEK membrane, which shows that the introduction of CUiO-66 particles effectively improves the mechanical properties of the membrane and can ensure that the hybrid membrane will not be damaged during battery testing.

[0081] Proton transfer rate

[0082] An ideal proton exchange membrane should have a high proton transfer rate. As the CUiO-66 content increases, the proton transfer rate increases first and then decreases ( Fig.11 ), when the addition amount of CUiO-66 is 3wt%, the proton transfer rate reaches a maximum value of 0.079S cm -1 On the one hand, the pores of CUiO-66 provide additional channels for the transmission of protons, thereby improving the proton transfer rate. On the other hand, the hydroxyl groups in CUiO-66 can combine with protons to form hydrated protons through the on-board mechanism, thereby improving the proton conductivity of the membrane. This also further proves that the proton transfer rate of SPEEK-based membranes can be improved by adding carbonized materials.

[0083] Vanadium ion permeability and ion selectivity

[0084] The vanadium ion permeability and ion selectivity of SPEEK membrane and S / CUiO-66-x% (x=1, 2, 3, 4wt%) hybrid membrane are shown in the figure below. Fig.12It can be seen from region a that the hybrid membrane has good vanadium resistance, and the vanadium ion permeability of all membranes is lower than that of SPEEK membrane (8.14×10 -7 cm 2 min -1 ), and gradually decreases with the increase of doping amount. The vanadium ion permeability of S / CUiO-66-4% membrane is 5.06×10 -7 cm 2 min -1 It is worth noting that the vanadium ion permeation of SPEEK / CUiO-66 membrane is slightly higher than that of SPEEK / CZIF-8 membrane, which is due to the different prepared membrane thicknesses.

[0085] An ideal proton exchange membrane should have lower vanadium ion permeability and higher ion selectivity. Ion selectivity is used as an indicator to measure the comprehensive performance of the membrane. Fig.12 In region b, it is observed that the ion selectivity of the hybrid membrane is higher than that of the SPEEK membrane (0.71×10 5 S min cm -3 ), thanks to the higher proton transfer rate, the S / CUiO-66-3% membrane showed the best ion selectivity (1.51×10 5 S min cm -3 ), indicating that the membrane has a higher VE value than the SPEEK membrane in battery performance.

[0086] Performance and stability of all-vanadium redox flow batteries

[0087] In battery performance analysis, CE, VE and EE are three important factors to determine battery efficiency. The S / CUiO-66-3% hybrid membrane was installed in an all-vanadium liquid flow battery and its performance at 20-100 mA cm -2 The battery performance under current density is compared with Nafion212 membrane and SPEEK membrane. The results are as follows Fig.13 As shown. With the increase of current density, the CE of S / CUiO-66-3% membrane shows a linear increasing trend. This is because with the increase of current density, the time required for charge and discharge test decreases and the penetration of vanadium ions decreases. The CE of S / CUiO-66-3% membrane is higher than that of Nafion 212 membrane and SPEEK membrane, which indicates that the membrane has better vanadium barrier performance. The VE of the battery shows the opposite trend and decreases with the increase of current density. This is because voltage drop and concentration polarization will be generated during the test. The EE value has the same change as VE. The EE of SPEEK / CUiO-66-3% membrane is always higher than that of Nafion 212 membrane and SPEEK membrane. In addition, although the battery performance of S / CUiO-66-3% membrane is slightly lower than that of S / CZIF-8-3%, it is better at 100mA cm -2Under the current density, the S / CUiO-66-3% membrane still showed a higher efficiency than the SPEEK membrane (CE: 99.1%, VE: 82.9%, EE: 82.1%), which shows that the addition of CUiO-66 can improve the proton transfer rate of the membrane and reduce the vanadium ion permeability, thereby improving the battery performance.

[0088] The battery efficiency and cycle stability of proton exchange membranes in long-term charge and discharge cycles are also important factors in determining membrane performance. Fig.14 As shown, at 100mA cm -2 The long-cycle stability test of SPEEK membrane and S / CUiO-66-3% membrane was carried out under current density. It can be seen that compared with SPEEK membrane, the CE and VE of S / CUiO-66-3% membrane remained stable during the cycle, and still had 98.1% CE and 84.5% VE after about 500 charge and discharge cycles, and the EE of the hybrid membrane was always higher than that of SPEEK membrane.

[0089] Fig.15 Region a shows the SPEEK membrane and S / CUiO-66-3% membrane at 100 mA cm -2 Capacity retention rate after 300 cycles at the same current density. After 300 charge-discharge cycles, the S / CUiO-66-3% membrane has a high capacity retention rate of 82.3%, which is much higher than the SPEEK membrane, indicating that the hybrid membrane has a higher capacity retention ability than the SPEEK membrane. In addition, the cross-sectional morphology of the hybrid membrane after charge-discharge cycles was observed by SEM, and it was found that there were no cracks and other defects in the membrane ( Fig.15 b area), which indicates that the introduction of CUiO-66 nanoparticles can improve the structural and chemical stability of the membrane and enable stable operation in all-vanadium redox flow batteries.

[0090] Example 1 Acid-stabilized CUiO-66 was prepared, and SPEEK / CUiO-66 hybrid membrane was prepared by mixing it with SPEEK. The crystals and hybrid membranes before and after carbonization were characterized and their performances were analyzed. The main conclusions are as follows:

[0091] (1) SEM and other characterizations indicate the successful synthesis of UiO-66 and CUiO-66. In addition, CUiO-66 powder has good acid resistance in sulfuric acid solution and vanadium-containing electrolyte solution and can be used in all-vanadium liquid flow battery system.

[0092] (2) The hybrid membranes with different loading amounts are all dense, and CUiO-66 particles uniformly dispersed in the matrix and a good filler / polymer interface can be observed. In addition, the composite membranes have good chemical stability in acidic vanadium-containing electrolyte solutions.

[0093] (3) SPEEK / CUiO-66 hybrid membrane has enhanced water absorption and swelling, mechanical strength, and proton transfer rate. In particular, the proton transfer rate of S / CUiO-66-3% membrane is 0.079S cm -1 This is attributed to the porous structure of CUiO-66 and the rapid transport of protons through the on-board mechanism, which improves the proton transfer rate.

[0094] (4) In the all-vanadium flow battery test at different current densities, the S / CUiO-66-3% membrane showed higher CE, VE and EE than the Nafion212 membrane and SPEEK membrane. 100mA cm -2 The EE can reach 82.1% under the current density, and the long cycle test can stably cycle 500 times, with a capacity retention rate of 82.3%. After the cycle, the membrane morphology is kept good without obvious defects.

[0095] Example 2

[0096] The results of Example 1 show that the introduction of CUiO-66 can improve many physical and chemical properties of the original SPEEK membrane, but the hybrid membrane has a small improvement in water absorption and tensile strength, which may be due to the poor binding force between CUiO-66 and SPEEK and weak hydrophilicity. In order to further improve its performance, external hydrophilic, low-cost and environmentally friendly β-cyclodextrin (β-CD) was selected as a regulator to modify the surface of CUiO-66. Fig.16 It can be seen that the cyclodextrin molecule is rich in hydroxyl groups, which is conducive to enhancing the binding force between β-CUiO-66 and the SPEEK matrix. Based on this, Example 2 investigated the effect of β-cyclodextrin on the structure of CUiO-66 and compared the physical and chemical properties of the hybrid membrane before and after modification and the battery performance.

[0097] Preparation of β-CUiO-66

[0098] UiO-66 was prepared by hydrothermal synthesis. The specific experimental steps are as follows: 81.7 mL of DMF was added to a 250 mL beaker, 190.3 mg of ZrCl4, 133 mg of terephthalic acid and 9.6 g of acetic acid were weighed and dissolved in the above solution, stirred continuously at room temperature for 4 hours, and ultrasonicated for 20 minutes. After complete mixing, it was transferred to a 100 mL reactor and hydrothermally treated at 120 ° C for 24 hours. After cooling naturally to room temperature, centrifugation (10000 r / min, 5 min) was performed to collect UiO-66 nanocrystals, and then washed with excess DMF and methanol several times in turn to collect the white product. Finally, it was dried in an oven at 60 ° C overnight, and the obtained sample was recorded as UiO-66.

[0099] Weigh a certain amount of UiO-66 powder, put it into a crucible and send it into a handheld tube furnace for direct carbonization under argon atmosphere. The carbonization process is as follows: first, at 5℃min -1 The heating rate was from 20℃ to 200℃, and kept at this temperature for 1h; then it was raised to 400℃ at the same rate, and kept at this temperature for 1h; finally, it was heated at 3℃min -1 The heating rate was raised to 600°C. After reaching the target temperature, annealing was performed at the target temperature for 5 h, and finally the temperature was naturally lowered. The obtained product was recorded as CUiO-66.

[0100] A certain amount of CUiO-66 was weighed and dissolved in 10 mL of DMF, and then an equal amount of β-CD was weighed and added to the above solution. The mixed solution was stirred at room temperature for 30 min, and the black product was collected by filtration, and finally dried in an oven at 80°C overnight. The obtained product was recorded as β-CUiO-66.

[0101] Preparation of SPEEK / β-CUiO-66 hybrid membrane

[0102] The SPEEK / β-CUiO-66 hybrid membrane was prepared by solution casting method. The preparation method of the hybrid membrane was as follows: a certain amount of β-CUiO-66 was dispersed in 10mL DMF, and then 1.5g SPEEK was added to the β-CUiO-66 / DMF mixed solution, ultrasonicated for 30min, and ball milled for 24h to obtain a uniform casting solution. The casting solution was allowed to stand for a few minutes before scraping the membrane. After scraping the membrane on the scraper, the glass plate was placed in a 60℃ forced air drying oven for 6h for preforming, and then transferred to a 100℃ vacuum drying oven for 12h. Finally, the glass plate was cooled naturally and immersed in deionized water to peel off the membrane. The prepared hybrid membrane was immersed in 1M H2SO4 solution for 24h for activation, and then the membrane was stored in fresh deionized water for standby use. The obtained hybrid membrane was recorded as S / β-CUiO-66-x% (x=1, 2, 3, 4wt%).

[0103] Characterization of materials

[0104] Morphology analysis

[0105] The morphology of β-CUiO-66 samples was analyzed by SEM. Fig.17 After surface modification by cyclodextrin, the sample still has a regular octahedral structure, the particle size is more uniform, and the average particle size is reduced to about 300nm, which shows that the modification of β-cyclodextrin has no significant effect on the morphology of CUiO-66.

[0106] BET characterization

[0107] N2 adsorption-desorption curve and pore size distribution of β-CUiO-66 are shown in Fig.18As shown in the figure. From the results of N2 adsorption and desorption in Chapter 4, it can be seen that CUiO-66 has typical mesoporous structural characteristics. However, β-CUiO-66 retains the original porous structure, has no obvious mesopores, and has a significantly reduced N2 adsorption amount, with a significantly reduced specific surface area to 15.8 m 2 g -1 , the pore size is more concentrated, mainly distributed at 1.6nm.

[0108] Stability analysis

[0109] Similarly, β-CUiO-66 was immersed in 3M sulfuric acid solution for 48 h, and its morphology was observed by SEM. Fig.19 It can be clearly seen that after acid immersion, the morphology of β-CUiO-66 is not much different from that of the original sample, which indicates that β-CUiO-66 still has good acid resistance.

[0110] Characterization and analysis of SPEEK / β-CUiO-66 hybrid membrane

[0111] Morphology analysis

[0112] The surface and cross section of the hybrid membrane were observed by SEM. Fig. 20 In area a, it can be found that when the addition amount of β-CUiO-66 increases from 1wt% to 4wt%, the surface of the hybrid membrane is dense without any obvious wrinkles and phase separation. Fig. 20 In the cross-sectional diagram of region b, when the filler content is low, it is evenly dispersed in the hybrid membrane. When it exceeds 3wt%, obvious particle agglomeration occurs, and the dispersibility of β-CUiO-66 deteriorates, which is the same as the case of the S / CUiO-66 hybrid membrane. There is some collapse at the top of the cross-sectional diagram, which is caused by the quenching process in liquid nitrogen. A good matrix / filler bonding interface can be observed by zooming in on the cross section of the S / β-CUiO-66-3% membrane ( Fig.21 ).

[0113] Chemical stability analysis

[0114] The S / β-CUiO-66-3% membrane was added to an acidic electrolyte containing vanadium ions for a certain period of time to investigate its chemical stability in a strong acid and strong oxidizing environment. Fig. 22 As shown. Similar to the S / CUiO-66 membrane, after immersion in the electrolyte solution for 14 days, no significant defects were observed on the surface of the hybrid membrane, the β-CUiO-66 particles were still evenly dispersed in the membrane, and there were no cracks between the membrane and SPEEK. This shows that the modification of β-cyclodextrin did not change the acid and oxidation resistance of the original CUiO-66, and the prepared hybrid membrane has good chemical stability.

[0115] Water absorption and swelling

[0116] Fig.23 The figure shows the changes in the water absorption and swelling rate of the S / β-CUiO-66 hybrid membrane with the content of β-CUiO-66 in the membrane (the membrane is abbreviated as S / β-Cx%, x = 1, 2, 3, 4wt%). It can be clearly seen from the figure that the water absorption of the hybrid membrane is significantly improved by doping CUiO-66 modified with β-cyclodextrin, among which the water absorption of the S / β-C-3% membrane reaches 40.2%, which is 12.3% higher than that of the SPEEK membrane. Compared with the S / CUiO-66 membrane, the increase in water absorption increases with the increase in the doping amount of β-CUiO-66, and the S / β-C-4% membrane is about 4.6% higher than the S / CUiO-66-4% membrane, proving that the hydrophilic β-CUiO-66 has a promoting effect on the water absorption of the membrane. In addition, the swelling rate of the hybrid membrane is further reduced.

[0117] Mechanical properties

[0118] Fig.24 The mechanical properties of SPEEK membrane and S / β-CUiO-66 hybrid membrane are shown. As can be seen from the figure, the tensile strength of the hybrid membrane increases significantly with the increase of β-CUiO-66 content. When the mass fraction of β-CUiO-66 is 3wt%, the tensile strength increases to 29.6MPa. Secondly, compared with the SPEEK / CUiO-66 hybrid membrane, the tensile strength of the membrane is also improved. The good mechanical properties of the hybrid membrane are attributed to the interaction between SPEEK and β-CUiO-66, which effectively improves the rigidity of the membrane and makes it less likely to deform. This is related to Figure 5-8 On the other hand, the good compatibility between the SPEEK polymer and the β-CUiO-66 filler in the membrane ( Fig.21 ) also enhances the tensile strength of the membrane. Therefore, the hybrid membrane has stronger mechanical properties than the SPEEK membrane.

[0119] All-vanadium redox flow battery performance

[0120] Fig.25 The all-vanadium redox flow battery assembled with S / β-CUiO-66-3% hybrid membrane, Nafion 212 membrane and SPEEK membrane has a current of 20-100 mA cm -2 Efficiency curve under current density. Similar to the S / CUiO-66-3% hybrid membrane, the CE of the S / β-CUiO-66-3% membrane increases with the increase of current density, but the CE at all current densities is lower than that of the SPEEK membrane, and the CE of the membrane is mainly affected by VO 2+ The effect of the permeability indicates that β-CUiO-66 may not have the ability to improve the vanadium barrier performance of SPEEK-based membranes. The VE of the battery decreases with increasing current density, even at a current density of 100 mA cm-2 , VE also reached 86.0%. Compared with SPEEK membrane, VE is greatly improved, indicating that S / β-CUiO-66-3% membrane has higher proton transfer capacity. S / β-CUiO-66-3% membrane has higher EE, because the battery voltage drop increases at high current density, resulting in EE decreasing with increasing current density, while Nafion 212 membrane and SPEEK membrane decrease faster, 100mA cm -2 The EE of the hybrid membrane under current density is increased by about 8.0% and 8.5% compared with Nafion 212 membrane and SPEEK membrane, respectively.

[0121] In order to understand the difference in the effects of CUiO-66 and β-CUiO-66 on the performance of membrane batteries, the CE, VE and EE of S / CUiO-66-3% membrane and S / β-CUiO-66-3% membrane at the same current density were compared. Fig.26 As shown. On the one hand, the addition of β-CUiO-66 reduces the CE of the membrane, which is attributed to the fact that the large-mouth hollow pore size in β-CD is slightly larger than the diameter of the hydrated vanadium ions, causing the vanadium ions to enter the pores of CUiO-66 through its cavity, thereby reducing the vanadium barrier performance of the membrane. On the other hand, the VE of the hybrid membrane is improved relative to the hybrid membrane with CUiO-66 added, especially at high current density. This is because after CUiO-66 is surface-modified by β-CD molecules, the large number of -OH groups on it can form hydrogen bonds with water molecules, further accelerating proton transfer in the membrane. Therefore, the S / β-CUiO-66-3% membrane has higher battery performance at 100mA cm -2 The VE and EE at the current density were 86.0% and 85.0%, respectively, which were higher than 82.9% and 82.1% of the S / CUiO-66-3% membrane.

[0122] In this example, β-cyclodextrin-modified β-CUiO-66 was added to the SPEEK matrix to prepare a SPEEK / β-CUiO-66 hybrid membrane, and the hybrid membrane was characterized and the performance was tested. The conclusions are as follows:

[0123] (1) SEM characterization results show that the hybrid membrane has a dense and uniform cross-section and has good chemical stability under strong acid and strong oxidizing conditions.

[0124] (2) The interaction between β-CUiO-66 and SPEEK greatly improves the water absorption and tensile strength of the SPEEK / β-CUiO-66 hybrid membrane compared with the SPEEK membrane, and the swelling rate is significantly reduced. In addition, the performance of membranes with different β-CUiO-66 contents is better than that of the SPEEK / CUiO-66 hybrid membrane with the corresponding doping ratio. Taking the S / CUiO-66-3% membrane as an example: the water absorption rate increased by 2.6%, and the tensile strength increased by 3.1 MPa.

[0125] (3) The all-vanadium redox flow battery assembled with S / β-CUiO-66-3% hybrid membrane has higher VE and EE than SPEEK membrane and S / CUiO-66-3% hybrid membrane, 100 mA cm -2 The VE and EE at the current density were 86.0% and 85.0%, which were 8.5% and 2.9% higher than those of SPEEK membrane and S / CUiO-66-3% membrane.

[0126] The above is only a preferred implementation of the patent of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the patent of the present invention. These improvements and modifications should also be regarded as the scope of protection of the patent of the present invention.

Claims

1. A hybrid membrane based on UiO66 modification, characterized in that: The hybrid membrane includes a polymer matrix doped with carbonized UiO-66; the surface of the carbonized UiO-66 is also modified by β-CD; The polymer matrix is ​​SPEEK; The method for preparing the hybrid membrane based on UiO66 modification comprises the following steps: S1: preparing UiO-66 and carbonizing UiO-66; S2: The carbonized UiO-66 is mixed with a polymer matrix to prepare a casting solution, and a film is prepared by a casting method; After step S1 and before step S2, the method further includes modifying the surface of the carbonized UiO-66 with β-CD; The specific method of surface β-CD modification of carbonized UiO-66 is as follows: dissolving carbonized UiO-66 in DMF, adding β-CD, stirring and filtering, and drying the filter residue; Among them, the mass ratio of β-CD to carbonized UiO-66 is 1:(0.8-1.2); The amount of carbonized UiO-66 added is 1-3% of the amount of SPEEK added.

2. The hybrid membrane based on UiO66 modification according to claim 1, characterized in that In step S1, UiO-66 is prepared by a hydrothermal synthesis method, specifically, ZrCl4, terephthalic acid, and acetic acid are dissolved in DMF, mixed evenly, and then subjected to hydrothermal treatment; after the completion, the mixture is cooled, centrifuged, washed, and dried to obtain UiO-66; Among them, the ratio of ZrCl4, terephthalic acid and acetic acid is: (180-200) mg: (120-140) mg: (8-12) g.

3. The hybrid membrane based on UiO66 modification according to claim 1, characterized in that In step S1, the specific method of carbonizing UiO-66 is: placing UiO-66 in a tubular furnace, under an argon atmosphere, gradually heating and keeping the temperature until the temperature reaches 550-650°C, and then annealing for 4-6 hours and then cooling.

4. The hybrid membrane based on UiO66 modification according to claim 1, characterized in that In step S2, the casting solution is prepared by dispersing the carbonized UiO-66 and SPEEK in DMF, and then ball milling after ultrasonication.

5. The hybrid membrane based on UiO66 modification according to claim 1, characterized in that: In step S2, the specific method of forming the film by the casting method is: after the film is scraped on the scraper, it is preformed at 55-75° C. for 5-7 hours, then dried at 90-110° C. for 11-14 hours under vacuum, and the film is peeled off after cooling.

6. Use of the hybrid membrane modified based on UiO66 as described in any one of claims 1-2 in all-vanadium liquid flow battery.