Semi-aromatic copolymer polyamide, semi-aromatic polyamide composition and preparation method and application thereof

By copolymerizing composite short-chain diamines and terephthalic acid in semi-aromatic nylon materials, introducing long-chain diamines and cyclic polymers, and combining them with thermally stable hydrolysis-resistant and alcoholysis-resistant masterbatch, a high-performance The semi-aromatic polyamide composition with glass transition temperature and good processing properties solves the problem of insufficient resistance of existing materials to ethylene glycol and high temperature, and achieves improvements in high strength and thermal oxygen aging resistance.

CN117777435BActive Publication Date: 2024-10-25SHANGHAI BEIGANG NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311060645.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-22
Publication Date
2024-10-25
Estimated Expiration
2043-08-22

AI Technical Summary

Technical Problem

Existing semi-aromatic nylon materials have insufficient resistance to ethylene glycol and high temperatures, especially poor performance in long-term thermal oxygen aging and aqueous solutions, making it difficult to meet the needs of automotive cooling systems for heat resistance, hydrolysis resistance and chemical resistance.

Method used

It adopts polycondensation of composite short-chain diamine and terephthalic acid, introduces long-chain diamine and cyclic polymer, and prepares semi-aromatic copolymer polyamide through copolymerization and melt extrusion process, combined with thermal stability, hydrolysis resistance and alcohol decomposition resistance. particles, forming a semi-aromatic polyamide composition with a high glass transition temperature and good processing properties.

Benefits of technology

It achieves high strength and thermal oxygen aging resistance when the material is in contact with ethylene glycol for a long time at high temperature. The tensile strength retention rate is greater than 50%, and it maintains good tensile strength after being immersed in a 130°C ethylene glycol-water mixture. Strength, significantly improving the material's water resistance and ethylene glycol aqueous solution resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
  • Figure BDA0004407706790000021
    Figure BDA0004407706790000021
Patent Text Reader

Abstract

The present invention relates to the field of polymer material preparation, and in particular to a semi-aromatic copolymer polyamide, a semi-aromatic polyamide composition, and a preparation method and application thereof. The raw materials of the semi-aromatic copolymer polyamide include the following components by weight: (a1) 30 to 65 parts by weight of 6T units (a2) 30 to 60 parts by weight of 4T units, 5T units or M5T units; (a3) ​​0 to 15 parts by weight of 9T units, 10T units, or 12T units; (a4) 0 to 3 parts by weight of cyclic polymer units; wherein the sum of components (a1) to (a4) constitutes 100 parts by weight of the semi-aromatic copolymer polyamide. Further, after the semi-aromatic copolymer polyamide and the heat-stable hydrolysis-resistant and alcoholysis-resistant masterbatch are melt-extruded, a semi-aromatic polyamide composition with better high temperature resistance, ethylene glycol solution resistance, long-term thermal oxidation aging resistance and processing performance is prepared, and the prepared parts can be in contact with ethylene glycol for a long time at high temperature and maintain high strength, especially in the automotive field.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of polymer material preparation, and in particular to a semi-aromatic copolymer polyamide, a semi-aromatic polyamide composition, and a preparation method and application thereof. Background Art

[0002] Semi-aromatic nylon is widely used in the automotive, LED and electrical and electronic fields due to its excellent high temperature resistance and mechanical properties. Among them, the water pipe joints in automotive parts require the parts to have high strength and hot water resistance; the intake manifold, injector and throttle module of the intake module use semi-aromatic nylon because of its excellent heat resistance and chemical resistance; the cooling system water chamber, inlet (outlet) fasteners, and control valves pay more attention to the heat resistance, hot water resistance and coolant resistance of the material itself. The coolant is mainly composed of ethylene glycol and water. Improved semi-aromatic nylon can be used in many application scenarios that are in direct contact with ethylene glycol.

[0003] CN111117230A discloses a case of PA56 composition being used for resistance to automobile coolant. Even after being compounded with PA513 or PA514, the tensile strength is only 71-91 MPa after being soaked in ethylene glycol for 48 hours. At the same time, the composition based on PA56 does not have the property of high temperature resistance. CN111117233A discloses an unsaturated anhydride-olefin copolymer based on PA56. The tensile strength retention rate of the composition after soaking in ethylene glycol can only reach 40%. Based on the high water absorption of PA56 itself, it is difficult to achieve good ethylene glycol resistance even after being composite-modified with long-chain nylon and graft-modified olefin polymer blends.

[0004] The resin used in the example of CN103732653A is based on a PA5T / 6T composition, and does not involve use cases of hydrolysis resistance and coolant resistance. CN114920926A discloses PA5T / XT (X<=6), which is used for automotive cooling system pipe parts. The tensile strength retention rate after hydrolysis at 80°C is only 60-70%. CN119928665 discloses PA5T / 512, but does not involve the introduction of other monomers to improve its high water absorption, and the temperature resistance decreases after the introduction of aliphatic copolymers, especially in terms of glass transition temperature. The glass transition temperature is reported as a key indicator of coolant-resistant materials by EP3222649 (CN107325548A). Summary of the invention

[0005] In view of the above-mentioned shortcomings of the prior art, the purpose of the present invention is to provide a semi-aromatic copolymer polyamide that is resistant to solvents and heat and oxygen aging, a semi-aromatic polyamide composition, and a preparation method and application thereof. The semi-aromatic polyamide composition or a product prepared by the index method thereof can be applied to the automotive field, especially to cooling systems with direct contact / indirect contact of ethylene glycol-water mixture (1:1), to solve the problems in the prior art.

[0006] To achieve the above objectives and other related objectives, the present invention is achieved through the following technical solutions.

[0007] In one aspect, the present invention provides a semi-aromatic copolymer polyamide, wherein the raw materials of the semi-aromatic copolymer polyamide include the following components by weight:

[0008] (a1) 30 to 65 parts by mass of 6T units; (a2) 30 to 60 parts by mass of 4T units, 5T units or M5T units;

[0009] (a3) 0 to 15 parts by mass of 9T units, 10T units, or 12T units; (a4) 0 to 3 parts by mass of cyclic multimer units; wherein the sum of components (a1) to (a4) constitutes 100 parts by mass of the semi-aromatic copolymer polyamide;

[0010]

[0011] The second aspect of the present invention provides a semi-aromatic polyamide composition, wherein the raw materials of the composition include the following components by weight:

[0012] Component A: 40-65 parts by weight of the semi-aromatic copolymer polyamide as described in the first aspect of the present invention;

[0013] Component B: 3-15 parts by weight of heat-stable, hydrolysis-resistant and alcoholysis-resistant masterbatch;

[0014] Component C: 30-60 parts by mass of reinforcing material and / or filler;

[0015] Component D: 0-2 parts by mass of heat stabilizer;

[0016] Component E: 0-5 parts by weight of auxiliary agents and / or additives;

[0017] The total of component A to component E constitutes 100 parts by mass.

[0018] The third aspect of the present invention provides a method for preparing the semi-aromatic polyamide composition according to the second aspect of the present invention, comprising the following steps:

[0019] S1: Components (a1) to (a4) are mixed and subjected to salt formation, prepolymerization and post-polymerization processes to obtain component A;

[0020] S2: After component A and component E are fully mixed, they are extruded and granulated.

[0021] The fourth aspect of the present invention provides a semi-aromatic polyamide composition prepared by the method for preparing the semi-aromatic polyamide composition according to the third aspect of the present invention.

[0022] The fifth aspect of the present invention provides use of the semi-aromatic polyamide composition according to the second aspect of the present invention in preparing a component that is in direct or indirect contact with an ethylene glycol-water coolant.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] The high temperature resistant semi-aromatic copolymer polyamide is formed by polycondensation of composite short-chain diamine and terephthalic acid, and long-chain diamine and terephthalic acid can be optionally introduced for copolymerization, and cyclic polymer units (such as cyclic dimer, trimer or tetramer units, etc.) can be further optionally added for polymerization. Further, after the semi-aromatic copolymer polyamide and the heat-stable hydrolysis-resistant and alcoholysis-resistant masterbatch are melt-extruded, in this application, through the synergistic effect of each component, a semi-aromatic polyamide composition (i.e., semi-aromatic copolymer high temperature resistant nylon) with better high temperature resistance, ethylene glycol solution resistance, long-term thermal oxidation aging resistance and processing performance is prepared. Its glass transition temperature is controllable, and the processing melt fluidity is good, which has obvious advantages in preparing high-filled composite materials or manufacturing complex parts. In addition, the polymerization conditions of the present invention are mild, the equipment is simple, the product performance is excellent, it is simple and easy to operate, and the application field is broad.

[0025] The material has good resistance to heat and oxygen aging. After 500h of heat and oxygen aging at 170℃, the tensile elongation at break is higher than 1.3%. At the same time, the material has good resistance to ethylene glycol aqueous solution. After being immersed in ethylene glycol-water mixture at 130℃ for 1008h, the elongation at break is greater than or equal to 1.8%, and the tensile strength reaches more than 140MPa. DETAILED DESCRIPTION

[0026] The applicant of the present invention has discovered through experiments that the main body is copolymerized with composite short-chain diamines (for example, 1,4-butanediamine, 1,5-pentanediamine, 2-methylpentanediamine and 1,6-hexanediamine in proportion) and terephthalic acid, and long-chain diamines (for example, 1,9-nonanediamine, 1,10-decanediamine, 1,12-dodecanediamine, etc.) and cyclic dimers are introduced at the same time. This can adjust the flexibility of the chain segment, improve the processability, achieve high rigidity and high heat resistance of the product, while retaining the high crystallinity of the semi-aromatic nylon, and then the mechanical properties and chemical resistance of the composite reinforced material can be improved with more reinforcing materials, and the thermally stable, hydrolysis-resistant and alcoholysis-resistant masterbatch can be blended and melt-extruded. Through the synergistic effect of each component, the composition can still maintain good tensile strength after being immersed in a 130°C ethylene glycol-water mixture (1:1) for 1008 hours, and the tensile strength retention rate is above 50%, which increases the water resistance and ethylene glycol aqueous solution resistance of the material, and finally prepares a semi-aromatic copolymer high-temperature nylon composition with high filling, excellent heat-oxidative aging resistance, ethylene glycol aqueous solution resistance and better processing performance. The prepared parts can maintain high strength when in contact with ethylene glycol for a long time at high temperature, especially in the automotive field. And on this basis, the present invention is completed.

[0027] Half Aromatic copolymer polyamide

[0028] The first aspect of the present invention provides a semi-aromatic copolymer polyamide, which comprises, by weight: (a1) 30 to 65 parts by weight of 6T units; (a2) 30 to 60 parts by weight of 4T units, 5T units or M5T units; (a3) ​​0 to 15 parts by weight of 9T units, 10T units or 12T units; (a4) 0 to 3 parts by weight of cyclic polymer units; wherein the sum of components (a1) to (a4) constitutes 100 parts by weight of the semi-aromatic copolymer polyamide.

[0029] In the semi-aromatic copolymer polyamide provided by the present invention, the 6T unit, 4T unit, 5T unit, M5T unit, 9T unit, 10T unit, 11T unit, and 12T unit are as follows:

[0030]

[0031] In the semi-aromatic copolyamide provided by the present invention, the mass fraction of the semi-aromatic copolyamide in component (a1) can be 30-40 mass fractions, 40-50 mass fractions or 50-65 mass fractions, etc. The 6T unit is formed by 1,6-hexamethylenediamine and terephthalic acid.

[0032] In the semi-aromatic copolyamide provided by the present invention, the mass fraction of the semi-aromatic copolyamide in component (a2) can be 30-40 mass fractions, 40-50 mass fractions or 50-60 mass fractions. The 4T unit is formed by 1,4-butylene diamine and terephthalic acid. The 5T unit is formed by 1,5-pentane diamine and terephthalic acid. The M5T unit is formed by 2-methyl-pentane diamine and terephthalic acid.

[0033] In the semi-aromatic copolymer polyamide provided by the present invention, the component (a3) ​​can be selected from 0-5 parts by mass, 0-1 parts by mass, 1-5 parts by mass, 5-10 parts by mass or 10-15 parts by mass, etc. The 9T unit is formed by 1,9-nonanediamine and terephthalic acid; the 10T unit is formed by 1,10-decanediamine and terephthalic acid; the 12T unit is formed by 1,12-dodecanediamine and terephthalic acid.

[0034] In the semi-aromatic copolyamide provided by the present invention, the component (a4) can be selected to be 0-1 mass part, 1-2 mass parts or 2-3 mass parts, etc., based on the mass part of the semi-aromatic copolyamide.

[0035] In the semi-aromatic copolymer polyamide provided by the present invention, the cyclic polymer unit is selected from a combination of one or more of a cyclic dimer unit (1), a cyclic trimer unit (2) or a cyclic tetramer unit (3); preferably, the cyclic polymer unit is one or more of the following structures:

[0036]

[0037] Semi-aromatic polyamide composition

[0038] The second aspect of the present invention provides a semi-aromatic polyamide composition, wherein the raw materials of the composition include the following components by weight:

[0039] Component A: 40-65 parts by weight of the semi-aromatic copolymer polyamide as described in the first aspect of the present invention;

[0040] Component B: 3-15 parts by weight of heat-stable, hydrolysis-resistant and alcoholysis-resistant masterbatch;

[0041] Component C: 30-60 parts by mass of reinforcing material and / or filler;

[0042] Component D: 0-2 parts by mass of heat stabilizer;

[0043] Component E: 0-5 parts by weight of auxiliary agents and / or additives;

[0044] Preferably, when the raw materials of the composition include component A to component E, the sum of component A to component E constitutes 100 parts by mass.

[0045] In the semi-aromatic polyamide composition provided by the present invention, component A can be selected from 40-50 parts by mass, 50-65 parts by mass, 40-45 parts by mass, 45-50 parts by mass, 50-55 parts by mass, 55-60 parts by mass or 60-65 parts by mass, etc., based on the mass parts of the semi-aromatic polyamide composition.

[0046] In the semi-aromatic polyamide composition provided by the present invention, in component B, the heat-stable hydrolysis-resistant and alcoholysis-resistant masterbatch is selected from polyamide, hydrolysis-resistant agent, copper salt heat stabilizer and lubricant, wherein the polyamide is selected from the semi-aromatic copolyamide PA6T / 66. The hydrolysis-resistant agent is selected from one or more combinations of monomeric carbodiimide hydrolysis-resistant agent, polymeric carbodiimide hydrolysis-resistant agent and liquid carbodiimide hydrolysis-resistant agent, preferably high polymer carbodiimide;. The copper salt stabilizer is selected from any one of copper chloride, copper bromide, copper iodide and copper phosphate, preferably copper iodide. The lubricant is selected from any one of carboxylic acid calcium salt with a long carbon chain as the main component, vinyl bisstearamide EBS, TAF, silicone powder and pentaerythritol stearate, preferably carboxylic acid calcium salt with a long carbon chain as the main component, and the trade name is CAV102.

[0047] The mass ratio of polyamide, anti-hydrolysis agent, copper salt heat stabilizer and lubricant is 85-90: 5-10: 2-6: 0.2-1.0.

[0048] In the semi-aromatic polyamide composition provided by the present invention, component (B) can be selected to be 3-8 parts by mass, 3-5 parts by mass, 5-10 parts by mass or 10-15 parts by mass, etc., based on the mass parts of the semi-aromatic polyamide composition.

[0049] In the semi-aromatic polyamide composition provided by the present invention, the component C is selected from a combination of one or more of glass fiber, carbon fiber, talcum powder and mica flakes.

[0050] In the semi-aromatic polyamide composition provided by the present invention, component C can be selected to be 30-40 parts by mass, 40-50 parts by mass or 50-60 parts by mass, etc., based on the mass parts of the semi-aromatic polyamide composition.

[0051] In the semi-aromatic polyamide composition provided by the present invention, in component D, the heat stabilizer is selected from a combination of one or more of hindered phenol stabilizers, phosphite stabilizers, hindered amine stabilizers, triazine stabilizers, sulfur-containing stabilizers, and inorganic phosphorus-containing stabilizers. The above stabilizers can be used alone or in combination.

[0052] In the semi-aromatic polyamide composition provided by the present invention, component D can be selected from 0-0.005 mass parts, 0.005-2 mass parts, 0.005-1 mass parts or 1-2 mass parts, etc., based on the mass parts of the semi-aromatic polyamide composition.

[0053] In the semi-aromatic polyamide composition provided by the present invention, component E includes one or more combinations of lubricants, nucleating agents, antistatic agents, release agents, flow-improving aids, etc. Among them, the lubricant is selected from one or more combinations of carboxylic acid calcium salts (trade name such as CAV102) with long carbon chains as the main component, vinyl bis stearamide EBS, TAF, silicone powder, pentaerythritol stearate, etc. The nucleating agent is selected from one or more combinations of P22, P32, LH-501, HK-145, etc. The antistatic agent is selected from one or more combinations of conductive carbon black, graphene and carbon nanotubes. The release agent is selected from zinc stearate, stearic acid, paraffin, silicone oil, etc. The flow-improving aid is selected from one or more combinations of stearic acid, nano-silicon dioxide, talcum powder and glass microbead powder, etc.

[0054] In the semi-aromatic polyamide composition provided by the present invention, component E can be selected from 0-2 parts by weight, 0-1 parts by weight, 1-2 parts by weight or 2-5 parts by weight, etc., preferably 0-2 parts by weight.

[0055] The semi-aromatic polyamide composition provided by the present invention has good long-term heat resistance. The polyamide particles are tested using differential scanning calorimetry (DSC). At a heating rate of 10°C / min, the glass transition temperature is in the range of 120°C-170°C, preferably in the range of 130°C-170°C, and particularly in the range of 135°C-170°C.

[0056] The semi-aromatic polyamide composition has good heat-oxidative aging resistance. After aging at 170° C. for 500 hours, the tensile strength retention rate is greater than or equal to 70%, preferably greater than or equal to 75%; more preferably greater than or equal to 75% and less than 100%.

[0057] In addition, the material has good resistance to ethylene glycol-water mixture (1:1). After being immersed in the ethylene glycol-water mixture at 130°C for 1008 hours, the elongation at break is greater than or equal to 1.5%, preferably greater than or equal to 1.8%, and more preferably 1.8%-3.4%.

[0058] Method for preparing semi-aromatic polyamide composition

[0059] The third aspect of the present invention provides a method for preparing the semi-aromatic polyamide composition according to the second aspect of the present invention, comprising the following steps:

[0060] S1: Components (a1) to (a4) are subjected to salt formation, prepolymerization and post-polymerization processes to obtain component A;

[0061] S2: After component A and component E are fully mixed, they are extruded and granulated.

[0062] In step S1, the salt formation (a1) to (a4) and the prepolymerization are completed in the same pressure reaction vessel.

[0063] In the step S1, the monomers described in (a1)-(a4) and an appropriate amount of water are subjected to a salt-forming reaction in a first temperature section, and a prepolymerization reaction is carried out in a second temperature section; wherein the amount of water added for the salt-forming and prepolymerization is 0-30wt.%, preferably 1-20wt.%; the first temperature section for the salt-forming is 150°C-190°C, preferably 170°C-180°C; the second temperature section for the polymerization is 200°C-280°C, preferably 220°C-270°C; the pressure reaction vessel is a conventional vertical reactor, horizontal reactor, rotary drum or other pressure polymerization equipment; the stirring equipment is an anchor type, frame type or screw ribbon type stirrer.

[0064] Specifically, in component (a1), the raw materials of the 6T unit include 1,6-hexanediamine and terephthalic acid; in component (a2), the raw materials of the 4T unit include 1,4-butanediamine and terephthalic acid; in component (a2), the raw materials of the 5T unit include 1,5-pentanediamine and terephthalic acid; in component (a2), the raw materials of the M5T unit include 2-methyl-pentanediamine and terephthalic acid; in component (a3), the raw materials of the 9T unit include 1,9-nonanediamine and terephthalic acid; the raw materials of the 10T unit include 1,10-decanediamine and terephthalic acid; the raw materials of the 12T unit include 1,12-dodecanediamine and terephthalic acid. In component (a4), the cyclic multimer unit is selected from a combination of one or more of a cyclic dimer unit (1), a cyclic trimer unit (2) or a cyclic tetramer unit (3); preferably, the cyclic multimer unit is one or more of the following structures:

[0065]

[0066] In the step S1, after the polymerization is completed, the material is discharged and crushed, and the size of the crushed particles is ≤3 mm. The crushed material is solid-phase polymerized (specifically, for example, transferred to a solid-phase polymerization kettle for post-polymerization), and the post-polymerization temperature is 220-280° C., preferably 230-260° C. The post-polymerization pressure is less than 400 Pa, preferably ≤50 Pa, and the copolymer component A is obtained by viscosity enhancement.

[0067] In the step S2, component A-component E are dispersed at high speed (for example, in a high-speed disperser) and fully mixed, and then extruded and granulated at a higher processing temperature. Optionally, component A and component B are preliminarily mixed in a high mixer, and then blended with component D and component E in a high mixer, component C is added through a side feed port, and after being fully mixed, extruded and granulated at a high processing temperature, the extruder temperature and speed are 100 to 350 rpm (the speed can also be, for example, 150 to 350 rpm, 100 to 150 rpm, 150 to 250 rpm, 250 to 350 rpm, etc.), and the temperature of each section of the extruder is 210 ℃~230℃, 270℃~290℃, 300℃~310℃, 310℃~330℃, 320℃~340℃, 330℃~350℃, 330℃~350℃, 320℃~340℃, 310℃~330℃ (preferably 220℃, 280℃, 310℃, 320℃, 330℃, 340℃, 340℃, 330℃, 320℃), after melt plasticization, extrusion and pelletization to obtain a semi-aromatic composition.

[0068] The semi-aromatic polyamide composition can further be prepared by using the preparation method of the semi-aromatic polyamide composition described in the third aspect of the present invention.

[0069] application

[0070] The fourth aspect of the present invention provides use of the semi-aromatic polyamide composition according to the second aspect of the present invention in preparing a component that is in direct or indirect contact with an ethylene glycol-water solution.

[0071] Specifically,

[0072] Parts that are directly in contact with glycol-water solutions by injection molding, extrusion or blow molding, or parts that are indirectly in contact with glycol, and have a chemical-resistant coating on their surfaces. In particular, the following automotive coolant manifolds, coolant fluid lines, water inlets and outlets, thermostats, coolers, cooling water tanks, pumps, valves and connectors in coolant circuits or assemblies of these parts, or in the form of fuel lines, hydraulic lines, brake lines, clutch lines, urea lines or brake fluid tanks or fuel tanks.

[0073] The following is a description of the implementation of the present invention by means of specific embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification.

[0074] Before further describing the specific embodiments of the present invention, it should be understood that the scope of protection of the present invention is not limited to the specific embodiments described below; it should also be understood that the terms used in the examples of the present invention are intended to describe specific embodiments, rather than to limit the scope of protection of the present invention. The test methods in the following examples without specifying specific conditions are generally carried out under conventional conditions or under conditions recommended by the manufacturers.

[0075] When the embodiments give numerical ranges, it should be understood that, unless otherwise specified in the present invention, both endpoints of each numerical range and any numerical value between the two endpoints can be selected. Unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those generally understood by those skilled in the art. In addition to the specific methods, equipment, and materials used in the embodiments, according to the grasp of the prior art by those skilled in the art and the record of the present invention, any methods, equipment, and materials of the prior art similar or equivalent to the methods, equipment, and materials described in the embodiments of the present invention can also be used to realize the present invention.

[0076] 1. Test Standards

[0077] (1) Tensile and bending test conditions: The tensile strength and elongation at break were determined by placing the tensile specimens in a constant temperature and humidity chamber (25°C, RH = 50%) for 24 hours, using a testing machine for testing, with a tensile speed of 5 mm / min, and the test standard was ISO 527-1 / -2:2019. The bending strength test was performed by placing the bending specimens in a constant temperature and humidity chamber for 24 hours, using a testing machine for testing, and the test standard was ISO178:2019.

[0078] (2) Water absorption test conditions: The test sample was dried in an oven at 100°C, cooled in the oven, and the tensile specimen was immersed in water at 95°C for 336 hours. After the surface moisture was wiped off with cotton cloth, the weight increase percentage relative to the initial weight was measured. Test standard ISO 62:2008.

[0079] (3) Relative viscosity: The test sample was dissolved in 98% concentrated sulfuric acid at a concentration of 0.01 g / mL, the test temperature was 25° C., and the test standard was ISO 307:2019.

[0080] (4) Melting point and glass transition temperature test conditions: Weigh 5-8 mg of polymer particles. Under nitrogen protection, heat the sample to 350°C for 3 min, then cool to 50°C, and then heat to 350°C. The heating and cooling rates are both 10°C / min. Test standard ISO11357-3:2018.

[0081] (5) Test of hydrolysis stability of coolant: Ethylene glycol stability is determined according to GM standard GMW16360 (2016). The tensile specimens are treated in a pressure vessel filled with a 130°C ethylene glycol-water mixture (1:1) for 504 hours or 1008 hours. After treatment, the specimens are cooled to 23°C in the coolant, taken out of the coolant, rinsed with water, and subjected to tensile test after being fully dried and humidified.

[0082] 2.Raw materials

[0083] (1) Aliphatic diamines:

[0084] 1,6-Hexanediamine: INVISTA Nylon Chemical Co., Ltd.

[0085] 1,5-Pentanediamine: Cathay Biomaterials Co., Ltd.

[0086] 1,10-Decanediamine: Shandong Chiyue Chemical Co., Ltd.

[0087] (2) Aromatic diacids:

[0088] Terephthalic acid: Sinopec Yangzi Petrochemical Co., Ltd.

[0089] (3) Dimer:

[0090] Caprolactam cyclic dimer: Shanghai Myril Biochemical Technology Co., Ltd.

[0091] (4) Preparation method of heat-stable hydrolysis-resistant and alcoholysis-resistant masterbatch

[0092] The following raw materials are mixed and melt-extruded, and the raw materials include, by mass fraction: 85%-90% of polyamide PA6T / 66, 5%-10% of high-polymer carbodiimide (STABILIZER 4000 of PUZHAN), 2%-6% of cuprous iodide, and 0.2%-0.5% of lubricant Licomont CaV102.

[0093] (5) Fiber-like reinforcement materials

[0094] Glass fiber: Chongqing glass fiber, brand ECS301HP-3-H, Chongqing International Composite Materials Co., Ltd., average fiber diameter 10μm, average fiber length 3μm, excellent resistance to freezing liquid, excellent high temperature resistance.

[0095] (6) Heat stabilizer: antioxidant

[0096] AO-1: 1098 and 608 compound antioxidant, mass ratio is 2:3.

[0097] 1098: N,N'-(Hexane-1,6-diyl)bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamide], BASF.

[0098] 608: Bis(2,4-dicumylphenyl)pentaerythritol diphosphite, Qitai Technology Co., Ltd.

[0099] (7) Lubricant

[0100] Licomont CaV102: Calcium salt of carboxylic acid with long carbon chain as main component, Clariant.

[0101] PETS: Pentaerythritol Stearate, P, Lonza

[0102] Other raw materials used in the present invention are all commercially available products.

[0103] Example 1

[0104] Synthesis of PA6T / 5T / 10T / dimer copolymer: 4113g hexamethylenediamine, 3806g pentamethylenediamine, 1908g decanediamine, 13922g terephthalic acid, 484g caprolactam cyclic dimer, 154g benzoic acid, 3.1g sodium hypophosphite and 1346g water were added to a pressure reactor equipped with a magnetic coupler for stirring. The high-pressure reactor was replaced with nitrogen and filled with high-purity nitrogen as a protective gas. It was heated to 180°C within 1 hour under stirring for salt formation reaction. After 1 hour of reaction, the reaction mixture was heated to 250°C, and the reaction was reacted at a constant temperature of 250°C and a constant pressure of 2.5MPa for 2 hours. The water was discharged by pressure relief to keep the pressure in the reactor constant. After the reaction was completed, the material was discharged, and the prepolymer was vacuum dried at 80°C for 24 hours to obtain a prepolymer. The prepolymer was crushed and solid phase thickened in a vacuum drum at 260°C and 50 Pa to obtain a PA6T / 5T / 10T / dimer copolymer. The copolymer had a melting point of 305°C, a glass transition temperature of 141°C, and a relative viscosity of 2.45.

[0105] Preparation of ethylene glycol high temperature resistant polyamide mixture: 23.75kg PA6T / 5T / 10T / dimer copolymer, 5.48kg heat stable hydrolysis resistant alcoholysis resistant masterbatch, lubricant and other additives were mixed at a high speed of 150rpm, extruded through a twin screw, and glass fiber was added from the side feed port. The temperature of each section of the extruder was 220℃, 280℃, 310℃, 320℃, 330℃, 340℃, 340℃, 330℃, 320℃, and after melt plasticization, extrusion and pelletization, the semi-aromatic polyamide composition PA-1 was obtained.

[0106] The preparation methods of Examples 2 to 8 are similar to those of Example 1, and the differences are detailed in Table 1.

[0107] Comparative Example 1:

[0108] Synthesis of PA6T / 5T: 5142g of hexamethylenediamine, 4757g of pentamethylenediamine, 15101g of terephthalic acid, 162g of benzoic acid, 3.1g of sodium hypophosphite and 1346g of water were added to a pressure reactor equipped with a magnetic coupler for stirring. PA6T / 5T copolymer was prepared by the same preparation method as in Example 1. The melting point of the copolymer was 309°C, the glass transition temperature was 138°C, and the relative viscosity was 2.45. A semi-aromatic polyamide composition based on PA6T / 5T was obtained according to the same modification process, and was tested and compared as Comparative Example 1.

[0109] Comparative Example 2:

[0110] Synthesis of PA10T homopolymer: 12722g of decanediamine, 12278g of terephthalic acid, 162g of benzoic acid, 3.1g of sodium hypophosphite and 1346g of water were added to a pressure reactor equipped with a magnetic coupler and stirred. PA10T homopolymer was prepared by the same preparation method as in Example 1. The melting point of the product was 318°C, the glass transition temperature was 125°C, and the relative viscosity was 2.10. A semi-aromatic polyamide composition based on PA10T was obtained according to the same modification process, and was tested and compared as Comparative Example 2.

[0111] Comparative Example 3:

[0112] Synthesis of PA6T / 6I copolymer: 10280g hexamethylenediamine, 10301g terephthalic acid, 4415g isophthalic acid, 162g benzoic acid, 3.1g sodium hypophosphite and 1346g water were added to a pressure reactor equipped with a magnetic coupler for stirring. PA6T / 6I copolymer was prepared by the same preparation method as in Example 1. The melting point of the copolymer was 325°C, the glass transition temperature was 125°C, and the relative viscosity was 2.18. A semi-aromatic polyamide composition based on PA6T / 6I was obtained according to the same modification process, which was tested and compared as Comparative Example 3.

[0113] Table 1 Relevant performance data of the semi-aromatic copolymer polyamide obtained in each embodiment

[0114]

[0115]

[0116] Table 2 Relevant performance data of semi-aromatic high temperature resistant nylon obtained in each embodiment

[0117]

[0118]

[0119] From the comparison between Examples 1-8 and Comparative Examples 1-3, it can be seen that the material composed of long-chain and short-chain semi-aromatic copolyamides, dimers, and hydrolysis-resistant masterbatch exhibits obvious ethylene glycol resistance. After being soaked in ethylene glycol aqueous solution at 130°C for 1008 hours, the tensile strength of Examples 1-8 is about 140 MPa, while the strength of the comparative example after being soaked in ethylene glycol aqueous solution is only 120 MPa. In addition, the elongation at break and the flexural strength show the same trend.

[0120] Similarly, after 500 hours of thermal oxidative aging, the tensile strength retention rate of Examples 1-8 is 75% or above, showing good long-term heat resistance.

[0121] The semi-aromatic copolymer polyamide, the semi-aromatic polyamide composition and the preparation method and application thereof proposed in the present invention have been described through preferred embodiments. It is obvious that relevant technical personnel can modify or appropriately change and combine the process methods described herein without departing from the content, spirit and scope of the present invention to implement the technology of the present invention. It should be particularly pointed out that all similar substitutions and modifications are obvious to those skilled in the art, and they will be regarded as included in the spirit, scope and content of the present invention.

Claims

1. A semi-aromatic polyamide composition, wherein the raw materials of the composition include the following components by weight: Component A: 40-65 parts by weight of semi-aromatic copolymer polyamide; Component B: 3-15 parts by weight of heat-stable, hydrolysis-resistant and alcoholysis-resistant masterbatch; Component C: 30-60 parts by mass of reinforcing material; Component D: 0-2 parts by mass of heat stabilizer; Component E: 0-5 parts by weight of an auxiliary agent; The sum of component A to component E constitutes 100 parts by mass; The raw materials of the semi-aromatic copolymer polyamide include the following components by weight: (a1) 30 to 65 parts by mass of 6T units; (a2) 30 to 60 parts by mass of 4T units, 5T units or M5T units; (a3) ​​10 to 15 parts by mass of 9T units, 10T units or 12T units; (a4) 1 to 2 parts by mass of cyclic multimer units; wherein the sum of components (a1) to (a4) constitutes 100 parts by mass of the semi-aromatic copolymer polyamide; In component (a4), the cyclic polymer unit is one or more of the following structures: The heat-stable hydrolysis-resistant and alcoholysis-resistant masterbatch of component B is composed of polyamide, an anti-hydrolysis agent, a copper salt heat stabilizer and a lubricant; the glass transition temperature of the semi-aromatic polyamide composition is 135°C-170°C at a heating rate of 10°C / min.

2. The semi-aromatic polyamide composition according to claim 1, characterized in that In component (a1), the 6T unit is formed from 1,6-hexamethylenediamine and terephthalic acid; and / or, in component (a2), the 4T unit is formed from 1,4-butanediamine and terephthalic acid; and / or, in component (a2), the 5T unit is formed from 1,5-pentanediamine and terephthalic acid; and / or, in component (a2), the M5T unit is formed from 2-methyl-pentanediamine and terephthalic acid; and / or, in component (a3), the 9T unit is formed from 1,9-nonanediamine and terephthalic acid; and / or, in component (a3), the 10T unit is formed from 1,10-decanediamine and terephthalic acid; And / or, in component (a3), the 12T unit is formed from 1,12-dodecanediamine and terephthalic acid.

3. The semi-aromatic polyamide composition according to claim 1, characterized in that The component C is selected from one or more combinations of glass fiber, carbon fiber, talcum powder, and mica flakes; And / or, the component D is selected from one or more combinations of hindered phenol stabilizers, phosphite stabilizers, hindered amine stabilizers, triazine stabilizers, sulfur-containing stabilizers, and inorganic phosphorus-containing stabilizers; And / or, the component E is selected from a combination of one or more of a lubricant, an antistatic agent, and a release agent; And / or, the mass parts of the component E is 0-2 mass parts.

4. The semi-aromatic polyamide composition according to claim 1, characterized in that In the heat-stable hydrolysis-resistant and alcoholysis-resistant masterbatch of component B, the polyamide is selected from the semi-aromatic copolyamide PA6T / 66; And / or, the anti-hydrolysis agent is selected from one or more combinations of monomeric carbodiimide anti-hydrolysis agents, polymeric carbodiimide anti-hydrolysis agents and liquid carbodiimide anti-hydrolysis agents; And / or, the copper salt heat stabilizer is selected from any one of copper chloride, copper bromide, copper iodide, and copper phosphate; And / or, the lubricant is selected from any one of carboxylic acid calcium salt with a long carbon chain as the main component, vinyl bis stearamide EBS, TAF, silicone powder, and pentaerythritol stearate.

5. The semi-aromatic polyamide composition according to claim 1, characterized in that The anti-hydrolysis agent is a highly polymerized carbodiimide; and / or, the copper salt heat stabilizer is copper iodide; And / or, the lubricant is a calcium salt of a carboxylic acid having a long carbon chain as a main component.

6. The semi-aromatic polyamide composition according to any one of claims 1 to 5, characterized in that The semi-aromatic polyamide composition is aged at 170° C. for 500 hours, and the tensile strength retention rate is greater than or equal to 70%; And / or, after the semi-aromatic polyamide composition is immersed in an ethylene glycol-water mixture at 130° C. for 1008 hours, the elongation at break is greater than or equal to 1.5%.

7. The semi-aromatic polyamide composition according to claim 6, characterized in that The tensile strength retention rate is greater than or equal to 75%; And / or, the elongation at break is greater than or equal to 1.8%.

8. The method for preparing the semi-aromatic polyamide composition according to any one of claims 1 to 7, characterized in that: The steps include: S1: Components (a1) to (a4) are mixed and subjected to salt formation, prepolymerization and post-polymerization processes to obtain component A; S2: After component A and component E are fully mixed, they are extruded and granulated.

9. The method for preparing the semi-aromatic polyamide composition according to claim 8, characterized in that: In step S1, the salt formation and prepolymerization of components (a1)-(a4) are completed in the same pressure reaction vessel; And / or, in step S1, the monomers of components (a1)-(a4) and water are subjected to a salt-forming reaction in a first temperature section, and a prepolymerization reaction is carried out in a second temperature section; wherein the amount of water added in the salt-forming and prepolymerization is 0-30 wt.%; the first temperature section for salt-forming is 150° C.-190° C.; and the second temperature section for prepolymerization is 200° C.-280° C.; And / or, in step S1, after the prepolymerization is completed, the material is discharged and crushed, and the size of the crushed particles is ≤3mm; the crushed material is solid-phase polymerized, and the post-polymerization temperature is 220-280°C; the post-polymerization pressure is ≤50Pa, and the semi-aromatic copolymer polyamide is obtained by viscosity increase; And / or, step S2 also includes dispersing and mixing component A-component E at high speed, extruding and granulating at a high processing temperature, wherein the extruder speed is 100-350 rpm, and the temperature of each section of the extruder is 210°C-230°C, 270°C-290°C, 300°C-310°C, 310°C-330°C, 320°C-340°C, 330°C-350°C, 330°C-350°C, 320°C-340°C, 310°C-330°C, and after melt plasticization, extrusion and granulation are obtained to obtain a semi-aromatic polyamide composition.

10. The method for preparing the semi-aromatic polyamide composition according to claim 9, characterized in that: The amount of water added during salt formation and prepolymerization is 1-20wt.%; the first temperature section for salt formation is 170°C-180°C; the second temperature section for prepolymerization is 220°C-270°C; And / or, the post-polymerization temperature is 230-260°C; the post-polymerization pressure is ≤50Pa.

11. A semi-aromatic polyamide composition prepared by the method for preparing a semi-aromatic polyamide composition according to any one of claims 8 to 10.

12. Use of the semi-aromatic polyamide composition according to any one of claims 1 to 7 in the preparation of a component that is in direct or indirect contact with an ethylene glycol-water coolant.