A ni-mof derived capsule type carbon-coated composite material and a preparation method and application thereof
By preparing Ni-MOF-derived capsule-type carbon-coated composite material Ni9S8@PC-500, the problems of insufficient conductivity and stability of MOF materials were solved, enabling the application of supercapacitors with high specific capacitance and high energy density, and improving the efficiency and stability of electrochemical reactions.
Patent Information
- Application Number
- CN202311761639.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-20
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-12-20
AI Technical Summary
Existing MOF materials have low electrical conductivity and low stability, which limits their practical application in supercapacitors. Furthermore, porous carbon materials have insufficient specific capacitance and energy density, making it difficult to meet the huge demand for electrical energy.
A Ni-MOF-derived capsule-shaped carbon-coated composite material, Ni9S8@PC-500, was prepared by high-temperature vulcanization. By introducing uniformly dispersed Ni9S8 nanoparticles and capsule-shaped carbon layer structures into MOF materials, a composite material was formed for the preparation of asymmetric supercapacitors.
Rapid electron and ion migration was achieved, which enhanced the active sites of electrochemical reactions, improved specific capacitance and energy density, ensured the stability and conductivity of the material, and demonstrated excellent electrochemical performance.
Smart Images

Figure CN117790197B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of clean energy electrode materials technology, and in particular relates to a Ni-MOF-derived capsule-type carbon-coated composite material, its preparation method and application. Background Technology
[0002] In recent years, the surge in human consumption of fossil fuels has led to increasingly serious environmental problems such as energy depletion and pollution. Developing efficient, environmentally friendly, and sustainable energy conversion systems and energy storage devices is crucial. Supercapacitors (SCs), due to their high charge-discharge efficiency, stable practicality, reliable environmental applicability, and high power density, have become an important solution for energy storage and release. However, compared to secondary batteries, their lower energy density limits their practical applications. Therefore, researchers have invested heavily in exploring supercapacitor electrode materials that combine high power density and energy density. Common supercapacitor electrode materials can be divided into double-layer capacitor electrodes and pseudocapacitive electrodes. Porous carbon materials, due to their well-developed pore structure, large specific surface area, and strong structural stability, are the preferred choice for preparing double-layer capacitor electrode materials. However, their disadvantages include low specific capacitance and low energy density, making it difficult to meet the huge demand for electrical energy. Therefore, developing structurally stable pseudocapacitive electrode materials with rich electrochemical reactions has become a research focus.
[0003] Metal-organic frameworks (MOFs) are a novel class of crystalline materials composed of metal nodes or clusters linked to organic ligands via coordination bonds. They possess advantages such as abundant porosity, large specific surface area, and customizable structure, with their active metal centers providing a foundation for rich redox reactions. These characteristics enable rapid electron transfer and ion migration, as well as a wide range of electrochemical reactions. However, most MOF materials suffer from low electrical conductivity and stability, limiting their practical applications. Therefore, exploring a MOF material modification method that can inherit the porous structure of MOF materials while improving stability and electrical conductivity is crucial. To this end, this application proposes a Ni-MOF-derived capsule-type carbon-coated composite material, its preparation method, and its applications to address the aforementioned problems. Summary of the Invention
[0004] The purpose of this invention is to provide a Ni-MOF-derived capsule-type carbon-coated composite material, its preparation method, and its application. A composite material Ni9S8@PC-500 with abundant active sites is prepared by high-temperature vulcanization, and an asymmetric supercapacitor is prepared using this Ni9S8@PC-500 for energy storage, thus solving the problems in the background art mentioned above.
[0005] To solve the above-mentioned technical problems, the present invention is achieved through the following technical solution:
[0006] The present invention is a Ni-MOF-derived capsule-type carbon-coated composite material. The composite material has a capsule-shaped carbon-coated structure, the interior of the composite material is a uniformly dispersed Ni9S8 nanoparticle structure, and the exterior of the composite material is a capsule-shaped carbon layer structure.
[0007] The preparation method of the Ni-MOF-derived capsule-type carbon-coated composite material mainly includes the following steps:
[0008] Step 1: Dissolve the nickel salt in N,N-dimethylacetamide, stir until homogeneous, then add 1,2,4,5-pyromellitic acid and polyvinylpyrrolidone in sequence, and continue stirring to obtain a homogeneous solution.
[0009] Step 2: Transfer the above homogeneous solution to a stainless steel reactor, then place the stainless steel reactor in an oven and keep it at a temperature of 48-120 hours. After filtration and washing, obtain a green powder, and dry it in a vacuum environment to obtain the intermediate product Ni-MOF.
[0010] Step 3: Place Ni-MOF in the middle of a tubular furnace, place sublimed sulfur in the upper part of the tubular furnace, and then place the tubular furnace in an environment of Ar2 / H2 mixed gas at 500℃ to carry out a high-temperature vulcanization reaction to obtain the capsule-type carbon-coated composite material Ni9S8@PC-500.
[0011] As a preferred embodiment of the present invention, the specific method of step 1 is as follows: dissolve 1.164g of nickel salt in 60-100ml of N,N-dimethylacetamide, stir evenly, and then add 0.5096g of 1,2,4,5-pyromellitic acid and 1.2-2.0g of polyvinylpyrrolidone in sequence, and continue stirring to obtain a homogeneous solution.
[0012] As a preferred technical solution of the present invention, the specific method of step 2 is as follows: the homogeneous solution is transferred to a 100ml stainless steel reaction vessel, and then the stainless steel reaction vessel is placed in an oven at 110-140℃ for 48-120h. After filtration, the solution is washed several times with ethanol to obtain a green powder, and then dried in a vacuum environment to obtain the intermediate product Ni-MOF.
[0013] As a preferred technical solution of the present invention, the specific method of step 3 is as follows: 100mg of Ni-MOF is placed in the middle of the tubular furnace, 200-400mg of sublimed sulfur is placed in the upper part of the tubular furnace, and then the tubular furnace is placed in the environment of Ar2 / H2 mixed gas at 500℃ to carry out high-temperature vulcanization reaction to obtain capsule-type carbon-coated composite material Ni9S8@PC-500.
[0014] As a preferred embodiment of the present invention, the nickel salt is any one of nickel sulfate, nickel nitrate hexahydrate, nickel chloride, and nickel phosphate.
[0015] As a preferred embodiment of the present invention, during the high-temperature sulfidation reaction, the mass ratio of Ni-MOF in the midstream of the tubular furnace to sublimed sulfur in the upstream of the tubular furnace is 1:2-4, and the high-temperature sulfidation time is 2-4 hours.
[0016] As a preferred embodiment of the present invention, the application of Ni-MOF-derived capsule-type carbon-coated composite material Ni9S8@PC-500 in supercapacitors is described. The specific application process is as follows: A Ni9S8@PC-500 / / AC HSC device is assembled using Ni9S8@PC-500 as the positive electrode and AC as the negative electrode. In this HSC device, the active mass ratio of the positive electrode to the negative electrode is 1:0.32. Ni9S8@PC-500 exhibits significant electrochemical performance at a current density of 1 A·g-1. -1 At that time, the specific capacitance of the Ni9S8@PC-500 electrode was 2351.63 F·g. -1 At a current density of 10 A·g -1 At that time, after 10,000 constant current charge-discharge cycles, the capacity retention rate of the Ni9S8@PC-500 electrode was still as high as 94%.
[0017] Ni9S8@PC-500 / / AC HSC device at 827W·kg -1 It has a power density of 46 Wh·kg -1 The energy density is 7200 W·kg -1 It still maintains 31Wh·kg at high power density -1 Energy density, at 1 A·g -1 After 10,000 charge-discharge cycles at a current density, the Ni9S8@PC-500 / / AC HSC device still retains a capacity retention rate of up to 81%.
[0018] The present invention has the following beneficial effects:
[0019] 1. This invention uses the porous structure of MOFs materials as the structural basis, which can provide high-speed channels for the migration of electrons and ions during electrochemical reactions, enabling rapid migration of electrons and ions and facilitating the electrochemical reaction. The transition metal sulfides formed after high-temperature sulfidation based on carbon skeletons can have more reactive sites, providing the possibility for a variety of electrochemical reactions to occur.
[0020] 2. The uniform and ordered carbon skeleton used in this invention can provide high mechanical strength to cope with the decrease in stability caused by the phase transition of transition metal sulfides during electrochemical reactions. Compared with oxygen and phosphorus, sulfur has moderate electronegativity, and transition metal sulfides have better conductivity and suitable redox reactivity. The resulting capsule-type carbon-coated Ni9S8@PC-500 exhibits excellent electrochemical performance.
[0021] 3. The present invention has a high specific capacitance of 2351.63 F / g at 1 A / g, and the capacity retention rate reaches 94% after 10,000 constant current charge-discharge cycles. The assembled Ni9S8@PC-500 / / AC hybrid supercapacitor (HSC) provides a high energy density of 46 Wh / kg at 827 W / kg, and the capacity retention rate remains at 81% after 10,000 cycles.
[0022] Of course, any product implementing this invention does not necessarily need to achieve all of the advantages described above at the same time. Attached Figure Description
[0023] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0024] Figure 1 This is a flowchart illustrating the synthesis process of the Ni-MOF-derived capsule-type carbon-coated composite material in this invention.
[0025] Figure 2 The image shows the XRD pattern of the Ni-MOF in this invention.
[0026] Figure 3 The image shows the XRD pattern of Ni9S8@PC-500 in this invention.
[0027] Figure 4 This is the N2 adsorption curve of Ni9S8@PC-500 in this invention.
[0028] Figure 5 These are different characterization images of Ni9S8@PC-500 in this invention; wherein, Figure (a) is a SEM image of Ni9S8@PC-500, and Figure (bc) is a TEM image of Ni9S8@PC-500.
[0029] Figure 6 This is the XPS diagram of Ni9S8@PC-500 in this invention.
[0030] Figure 7 Figure 1 shows different electrical test results for Ni9S8@PC-500; Figure 2(a) shows Ni9S8@PC-500 at 2–100 mV·s. -1 The CV curves at different scan rates are shown in Figure (b), which is the curve of logi vs. logv, and Figure (c), which is the curve at 50 mV·s. -1Figure (d) shows the percentage of capacitance contribution rate at different scan rates, representing the total current.
[0031] Figure 8 Figure 1 shows different electrical test diagrams for Ni9S8@PC-500; Figure 2 shows the charge-discharge curve, Figure 3 shows the specific capacity at different current densities, Figure 4 shows the cycle stability test diagram, and Figure 5 shows the impedance diagram.
[0032] Figure 9 Figure 1 shows different electrical test results for Ni9S8@PC-500; Figure 2(a) shows the result at 50 mV·s. -1 Figure (b) shows the CV curves of AC and Ni9S8@PC-500. Figure (b) shows the Ni9S8@PC-500 / / AC hybrid supercapacitor at a scan rate of 50 mV·s. -1 Figure (c) shows the CV curves for different scan rates, and Figure (d) shows the GCD curves for different current densities within the 0-1.6V potential window.
[0033] Figure 10 Figure 1 shows different electrical test results for Ni9S8@PC-500; Figure 2(a) shows the results with a current density of 1 A·g -1 Figure (a) shows the retention rate after 10,000 cycles, and Figure (b) shows the Ragone plot of energy density and power density. Detailed Implementation
[0034] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0035] Example 1
[0036] Please see Figure 1-10 The present invention is a Ni-MOF-derived capsule-type carbon-coated composite material, wherein the composite material has a capsule-shaped carbon-coated structure, the interior of the composite material is a uniformly dispersed Ni9S8 nanoparticle structure, and the exterior of the composite material is a capsule-shaped carbon layer structure.
[0037] The preparation method of the Ni-MOF-derived capsule-type carbon-coated composite material mainly includes the following steps:
[0038] Step 1: Dissolve Ni(NO3)2·6H2O in 80 ml of N,N-dimethylacetamide (DMA), stir well, then add 0.5096 g of 1,2,4,5-pyromellitic acid (PMA) and 1.8 g of polyvinylpyrrolidone (PVP) in sequence, and continue stirring to obtain a homogeneous solution;
[0039] Step 2: Transfer the homogeneous solution to a 100ml stainless steel reactor, then place the stainless steel reactor in a 120℃ oven for 72h. After filtration, wash several times with ethanol to obtain a green powder, and dry it in a vacuum environment to obtain the intermediate product Ni-MOF.
[0040] Step 3: Place 100 mg of Ni-MOF in the middle of the tubular furnace and 200 mg of sublimed sulfur in the upper part of the tubular furnace. Then place the tubular furnace in an environment of Ar2 / H2 mixed gas at 500℃ for high-temperature vulcanization reaction for 2 hours to successfully obtain the capsule-type carbon-coated composite material Ni9S8@PC-500.
[0041] Example 2
[0042] Please see Figure 1-10 The present invention is a Ni-MOF-derived capsule-type carbon-coated composite material, wherein the composite material has a capsule-shaped carbon-coated structure, the interior of the composite material is a uniformly dispersed Ni9S8 nanoparticle structure, and the exterior of the composite material is a capsule-shaped carbon layer structure.
[0043] The preparation method of the Ni-MOF-derived capsule-type carbon-coated composite material mainly includes the following steps:
[0044] Step 1: Dissolve Ni(NO3)2·6H2O in 80 ml of N,N-dimethylacetamide (DMA), stir well, then add 0.5096 g of 1,2,4,5-pyromellitic acid (PMA) and 1.6 g of polyvinylpyrrolidone (PVP) in sequence, and continue stirring to obtain a homogeneous solution;
[0045] Step 2: Transfer the homogeneous solution to a 100ml stainless steel reactor, then place the stainless steel reactor in a 110℃ oven for 72h. After filtration, wash with ethanol several times to obtain a green powder, and dry in a vacuum environment to obtain the intermediate product Ni-MOF.
[0046] Step 3: Place 100 mg of Ni-MOF in the middle of the tubular furnace and 200 mg of sublimed sulfur in the upper part of the tubular furnace. Then place the tubular furnace in an environment of Ar2 / H2 mixed gas at 500℃ for high-temperature vulcanization reaction for 2 hours to successfully obtain the capsule-type carbon-coated composite material Ni9S8@PC-500.
[0047] Example 3
[0048] Please see Figure 1-10 The present invention is a Ni-MOF-derived capsule-type carbon-coated composite material, wherein the composite material has a capsule-shaped carbon-coated structure, the interior of the composite material is a uniformly dispersed Ni9S8 nanoparticle structure, and the exterior of the composite material is a capsule-shaped carbon layer structure.
[0049] The preparation method of the Ni-MOF-derived capsule-type carbon-coated composite material mainly includes the following steps:
[0050] Step 1: Dissolve Ni(NO3)2·6H2O in 80 ml of N,N-dimethylacetamide (DMA), stir well, then add 0.5096 g of 1,2,4,5-pyromellitic acid (PMA) and 1.7 g of polyvinylpyrrolidone (PVP) in sequence, and continue stirring to obtain a homogeneous solution;
[0051] Step 2: Transfer the homogeneous solution to a 100ml stainless steel reactor, then place the stainless steel reactor in a 130℃ oven for 72h. After filtration, wash with ethanol several times to obtain a green powder, and dry in a vacuum environment to obtain the intermediate product Ni-MOF.
[0052] Step 3: Place 100 mg of Ni-MOF in the middle of the tubular furnace and 200 mg of sublimed sulfur in the upper part of the tubular furnace. Then place the tubular furnace in an environment of Ar2 / H2 mixed gas at 500℃ for high-temperature vulcanization reaction for 2 hours to successfully obtain the capsule-type carbon-coated composite material Ni9S8@PC-500.
[0053] Example 4
[0054] Please see Figure 1-10 The present invention is a Ni-MOF-derived capsule-type carbon-coated composite material, wherein the composite material has a capsule-shaped carbon-coated structure, the interior of the composite material is a uniformly dispersed Ni9S8 nanoparticle structure, and the exterior of the composite material is a capsule-shaped carbon layer structure.
[0055] The preparation method of the Ni-MOF-derived capsule-type carbon-coated composite material mainly includes the following steps:
[0056] Step 1: Dissolve Ni(NO3)2·6H2O in 80 ml of N,N-dimethylacetamide (DMA), stir well, then add 0.5096 g of 1,2,4,5-pyromellitic acid (PMA) and 1.9 g of polyvinylpyrrolidone (PVP) in sequence, and continue stirring to obtain a homogeneous solution;
[0057] Step 2: Transfer the homogeneous solution to a 100ml stainless steel reactor, then place the stainless steel reactor in a 140℃ oven for 72h. After filtration, wash several times with ethanol to obtain a green powder, and dry it in a vacuum environment to obtain the intermediate product Ni-MOF.
[0058] Step 3: Place 100 mg of Ni-MOF in the middle of the tubular furnace and 200 mg of sublimed sulfur in the upper part of the tubular furnace. Then place the tubular furnace in an environment of Ar2 / H2 mixed gas at 500℃ for high-temperature vulcanization reaction for 2 hours to successfully obtain the capsule-type carbon-coated composite material Ni9S8@PC-500.
[0059] Example 5
[0060] Please see Figure 1-10 The present invention is a Ni-MOF-derived capsule-type carbon-coated composite material, wherein the composite material has a capsule-shaped carbon-coated structure, the interior of the composite material is a uniformly dispersed Ni9S8 nanoparticle structure, and the exterior of the composite material is a capsule-shaped carbon layer structure.
[0061] The preparation method of the Ni-MOF-derived capsule-type carbon-coated composite material mainly includes the following steps:
[0062] Step 1: Dissolve Ni(NO3)2·6H2O in 80 ml of N,N-dimethylacetamide (DMA), stir well, then add 0.5096 g of 1,2,4,5-pyromellitic acid (PMA) and 2.0 g of polyvinylpyrrolidone (PVP) in sequence, and continue stirring to obtain a homogeneous solution;
[0063] Step 2: Transfer the homogeneous solution to a 100ml stainless steel reactor, then place the stainless steel reactor in a 120℃ oven for 72h. After filtration, wash several times with ethanol to obtain a green powder, and dry it in a vacuum environment to obtain the intermediate product Ni-MOF.
[0064] Step 3: Place 100 mg of Ni-MOF in the middle of the tubular furnace and 200 mg of sublimed sulfur in the upper part of the tubular furnace. Then place the tubular furnace in an environment of Ar2 / H2 mixed gas at 500℃ for high-temperature vulcanization reaction for 2 hours to successfully obtain the capsule-type carbon-coated composite material Ni9S8@PC-500.
[0065] Example 6
[0066] Please see Figure 1-10 The present invention is a Ni-MOF-derived capsule-type carbon-coated composite material, wherein the composite material has a capsule-shaped carbon-coated structure, the interior of the composite material is a uniformly dispersed Ni9S8 nanoparticle structure, and the exterior of the composite material is a capsule-shaped carbon layer structure.
[0067] The preparation method of the Ni-MOF-derived capsule-type carbon-coated composite material mainly includes the following steps:
[0068] Step 1: Dissolve Ni(NO3)2·6H2O in 60 ml of N,N-dimethylacetamide (DMA), stir well, then add 0.5096 g of 1,2,4,5-pyromellitic acid (PMA) and 3.0 g of polyvinylpyrrolidone (PVP) in sequence, and continue stirring to obtain a homogeneous solution;
[0069] Step 2: Transfer the homogeneous solution to a 100ml stainless steel reactor, then place the stainless steel reactor in a 120℃ oven for 72h. After filtration, wash several times with ethanol to obtain a green powder, and dry it in a vacuum environment to obtain the intermediate product Ni-MOF.
[0070] Step 3: Place 100 mg of Ni-MOF in the middle of the tubular furnace and 200 mg of sublimed sulfur in the upper part of the tubular furnace. Then place the tubular furnace in an environment of Ar2 / H2 mixed gas at 500℃ for high-temperature vulcanization reaction for 2 hours to successfully obtain the capsule-type carbon-coated composite material Ni9S8@PC-500.
[0071] Example 7
[0072] Please see Figure 1-10 The present invention is a Ni-MOF-derived capsule-type carbon-coated composite material, wherein the composite material has a capsule-shaped carbon-coated structure, the interior of the composite material is a uniformly dispersed Ni9S8 nanoparticle structure, and the exterior of the composite material is a capsule-shaped carbon layer structure.
[0073] The preparation method of the Ni-MOF-derived capsule-type carbon-coated composite material mainly includes the following steps:
[0074] Step 1: Dissolve Ni(NO3)2·6H2O in 70 ml of N,N-dimethylacetamide (DMA), stir well, then add 0.5096 g of 1,2,4,5-pyromellitic acid (PMA) and 4.0 g of polyvinylpyrrolidone (PVP) in sequence, and continue stirring to obtain a homogeneous solution;
[0075] Step 2: Transfer the homogeneous solution to a 100ml stainless steel reactor, then place the stainless steel reactor in a 120℃ oven for 72h. After filtration, wash several times with ethanol to obtain a green powder, and dry it in a vacuum environment to obtain the intermediate product Ni-MOF.
[0076] Step 3: Place 100 mg of Ni-MOF in the middle of the tubular furnace and 200 mg of sublimed sulfur in the upper part of the tubular furnace. Then place the tubular furnace in an environment of Ar2 / H2 mixed gas at 500℃ for high-temperature vulcanization reaction for 2 hours to successfully obtain the capsule-type carbon-coated composite material Ni9S8@PC-500.
[0077] Example 8
[0078] Please see Figure 1-10 The present invention is a Ni-MOF-derived capsule-type carbon-coated composite material, wherein the composite material has a capsule-shaped carbon-coated structure, the interior of the composite material is a uniformly dispersed Ni9S8 nanoparticle structure, and the exterior of the composite material is a capsule-shaped carbon layer structure.
[0079] The preparation method of the Ni-MOF-derived capsule-type carbon-coated composite material mainly includes the following steps:
[0080] Step 1: Dissolve Ni(NO3)2·6H2O in 90 ml of N,N-dimethylacetamide (DMA), stir well, then add 0.5096 g of 1,2,4,5-pyromellitic acid (PMA) and 1.8 g of polyvinylpyrrolidone (PVP) in sequence, and continue stirring to obtain a homogeneous solution;
[0081] Step 2: Transfer the homogeneous solution to a 100ml stainless steel reactor, then place the stainless steel reactor in a 120℃ oven for 72h. After filtration, wash several times with ethanol to obtain a green powder, and dry it in a vacuum environment to obtain the intermediate product Ni-MOF.
[0082] Step 3: Place 100 mg of Ni-MOF in the middle of the tubular furnace and 300 mg of sublimed sulfur in the upper part of the tubular furnace. Then place the tubular furnace in an environment of Ar2 / H2 mixed gas at 500℃ for high-temperature vulcanization reaction for 2 hours to successfully obtain the capsule-type carbon-coated composite material Ni9S8@PC-500.
[0083] Example 9
[0084] Please see Figure 1-10 The present invention is a Ni-MOF-derived capsule-type carbon-coated composite material, wherein the composite material has a capsule-shaped carbon-coated structure, the interior of the composite material is a uniformly dispersed Ni9S8 nanoparticle structure, and the exterior of the composite material is a capsule-shaped carbon layer structure.
[0085] The preparation method of the Ni-MOF-derived capsule-type carbon-coated composite material mainly includes the following steps:
[0086] Step 1: Dissolve Ni(NO3)2·6H2O in 100ml of N,N-dimethylacetamide (DMA), stir well, then add 0.5096g of 1,2,4,5-pyromellitic acid (PMA) and 1.8g of polyvinylpyrrolidone (PVP) in sequence, and continue stirring to obtain a homogeneous solution;
[0087] Step 2: Transfer the homogeneous solution to a 100ml stainless steel reactor, then place the stainless steel reactor in a 120℃ oven for 48h. After filtration, wash several times with ethanol to obtain a green powder, and dry it in a vacuum environment to obtain the intermediate product Ni-MOF.
[0088] Step 3: Place 100 mg of Ni-MOF in the middle of the tubular furnace and 200 mg of sublimed sulfur in the upper part of the tubular furnace. Then place the tubular furnace in an environment of Ar2 / H2 mixed gas at 500℃ for high-temperature vulcanization reaction for 2 hours to successfully obtain the capsule-type carbon-coated composite material Ni9S8@PC-500.
[0089] Example 10
[0090] Please see Figure 1-10 The present invention is a Ni-MOF-derived capsule-type carbon-coated composite material, wherein the composite material has a capsule-shaped carbon-coated structure, the interior of the composite material is a uniformly dispersed Ni9S8 nanoparticle structure, and the exterior of the composite material is a capsule-shaped carbon layer structure.
[0091] The preparation method of the Ni-MOF-derived capsule-type carbon-coated composite material mainly includes the following steps:
[0092] Step 1: Dissolve Ni(NO3)2·6H2O in 80 ml of N,N-dimethylacetamide (DMA), stir well, then add 0.5096 g of 1,2,4,5-pyromellitic acid (PMA) and 1.8 g of polyvinylpyrrolidone (PVP) in sequence, and continue stirring to obtain a homogeneous solution;
[0093] Step 2: Transfer the homogeneous solution to a 100ml stainless steel reactor, then place the stainless steel reactor in a 120℃ oven for 48h. After filtration, wash several times with ethanol to obtain a green powder, and dry it in a vacuum environment to obtain the intermediate product Ni-MOF.
[0094] Step 3: Place 100 mg of Ni-MOF in the middle of the tubular furnace and 200 mg of sublimed sulfur in the upper part of the tubular furnace. Then place the tubular furnace in an environment of Ar2 / H2 mixed gas at 500℃ for high-temperature vulcanization reaction for 2 hours to successfully obtain the capsule-type carbon-coated composite material Ni9S8@PC-500.
[0095] Example 11
[0096] Please see Figure 1-10 The present invention is a Ni-MOF-derived capsule-type carbon-coated composite material, wherein the composite material has a capsule-shaped carbon-coated structure, the interior of the composite material is a uniformly dispersed Ni9S8 nanoparticle structure, and the exterior of the composite material is a capsule-shaped carbon layer structure.
[0097] The preparation method of the Ni-MOF-derived capsule-type carbon-coated composite material mainly includes the following steps:
[0098] Step 1: Dissolve Ni(NO3)2·6H2O in 80 ml of N,N-dimethylacetamide (DMA), stir well, then add 0.5096 g of 1,2,4,5-pyromellitic acid (PMA) and 1.8 g of polyvinylpyrrolidone (PVP) in sequence, and continue stirring to obtain a homogeneous solution;
[0099] Step 2: Transfer the homogeneous solution to a 100ml stainless steel reactor, then place the stainless steel reactor in a 120℃ oven for 96h. After filtration, wash several times with ethanol to obtain a green powder, and dry it in a vacuum environment to obtain the intermediate product Ni-MOF.
[0100] Step 3: Place 100 mg of Ni-MOF in the middle of the tubular furnace and 200 mg of sublimed sulfur in the upper part of the tubular furnace. Then place the tubular furnace in an environment of Ar2 / H2 mixed gas at 500℃ for high-temperature vulcanization reaction for 2 hours to successfully obtain the capsule-type carbon-coated composite material Ni9S8@PC-500.
[0101] Example 12
[0102] Please see Figure 1-10 The present invention is a Ni-MOF-derived capsule-type carbon-coated composite material, wherein the composite material has a capsule-shaped carbon-coated structure, the interior of the composite material is a uniformly dispersed Ni9S8 nanoparticle structure, and the exterior of the composite material is a capsule-shaped carbon layer structure.
[0103] The preparation method of the Ni-MOF-derived capsule-type carbon-coated composite material mainly includes the following steps:
[0104] Step 1: Dissolve Ni(NO3)2·6H2O in 80 ml of N,N-dimethylacetamide (DMA), stir well, then add 0.5096 g of 1,2,4,5-pyromellitic acid (PMA) and 1.8 g of polyvinylpyrrolidone (PVP) in sequence, and continue stirring to obtain a homogeneous solution;
[0105] Step 2: Transfer the homogeneous solution to a 100ml stainless steel reactor, then place the stainless steel reactor in a 120℃ oven for 120h. After filtration, wash with ethanol several times to obtain a green powder, and dry in a vacuum environment to obtain the intermediate product Ni-MOF.
[0106] Step 3: Place 100 mg of Ni-MOF in the middle of the tubular furnace and 200 mg of sublimed sulfur in the upper part of the tubular furnace. Then place the tubular furnace in an environment of Ar2 / H2 mixed gas at 500℃ for high-temperature vulcanization reaction for 2 hours to successfully obtain the capsule-type carbon-coated composite material Ni9S8@PC-500.
[0107] Example 13
[0108] Please see Figure 1-10 The present invention is a Ni-MOF-derived capsule-type carbon-coated composite material, wherein the composite material has a capsule-shaped carbon-coated structure, the interior of the composite material is a uniformly dispersed Ni9S8 nanoparticle structure, and the exterior of the composite material is a capsule-shaped carbon layer structure.
[0109] The preparation method of the Ni-MOF-derived capsule-type carbon-coated composite material mainly includes the following steps:
[0110] Step 1: Dissolve Ni(NO3)2·6H2O in 80 ml of N,N-dimethylacetamide (DMA), stir well, then add 0.5096 g of 1,2,4,5-pyromellitic acid (PMA) and 1.2 g of polyvinylpyrrolidone (PVP) in sequence, and continue stirring to obtain a homogeneous solution;
[0111] Step 2: Transfer the homogeneous solution to a 100ml stainless steel reactor, then place the stainless steel reactor in a 120℃ oven for 72h. After filtration, wash several times with ethanol to obtain a green powder, and dry it in a vacuum environment to obtain the intermediate product Ni-MOF.
[0112] Step 3: Place 100 mg of Ni-MOF in the middle of the tubular furnace and 200 mg of sublimed sulfur in the upper part of the tubular furnace. Then place the tubular furnace in an environment of Ar2 / H2 mixed gas at 500℃ for high-temperature vulcanization reaction for 4 hours to successfully obtain the capsule-type carbon-coated composite material Ni9S8@PC-500.
[0113] Example 14
[0114] Please see Figure 1-10 The present invention is a Ni-MOF-derived capsule-type carbon-coated composite material, wherein the composite material has a capsule-shaped carbon-coated structure, the interior of the composite material is a uniformly dispersed Ni9S8 nanoparticle structure, and the exterior of the composite material is a capsule-shaped carbon layer structure.
[0115] The preparation method of the Ni-MOF-derived capsule-type carbon-coated composite material mainly includes the following steps:
[0116] Step 1: Dissolve Ni(NO3)2·6H2O in 80 ml of N,N-dimethylacetamide (DMA), stir well, then add 0.5096 g of 1,2,4,5-pyromellitic acid (PMA) and 1.3 g of polyvinylpyrrolidone (PVP) in sequence, and continue stirring to obtain a homogeneous solution;
[0117] Step 2: Transfer the homogeneous solution to a 100ml stainless steel reactor, then place the stainless steel reactor in a 120℃ oven for 72h. After filtration, wash several times with ethanol to obtain a green powder, and dry it in a vacuum environment to obtain the intermediate product Ni-MOF.
[0118] Step 3: Place 100 mg of Ni-MOF in the middle of the tubular furnace and 200 mg of sublimed sulfur in the upper part of the tubular furnace. Then place the tubular furnace in an environment of Ar2 / H2 mixed gas at 500℃ for high-temperature vulcanization reaction for 3.5 h to successfully obtain capsule-type carbon-coated composite material Ni9S8@PC-500.
[0119] Example 15
[0120] Please see Figure 1-10 The present invention is a Ni-MOF-derived capsule-type carbon-coated composite material, wherein the composite material has a capsule-shaped carbon-coated structure, the interior of the composite material is a uniformly dispersed Ni9S8 nanoparticle structure, and the exterior of the composite material is a capsule-shaped carbon layer structure.
[0121] The preparation method of the Ni-MOF-derived capsule-type carbon-coated composite material mainly includes the following steps:
[0122] Step 1: Dissolve Ni(NO3)2·6H2O in 80 ml of N,N-dimethylacetamide (DMA), stir well, then add 0.5096 g of 1,2,4,5-pyromellitic acid (PMA) and 1.4 g of polyvinylpyrrolidone (PVP) in sequence, and continue stirring to obtain a homogeneous solution;
[0123] Step 2: Transfer the homogeneous solution to a 100ml stainless steel reactor, then place the stainless steel reactor in a 120℃ oven for 72h. After filtration, wash several times with ethanol to obtain a green powder, and dry it in a vacuum environment to obtain the intermediate product Ni-MOF.
[0124] Step 3: Place 100 mg of Ni-MOF in the middle of the tubular furnace and 200 mg of sublimed sulfur in the upper part of the tubular furnace. Then place the tubular furnace in an environment of Ar2 / H2 mixed gas at 500℃ for high-temperature vulcanization reaction for 3 hours to successfully obtain the capsule-type carbon-coated composite material Ni9S8@PC-500.
[0125] Example 16
[0126] Please see Figure 1-10 The present invention is a Ni-MOF-derived capsule-type carbon-coated composite material, wherein the composite material has a capsule-shaped carbon-coated structure, the interior of the composite material is a uniformly dispersed Ni9S8 nanoparticle structure, and the exterior of the composite material is a capsule-shaped carbon layer structure.
[0127] The preparation method of the Ni-MOF-derived capsule-type carbon-coated composite material mainly includes the following steps:
[0128] Step 1: Dissolve Ni(NO3)2·6H2O in 80ml of N,N-dimethylacetamide (DMA), stir well, then add 0.5096g of 1,2,4,5-pyromellitic acid (PMA) and 1.5g of polyvinylpyrrolidone (PVP) in sequence, and continue stirring to obtain a homogeneous solution;
[0129] Step 2: Transfer the homogeneous solution to a 100ml stainless steel reactor, then place the stainless steel reactor in a 120℃ oven for 72h. After filtration, wash several times with ethanol to obtain a green powder, and dry it in a vacuum environment to obtain the intermediate product Ni-MOF.
[0130] Step 3: Place 100 mg of Ni-MOF in the middle of the tubular furnace and 200 mg of sublimed sulfur in the upper part of the tubular furnace. Then place the tubular furnace in an environment of Ar2 / H2 mixed gas at 500℃ for high-temperature vulcanization reaction for 2.5 h to successfully obtain the capsule-type carbon-coated composite material Ni9S8@PC-500.
[0131] X-ray powder diffraction (XRD) results of the Ni-MOF precursor are as follows: Figure 2 As shown, the crystallinity is good. Figure 3 As shown, comparative analysis revealed that the active component of the Ni9S8@PC-500 nanocomposite material derived from Ni-MOF is Ni9S8.
[0132] The surface area (BET) and pore size distribution of the Ni9S8@PC-500 composite material were analyzed using N2 adsorption-desorption experiments. Figure 4 As shown, Ni9S8@PC-500 exhibits typical type II and type IV adsorption isotherms. The pore size of the material is concentrated in mesopores (3-4 and 20-50 nm) and macropores (50-80 nm), possessing a hierarchical pore structure and good nitrogen adsorption / desorption capacity. The specific surface area is 54.37 m². 2 / g. A larger specific surface area and abundant porosity facilitate the rapid migration of electrons and electrolyte ions within the material, resulting in better electrochemical performance.
[0133] After high-temperature sulfurization, the Ni-MOF precursor was successfully transformed into uniform, encapsulated carbon-coated Ni9S8@PC-500 nanoparticles, such as... Figure 5 As shown, TEM images reveal a distinct capsule-like carbon-encapsulated structure in the material, and HRTEM observation further confirms the microstructure of the nanoparticles. The particle length is 26.15 nm and the width is 11.03 nm. Figure 5 b). The measured fringe spacing was 0.241 nm. Figure 5 c), which belongs to the (042) plane of Ni9S8.
[0134] The surface elemental composition and chemical bond properties of Ni9S8@PC-500 were analyzed using X-ray photoelectron spectroscopy (XPS). Figure 6 As shown in figure a, Ni, C, O and S elements were successfully detected on the surface of the prepared nanocomposite material. Figure 6 The peak values of b at 855.26 and 873.07 eV represent Ni, respectively. 2+ Ni 2p 3 / 2 and Ni 2p 1 / 2 The peaks at 852.63 and 870.07 eV represent Ni. 3+ Furthermore, the peaks at 860.61 and 879.26 eV are satellite peaks of Ni 2p. Ni9S8@PC-500 exhibits two valence states of Ni: Ni 2+ and Ni 3+ This provides the possibility for the occurrence of a wide range of redox reactions. Figure 6 Figure c shows the S2p spectrum, indicating characteristic peaks at 161.28, 162.30, and 163.68 eV, corresponding to the CS bond, Sp3 / 2, and Sp1 / 2, respectively. Furthermore, the two peaks at 164.95 and 168.03 eV are satellite peaks of the sulfur element.
[0135] The electrochemical behavior of Ni9S8@PC-500 was investigated using CV, GCD, and EIS in a three-electrode testing system. Cyclic voltammetry (CV) curves of the Ni9S8@PC-500 electrode were studied at a scan rate of 20 mV / s and a voltage window of 0.5 V. It was clearly observed that the CV curve of Ni9S8@PC-500 material exhibited two symmetrical redox peaks, demonstrating the reversibility of the redox reaction. The optimized Ni9S8@PC-500 electrode material possessed a larger CV curve integral area and higher redox peak intensity, indicating that it has good electrochemical performance. These significant electrochemical characteristics can be attributed to its unique carbon framework structure and large specific surface area. Further testing of the CV curves of Ni9S8@PC-500 was conducted within a scan rate range of 2-100 mV / s, such as... Figure 7 As shown in figure a. The results show that the Ni9S8@PC-500 electrode exhibits significant redox peaks at different scan rates, which can be attributed to the electron gain and loss process of nickel.
[0136]
[0137] The relationship between log(i) and log(V) can be obtained from the CV curve of Ni9S8@PC-500, and is given by the following equation:
[0138] i = av b
[0139] logi = blogv + loga
[0140] The value of b is calculated. When b = 1.0, the charge storage process is controlled by capacitance, while when b = 0.5, the charge storage process is controlled by diffusion. For example... Figure 7 As shown in b, the b-values of the redox peaks of Ni9S8@PC-500 are 0.62 and 0.69, respectively, indicating that the charge storage process of the Ni9S8@PC-500 composite material is the result of the combined effect of diffusion control and capacitance control. Figure 7 c). The contribution rates of the two processes can be further calculated using the following formula:
[0141] i(V)=k1v+k2v 1 / 2
[0142] Where i and ν represent the current and scan rate, respectively, and k1ν and k2ν 1 / 2 These represent the relative contributions of the capacitance control and diffusion control processes, respectively. At a scan rate of 2 m / V ( Figure 7 d) The diffusion control process contributes 69% of the total charge storage, indicating that at lower scan rates, the charge storage mechanism of Ni9S8@PC-500 is mainly diffusion control. Furthermore, the proportion of contribution from capacitance control gradually increases with the increase of scan rate, indicating that the Ni9S8@PC-500 electrode mainly exhibits pseudocapacitive behavior.
[0143] To further investigate the electrochemical performance of Ni9S8@PC-500, such as... Figure 8 As shown in Figure a, the Ni9S8@PC-500 composite material underwent constant current charge-discharge (GCD) testing at a potential window of 1 A / g and 0-0.4 V. The Ni9S8@PC-500 composite material exhibited a relatively long discharge time, indicating that it possesses a high specific capacitance. The GCD curves show a typical charge-discharge plateau, reflecting the typical battery behavior of the electrode material. The specific capacitance of Ni9S8@PC-500 at different current densities is given by the formula:
[0144]
[0145] The calculated specific capacitances of Ni9S8@PC-500 at different current densities are 2351.63 (1A / g), 2183.26 (2A / g), 1845.06 (5A / g), 1657.35 (10A / g), 1494.78 (15A / g), 1387.47 (20A / g), and 1103.35 (40A / g) F / g, respectively. The specific capacitance of Ni9S8@PC-500 at 40A / g is 47% of that at 1A / g. Figure 8 b). The cycle stability of Ni9S8@PC-500 was tested at a current density of 10 A / g, maintaining 94% ( ) after 10,000 charge-discharge cycles. Figure 8 c) It exhibits excellent cycle stability.
[0146] EIS testing was used to further understand the charge transfer characteristics and ion diffusion mechanism of the material. Figure 8 Figure d describes the Nyquist plot of the Ni9S8@PC-500 electrode. In the low-frequency region, the slope of Ni9S8@PC-500 is relatively large, indicating a low Warburg impedance (Wo), which means that ions in the electrolyte diffuse to the electrode surface more quickly. In the high-frequency region, the intercept of the real part of the impedance reflects the magnitude of the series resistance (Rs). The small intercept of Ni9S8@PC-500 proves that the interfacial contact resistance at the electrolyte and electrolyte / collector ion resistance is small. The low resistivity of Ni9S8@PC-500 proves that this electrode has good conductivity and excellent charge transfer capability, which is beneficial to improving the specific capacitance and rate performance of the electrode material.
[0147] To better investigate the practicality of the Ni9S8@PC-500 electrode material, a high-performance Ni9S8@PC-500 / / AC HSC device was assembled using Ni9S8@PC-500 as the positive electrode and AC as the negative electrode. The calculated active mass ratio of the positive and negative electrodes was approximately 1:0.32. Figure 9 Figure a shows the CV curves of Ni9S8@PC-500 and AC electrodes in a three-electrode system at 50mV / s, with voltage windows of 0-0.5V and -1-0V, respectively. Experiments show that the optimal operating voltage of the HSC device is 1.6V. Figure 9 b). When the operating potential window of Ni9S8@PC-500 / / AC HSC was increased to 1.7V, significant polarization occurred, therefore 0-1.6V was determined as the optimal voltage window. CV tests were performed at different scan rates from 5-100mV / s. Figure 9 c). With increasing scan rate, the HSC exhibits double-layer and cell-like behavior. The curve did not show significant deformation with increasing scan rate, demonstrating that the HSC possesses good rate performance and stability at high scan rates. Figure 9 As shown in Figure d, the GCD curve approximates an isosceles triangle, proving that the Ni9S8@PC-500 / / AC HSC device has high coulombic efficiency. Based on the discharge curves, the specific capacitances of the HSC device at 1, 2, 5, 8, 10, 12, and 15 A / g are calculated to be 125.75, 112.77, 94.36, 85.14, 80.53, 77.20, and 75.70 F / g, respectively, demonstrating excellent rate capability. Notably, the Ni9S8@PC-500 / / AC HSC device retains 81% of its capacity after 10,000 charge-discharge cycles at a current density of 1 A / g, exhibiting good cycle stability. Figure 10 a).
[0148] The power density and energy density of the Ni9S8@PC-500 / / AC HSC device were further calculated, and a Ragone plot was plotted. The results are as follows: Figure 10 As shown in b, superior energy storage performance is demonstrated. The Ni9S8@PC-500 / / AC HSC can provide an energy density of 46 Wh / kg at a power density of 827 W / kg, and still maintains an energy density of 31 Wh / kg at a power density of 7200 W / kg. This result is superior to many recently reported Ni-based transition metal sulfide composites. Based on the above results, Ni9S8@PC-500 / / AC HSC can be considered a potentially efficient, stable, and high-performance supercapacitor device.
[0149] In summary, using a high-temperature sulfidation process with Ni-MOF as a sacrificial template, encapsulated carbon-coated Ni9S8@PC-500 nanoparticles were successfully synthesized. These nanoparticles exhibit high porosity, abundant redox active sites, and a large specific surface area. Furthermore, the excellent porous structure of Ni9S8 and the superior carbon framework synergistically enable them to simultaneously possess double-layer energy storage and pseudocapacitive energy storage effects. Therefore, the MOF-derived Ni9S8@PC-500 electrode material exhibits excellent electrochemical performance. At 1 A / g, the Ni9S8@PC-500 electrode displays 2351.63 F g. -1 The ideal specific capacitance is achieved; at 10 A / g, the capacity retention is 94% after 10,000 constant current charge-discharge cycles. Furthermore, the assembled Ni9S8@PC-500 / / AC HSC achieves an energy density of 46 Wh / kg at a power density of 827 W / kg and exhibits a long lifespan, with a capacity retention of 81% after 10,000 charge-discharge cycles. These results demonstrate the promising application prospects of Ni-MOF-derived capsule-type carbon-coated Ni9S8@PC-500 electrodes in energy storage devices.
[0150] In the description of this specification, references to terms such as "an embodiment," "example," "specific example," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0151] The preferred embodiments of the present invention disclosed above are merely illustrative of the invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the invention to the specific implementations described. Clearly, many modifications and variations can be made based on the content of this specification. This specification selects and specifically describes these embodiments to better explain the principles and practical applications of the invention, thereby enabling those skilled in the art to better understand and utilize the invention. The invention is limited only by the claims and their full scope and equivalents.
Claims
1. A Ni-MOF-derived capsule-type carbon-coated composite material, characterized in that, The composite material has a capsule-shaped carbon-coated structure, with a uniformly dispersed Ni9S8 nanoparticle structure inside and a capsule-shaped carbon layer structure on the outside. The preparation method of the Ni-MOF-derived capsule-type carbon-coated composite material mainly includes the following steps: Step 1: Dissolve the nickel salt in N,N-dimethylacetamide, stir until homogeneous, then add 1,2,4,5-pyromellitic acid and polyvinylpyrrolidone in sequence, and continue stirring to obtain a homogeneous solution. Step 2: Transfer the above homogeneous solution to a stainless steel reactor, then place the stainless steel reactor in an oven and keep it at a temperature of 48-120 hours. After filtration and washing, obtain a green powder, and dry it in a vacuum environment to obtain the intermediate product Ni-MOF. Step 3: Place Ni-MOF in the middle of a tubular furnace, place sublimed sulfur in the upper part of the tubular furnace, and then place the tubular furnace in an Ar / H2 mixed gas environment at 500℃ for high-temperature vulcanization reaction to obtain capsule-type carbon-coated composite material Ni9S8@PC-500.
2. The Ni-MOF-derived capsule-type carbon-coated composite material according to claim 1, characterized in that, The specific method of step 1 is as follows: Dissolve 1.164g of nickel salt in 60-100ml of N,N-dimethylacetamide, stir evenly, and then add 0.5096g of 1,2,4,5-pyromellitic acid and 1.2-2.0g of polyvinylpyrrolidone in sequence, and continue stirring to obtain a homogeneous solution.
3. The Ni-MOF-derived capsule-type carbon-coated composite material according to claim 1, characterized in that, The specific method of step 2 is as follows: the homogeneous solution is transferred to a 100ml stainless steel reactor, and then the stainless steel reactor is placed in an oven at 110-140℃ for 48-120h. After filtration, it is washed several times with ethanol to obtain a green powder, and then dried in a vacuum environment to obtain the intermediate product Ni-MOF.
4. The Ni-MOF-derived capsule-type carbon-coated composite material according to claim 1, characterized in that, The specific method of step 3 is as follows: 100 mg of Ni-MOF is placed in the middle of the tubular furnace, 200-400 mg of sublimed sulfur is placed in the upper part of the tubular furnace, and then the tubular furnace is placed in the environment of Ar / H2 mixed gas at 500℃ to carry out high-temperature vulcanization reaction to obtain capsule-type carbon-coated composite material Ni9S8@PC-500.
5. A Ni-MOF-derived capsule-type carbon-coated composite material according to claim 1 or 2, characterized in that, The nickel salt is any one of nickel sulfate, nickel nitrate hexahydrate, nickel chloride, and nickel phosphate.
6. The Ni-MOF-derived capsule-type carbon-coated composite material according to claim 1, characterized in that, During the high-temperature vulcanization reaction, the mass ratio of Ni-MOF in the midstream of the tubular furnace to sublimed sulfur in the upstream of the tubular furnace is 1:2-4, and the high-temperature vulcanization time is 2-4 hours.
7. The application of Ni-MOF-derived capsule-type carbon-coated composite material Ni9S8@PC-500 according to claim 1 in supercapacitors, characterized in that, The specific application process is as follows: A Ni9S8@PC-500 / / AC HSC device is assembled using Ni9S8@PC-500 as the positive electrode and AC as the negative electrode. In this HSC device, the active mass ratio of the positive electrode to the negative electrode is 1:0.
32. Ni9S8@PC-500 exhibits significant electrochemical performance at a current density of 1 A·g⁻¹. -1 At that time, the specific capacitance of the Ni9S8@PC-500 electrode was 2351.63 F·g. -1 At a current density of 10 A·g -1 At that time, after 10,000 constant current charge-discharge cycles, the capacity retention rate of the Ni9S8@PC-500 electrode was still as high as 94%; Ni9S8@PC-500 / / AC HSC device at 827W·kg -1 It has a power density of 46 Wh·kg -1 The energy density is 7200 W·kg -1 It still maintains 31Wh·kg at high power density -1 Energy density, at 1 A·g -1 After 10,000 charge-discharge cycles at a current density, the Ni9S8@PC-500 / / AC HSC device still retains a capacity retention rate of up to 81%.
Citation Information
Patent Citations
SnX2 nano-fiber material, preparation method, anode active material, anode, secondary battery, capacitor and preparation method thereof
CN111321477A
Carbon-coated biphase metal sulfide composite material as well as preparation method and application thereof
CN117174494A