An asymmetric thermally induced polyvinylidene fluoride hollow fiber membrane and its preparation method
By designing and optimizing the structure of asymmetric thermotropic polyvinylidene fluoride hollow fiber membranes, the problem of dense separation layers caused by water-soluble diluents was solved, resulting in membrane materials with high permeability and high separation accuracy, suitable for multiple industry applications.
Patent Information
- Application Number
- CN202311806217.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-26
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-12-26
AI Technical Summary
The existing method for preparing polyvinylidene fluoride hollow fiber membranes using a water-soluble diluent system with thermally induced phases easily leads to the formation of a dense separation layer, resulting in poor permeability.
An asymmetric thermotropic polyvinylidene fluoride hollow fiber membrane structure is designed, including an intermediate finger-shaped porous layer, a separation layer, and a supporting porous layer. By controlling the phase separation process between the casting solution system and the gel bath, optimizing the use of diluent, introducing inert gas support, and performing re-stretching and heat setting, a membrane structure with high strength and high separation accuracy is formed.
The polyvinylidene fluoride hollow fiber membrane achieves high permeability and high separation accuracy, and has excellent burst pressure resistance and tensile properties, making it suitable for traditional water treatment, pharmaceutical and food industries.
Smart Images

Figure CN117815929B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of hollow fiber separation membrane technology, and in particular to an asymmetric thermally induced polyvinylidene fluoride hollow fiber membrane and its preparation method. Background Technology
[0002] Membrane separation technology has been widely used in traditional water treatment, and its applications in the pharmaceutical and food industries are increasingly attracting attention. Phase separation is currently the most common method for preparing polymer microporous membranes. Based on the difference in the driving force of phase separation, it can be mainly divided into thermally induced phase separation (TIPS) and non-solvent-induced phase separation (NIPS). Polyvinylidene fluoride (PVDF) possesses strong resistance to biodegradation, good thermal stability, high mechanical strength, resistance to chemical oxidation, and resistance to UV aging, making it one of the most favored membrane materials in the current membrane manufacturing field. Early PVDF microporous membranes were typically prepared using the NIPS method, which suffered from problems such as wide pore size distribution, low separation accuracy, numerous structural defects, poor mechanical properties, low product quality, and homogeneous competition, negatively impacting the expansion of the membrane industry and its application areas. In comparison, PVDF microporous membranes prepared by the TIPS method typically exhibit higher mechanical properties, narrower pore size distribution, more regular pore structure, and more precise separation performance. However, most of the currently disclosed TIPS membrane preparation methods are based on organic ester diluent systems, which are prone to causing the polymer to tend to grow into spheroids during the cooling and phase separation process, resulting in a decrease in the mechanical properties of the prepared membrane material. At the same time, the extraction of organic esters is difficult, and there are significant safety hazards in the production process.
[0003] In recent years, researchers have successively explored the use of water-soluble diluent systems for the preparation of polymer microporous membranes via thermally induced phase separation. For example, patent CN103252173A discloses a method for preparing polyvinylidene fluoride (PVDF) microporous membranes using thermally induced phase separation. This method utilizes the water-soluble diluent caprolactam to prepare PVDF microporous membranes. Compared to oil-soluble diluents, water-soluble diluents are easier to extract, and their production process is safer and more environmentally friendly. However, the use of water-soluble diluents inevitably leads to rapid exchange between the diluent and water at the contact interface when the PVDF hollow fiber nascent membrane is introduced into water, resulting in a thick, dense separation layer. This leads to increased fluid resistance and decreased permeation flux after membrane formation. The preparation technology of thermally induced phase PVDF hollow fiber membranes using water-soluble diluent systems that combine high strength, high separation accuracy, and high permeability still urgently needs development. Summary of the Invention
[0004] To overcome the problem that the existing method of preparing polyvinylidene fluoride (PVDF) hollow fiber membranes using a water-soluble diluent system with a thermally induced phase often leads to the formation of a dense separation layer, resulting in poor permeability of the PVDF hollow fiber membrane, this invention provides an asymmetric thermally induced phase PVDF hollow fiber membrane. This membrane possesses high strength, high separation accuracy, and high permeability. This invention also provides a method for preparing the asymmetric thermally induced phase PVDF hollow fiber membrane, which is safe, reliable, and uses environmentally friendly reagents.
[0005] To achieve the above objectives, the present invention adopts the following technical solution: In a first aspect, the present invention provides an asymmetric thermotropic polyvinylidene fluoride hollow fiber membrane, comprising an intermediate finger-shaped porous layer, a separation layer located on a first surface of the intermediate finger-shaped porous layer, and a supporting porous layer located on a second surface of the intermediate finger-shaped porous layer, wherein the thickness of the finger-shaped porous layer accounts for less than 15% of the total thickness of the membrane, and the thickness of the supporting porous layer accounts for more than 85% of the total thickness of the membrane.
[0006] The non-thermally induced polyvinylidene fluoride hollow fiber membrane prepared by this invention not only possesses the advantages of membrane materials prepared by traditional thermally induced phase preparation techniques, such as narrow pore size distribution, high separation accuracy, and excellent resistance to burst pressure, tensile fracture force, and elongation, but also effectively penetrates the dense region between the membrane separation layer and the membrane support layer, significantly improving the permeation performance of the membrane material.
[0007] Furthermore, the thickness of the separation layer is less than 3 micrometers, and the average pore size of the separation layer is less than 300 nanometers.
[0008] Furthermore, the thickness of the asymmetric thermotropic polyvinylidene fluoride hollow fiber membrane is 100-300 micrometers, the tensile strength is greater than 6 MPa, and the elongation at break is greater than 100%.
[0009] Secondly, the present invention provides a method for preparing the above-mentioned asymmetric thermally induced polyvinylidene fluoride hollow fiber membrane, comprising the following steps: S1. Mix polyvinylidene fluoride, water-soluble diluent, high molecular weight glycol condensate, nanoporous agent and processing aid evenly to obtain a mixture; S2. The mixture obtained in S1 is extruded through a twin-screw extruder and supported by an inert material in the inner cavity to form a hollow fiber nascent membrane; S3. The hollow fiber nascent membrane obtained in S2 is placed in a gel bath containing interface-inducing components for curing, cleaning, and drying to obtain an asymmetric thermotropic polyvinylidene fluoride hollow fiber membrane.
[0010] This invention innovatively designs a thermo-phase film-forming formulation for a water-soluble diluent in polyvinylidene fluoride (PVDF) membrane materials and a thermo-phase separation extrusion spinning process. By controlling the instantaneous phase separation characteristics when the casting solution system and the gel bath system come into contact, the phase separation rate in the lower dimension region of the membrane separation layer is controlled in the traditional thermo-phase process. This results in the preparation of a multilayer asymmetric thermo-phase PVDF hollow fiber membrane with a surface separation layer, an internal double continuous support layer, and a finger-like pore layer located between the two.
[0011] Furthermore, in S1, the mass percentage of the raw materials used to prepare the mixture is as follows: polyvinylidene fluoride 25-40%, water-soluble diluent 30-50%, high molecular weight glycol condensate 10-25%, nanoporous agent 1-10%, and processing aid 1-3%.
[0012] Preferably, in step S1, the raw materials for preparing the mixture further include a hydrophilic polymer with a mass fraction of 1-5%, wherein the hydrophilic polymer is one or a mixture of polymethyl methacrylate, polyvinylpyrrolidone, polyvinyl alcohol, and polyurethane.
[0013] Introducing hydrophilic polymers into the formulation system can improve the hydrophilicity of polyvinylidene fluoride hollow fiber membranes.
[0014] Furthermore, in S1, the high molecular weight diol condensate is a diol condensate with a molecular weight greater than 5000; The nanoporogen is an oxide nanomaterial.
[0015] High molecular weight diol condensates with a molecular weight greater than 5000 are used to control the structural connectivity of the membrane and the viscosity of the membrane mixture during melt extrusion.
[0016] Furthermore, the high molecular weight diol is one or more of polyethylene glycol, polypropylene glycol, and ethylene glycol / propylene glycol copolymer; The nanoporous agent is one or more of silicon dioxide, zinc oxide, magnesium oxide and iron oxide, or a mixture thereof.
[0017] Furthermore, in S1, the water-soluble diluent is one or a mixture of cyclohexanone, caprolactam, and lactone. The processing aid is a mixture of antioxidant and lubricant, and the lubricant is a fatty acid amide lubricant with a mass ratio of antioxidant to lubricant of (2-8):1.
[0018] Furthermore, in S1, the lactone is butyrolactone or caprolactone.
[0019] Cyclohexanone, caprolactam, butyrolactone, and caprolactone are water-soluble. Using water-soluble diluents can make the production process safer. At the same time, these diluents are easily biodegradable and have low toxicity, which is conducive to the large-scale production of membrane products.
[0020] Preferably, the antioxidant is one or a mixture of antioxidant 1010, antioxidant 264 and antioxidant 1076; the fatty acid amide lubricant is one or a mixture of stearic acid, stearamide, stearate and oleamide.
[0021] Furthermore, in S2, the inert material support in the inner cavity is provided by an inert gas or an inert liquid grease; the inert gas is nitrogen or argon. Inert liquid greases are vegetable oils and / or mineral oils.
[0022] Preferably, the vegetable oil includes soybean oil, epoxidized soybean oil, peanut oil, and castor oil; The mineral oil includes paraffin oil and silicone oil.
[0023] Furthermore, in S3, the gel bath containing the interface-inducing component is an aqueous solution containing 0.5-8% by mass of a surfactant and 0-10% by mass of an aqueous diluent, wherein the surfactant is one or more of anionic surfactants, nonionic surfactants and zwitterionic surfactants.
[0024] Furthermore, in S3, the aqueous diluent is cyclohexanone, caprolactam, butyrolactone, and caprolactone.
[0025] Furthermore, the anionic surfactant is one or a mixture of sodium dodecyl sulfate, sodium dodecyl sulfonate, and sodium dodecylbenzene sulfonate; The nonionic surfactant is one or a mixture of Tween, polyoxyethylene ether, and Triton. The zwitterionic surfactant is one or more of dodecyl dimethyl betaine, tetradecyl dimethyl betaine, and octadecyl dimethyl betaine, or a mixture thereof.
[0026] Furthermore, the preparation method further includes: S4. The asymmetric thermo-induced polyvinylidene fluoride hollow fiber membrane obtained in S3 is restretched and heat-set.
[0027] Re-stretching and heat setting processes can improve the separation performance and mechanical properties of polymer hollow fiber membranes.
[0028] Therefore, the present invention has the following beneficial effects: 1) This invention targets the thermo-induced phase diluent system. Through the design of the casting solution component system, it optimizes the green water-soluble diluent system, avoiding the problems of easy crystallization of polyvinylidene fluoride and difficulty in removing organic esters during the phase separation process caused by the large-scale use of oil-soluble organic esters in traditional methods. The thermo-induced phase preparation process of asymmetric polyvinylidene fluoride hollow fiber membranes provided by this invention is based on the thermo-induced phase separation mechanism and water extraction diluent. The wastewater is easily biochemically treated, making it more environmentally friendly and safer. The prepared asymmetric polyvinylidene fluoride hollow fiber membrane has low leaching residue and wider application prospects. 2) This invention further optimizes the control design of the thermally induced phase separation process. By designing the composite ratio of surfactant and diluent in the gel bath, the interfacial phase separation at the micro-region depth of the contact interface is controlled during the instantaneous immersion of the nascent polyvinylidene fluoride hollow fiber membrane in water. This allows for the controllable shaping of the micro-region structure near the outer surface of the membrane fibers, eliminating the excessively thick near-surface dense stacking layer while retaining a high-precision thin separation layer. This balances the high permeability and high separation accuracy of the membrane fibers, realizing the innovative design concept and successful preparation of asymmetric thermally induced polyvinylidene fluoride hollow fiber membranes. 3) This invention further optimizes the internal support of the nascent polyvinylidene fluoride hollow fiber membrane during the thermally induced phase process. By using inert gas or inert grease as the internal support of the membrane fibers, it ensures that the nascent membrane fibers do not undergo significant temperature transfer or mass exchange before entering the gel bath. This allows the main body of the membrane fibers to undergo thermally induced phase separation of the casting solution due to temperature transfer only after entering the gel bath. This makes the internal support porous layer of the prepared polyvinylidene fluoride hollow fiber membrane more uniform, reduces the tendency of PVDF to induce spherulite growth, and makes it more complete, thereby giving the prepared membrane fiber material excellent mechanical properties. 4) The asymmetric thermotropic polyvinylidene fluoride hollow fiber membrane prepared by the technology of this invention has excellent separation performance, tensile strength, elongation at break and burst pressure resistance. It has a narrow pore size distribution and low leaching rate during use. It is not only suitable for traditional water treatment applications, but also particularly suitable for application and promotion in the pharmaceutical, food and other life and health and dietary health industries. Attached Figure Description
[0029] Figure 1 A panoramic electron micrograph of the cross-section of the thermo-induced polyvinylidene fluoride hollow fiber membrane prepared in Example 1.
[0030] Figure 2 An electron micrograph of the cross section near the outer surface of the thermo-induced polyvinylidene fluoride hollow fiber membrane prepared in Example 1.
[0031] Figure 3A panoramic electron micrograph of the cross-section of the thermo-induced polyvinylidene fluoride hollow fiber membrane prepared in Example 2.
[0032] Figure 4 This is an electron micrograph of the cross section of the thermo-induced polyvinylidene fluoride hollow fiber membrane prepared in Example 2, near the outer surface.
[0033] Figure 5 A panoramic electron micrograph of the cross-section of the thermo-induced polyvinylidene fluoride hollow fiber membrane prepared for Comparative Example 1.
[0034] Figure 6 An electron micrograph of the cross section of the thermo-induced polyvinylidene fluoride hollow fiber membrane prepared for Comparative Example 1, near the outer surface. Detailed Implementation
[0035] The present invention will be further described below with reference to the accompanying drawings and specific implementation methods.
[0036] Example 1 A thermo-induced polyvinylidene fluoride hollow fiber membrane is prepared by the following steps: Step 1): Add 30% by mass of polyvinylidene fluoride, 47% by mass of caprolactam, 15% by mass of polyethylene glycol 10000, 6% by mass of nano zinc oxide, 1.5% by mass of antioxidant 1010 and 0.5% by mass of stearic acid to a high-speed mixer and mix evenly. Step 2): Set the temperature of each section of the twin-screw extruder to 165℃-185℃ and the twin-screw speed to 230 rpm. Feed the uniformly mixed mixture into the twin-screw extruder through the feeder and extrude it through the hollow fiber spinneret to produce hollow fibers. The core support is nitrogen. Step 3): The hollow fibers are introduced into a gel bath at 15°C for curing. The gel bath is prepared by adding 3 parts by weight of sodium dodecyl sulfate and 2 parts by weight of caprolactam to every 100 parts by weight of tap water. The air gap is 10 cm. The cured hollow fibers are then transferred to 0.5% hydrochloric acid for 24 hours and then transferred to room temperature water. After washing and drying, an asymmetric thermotropic polyvinylidene fluoride hollow fiber membrane is obtained.
[0037] The polyvinylidene fluoride hollow fiber membrane prepared in Example 1 was observed by electron microscopy. A panoramic electron micrograph of the cross-section of the polyvinylidene fluoride hollow fiber membrane is shown below. Figure 1 As shown, the overall thickness of the membrane is approximately 180 micrometers. A finger-like pore layer, approximately 10 micrometers thick, is visible near the outer surface; above this is a separation layer; and below this is a double continuous support layer. A further magnified image of the area near the outer surface is shown below. Figure 2 As shown, its finger-like apertures are almost connected to the underlying double continuous support layer, and its separation layer thickness is about 500 nanometers.
[0038] Example 2 A thermo-induced polyvinylidene fluoride hollow fiber membrane is prepared by the following steps: Step 1): Add 26% by weight of polyvinylidene fluoride, 45% by weight of caprolactone, 18.5% by weight of polyethylene glycol 5000, 8% by weight of nano zinc oxide, 2% by weight of antioxidant 1078, and 0.5% by weight of stearamide to a high-speed mixer and mix thoroughly. Then add an additional 5 parts by weight of polymethyl methacrylate and mix thoroughly. Step 2): Set the temperature of each section of the twin-screw extruder to 160℃-175℃ and the twin-screw speed to 210 rpm. Feed the uniformly mixed mixture into the twin-screw extruder through the feeder, and extrude it through the hollow fiber spinneret to form hollow fibers. The core support is argon gas. Step 3): The hollow fibers are introduced into a gel bath at 10°C for curing. The gel bath is prepared by adding 8 parts by weight of sodium dodecyl sulfate and 10 parts by weight of caprolactone to every 100 parts by weight of tap water. The air gap is 5 cm. The cured hollow fibers are then transferred to 1% hydrochloric acid for 24 hours, then transferred to room temperature water, washed, and dried to obtain an asymmetric thermotropic polyvinylidene fluoride hollow fiber membrane.
[0039] The polyvinylidene fluoride hollow fiber membrane prepared in Example 2 was observed by electron microscopy. Figure 3 This is a cross-sectional panoramic electron microscope image of the polyvinylidene fluoride hollow fiber membrane prepared in Example 2. The membrane thickness is approximately 280 micrometers. A finger-like pore layer with a thickness of approximately 40 micrometers is visible near the outer surface of the membrane; above this is a separation layer; and below is a double continuous support layer. Figure 4 This is a further magnified photograph of the area near the outer surface of the polyvinylidene fluoride hollow fiber membrane prepared in Example 2. It can be seen that its finger-like pores are almost connected to the underlying double continuous support layer, and the thickness of its separation layer is about 400 nanometers.
[0040] Example 3 A thermo-induced polyvinylidene fluoride hollow fiber membrane is prepared by the following steps: Step 1): Add 28% by mass of polyvinylidene fluoride, 45% of γ-butyrolactone, 15% of polyethylene glycol 20000, 10% of nano silica, 1.5% of antioxidant 1010 and 0.5% of stearic acid to a high-speed mixer and mix evenly. Step 2): Set the temperature of each section of the twin-screw extruder to 165℃-185℃ and the twin-screw speed to 230 rpm. Feed the uniformly mixed mixture into the twin-screw extruder through the feeder and extrude it through the hollow fiber spinneret to produce hollow fibers. The core support is nitrogen. Step 3): The hollow fibers are introduced into a gel bath at 15°C for curing. The gel bath is prepared by adding 5 parts by weight of sodium dodecylbenzenesulfonate and 10 parts by weight of γ-butyrolactone to every 100 parts by weight of tap water. The air gap is 15 cm. The cured hollow fibers are transferred to 4% NaOH and soaked at 50°C for 8 hours. Then they are transferred to room temperature water, washed, and dried to obtain an asymmetric thermotropic polyvinylidene fluoride hollow fiber membrane.
[0041] Electron microscopy revealed that the prepared polyvinylidene fluoride hollow fiber membrane had an overall thickness of approximately 170 micrometers, with a finger-like pore layer near the outer surface of the membrane, which had a thickness of approximately 20 micrometers.
[0042] Example 4 A thermo-induced polyvinylidene fluoride hollow fiber membrane is prepared by the following steps: Step 1): Add 30% by mass of polyvinylidene fluoride, 47% by mass of caprolactam, 15% by mass of polyethylene glycol 10000, 6% by mass of nano zinc oxide, 1.5% by mass of antioxidant 1010 and 0.5% by mass of stearic acid to a high-speed mixer and mix evenly. Step 2): Set the temperature of each section of the twin-screw extruder to 165℃-185℃ and the twin-screw speed to 230 rpm. Feed the uniformly mixed mixture into the twin-screw extruder through the feeder and extrude it through the hollow fiber spinneret to produce hollow fibers. The core support is nitrogen. Step 3): The hollow fibers are introduced into a gel bath at 15°C for curing. The gel bath is prepared by adding 3 parts by weight of sodium dodecyl sulfate and 2 parts by weight of caprolactam to every 100 parts by weight of tap water. The air gap is 10 cm. The cured hollow fibers are then transferred to 0.5% hydrochloric acid for 24 hours and then transferred to room temperature water. After washing and drying, an asymmetric thermotropic polyvinylidene fluoride hollow fiber membrane is obtained. Step 4): Stretch the asymmetric thermo-induced polyvinylidene fluoride hollow fiber membrane by 50% in water at 70°C.
[0043] Comparative Example 1 A thermo-induced polyvinylidene fluoride hollow fiber membrane is prepared by the following steps: Step 1): Add 30% by mass of polyvinylidene fluoride, 47% by mass of caprolactam, 15% by mass of polyethylene glycol 10000, 6% by mass of nano zinc oxide, 1.5% by mass of antioxidant 1010 and 0.5% by mass of stearic acid to a high-speed mixer and mix evenly. Step 2): Set the temperature of each section of the twin-screw extruder to 165℃-185℃ and the twin-screw speed to 230 rpm. Feed the uniformly mixed mixture into the twin-screw extruder through the feeder and extrude it through the hollow fiber spinneret to produce hollow fibers. The core support is nitrogen. Step 3): Introduce the hollow fiber into water at 15°C for curing, with an air gap of 10 cm; transfer the cured hollow fiber to 0.5% hydrochloric acid for 24 hours, then transfer it to room temperature water, wash and dry it to obtain a thermo-induced polyvinylidene fluoride hollow fiber membrane.
[0044] The polyvinylidene fluoride hollow fiber membrane prepared in Comparative Example 1 was also observed using electron microscopy. Figure 5 As shown in the panoramic electron microscope image of the cross-section of the polyvinylidene fluoride hollow fiber membrane prepared in Comparative Example 1, a relatively thick dense layer with a thickness of approximately 20 micrometers is visible near the outer surface of the membrane; below this dense layer is a gradient-increasing bicontinuous support layer. Figure 6 This is a further magnified photograph of the polyvinylidene fluoride hollow fiber membrane near its outer surface, prepared in Comparative Example 1. Figure 6 It can be seen that the area near its outer surface is very dense.
[0045] Comparative Example 2 A hollow fiber membrane is prepared by the following steps: Step 1): Add 30% by mass of polyvinylidene fluoride, 47% by mass of caprolactam, 15% by mass of polyethylene glycol 10000, 6% by mass of nano zinc oxide, 1.5% by mass of antioxidant 1010 and 0.5% by mass of stearic acid to a high-speed mixer and mix evenly. Step 2): Set the temperature of each section of the twin-screw extruder to 165℃-185℃ and the twin-screw speed to 230 rpm. Feed the uniformly mixed mixture into the twin-screw extruder through the feeder and extrude it through the hollow fiber spinneret to produce hollow fibers. The core support is nitrogen. Step 3): The hollow fibers are introduced into a gel bath at 15°C for curing. The gel bath is prepared by adding 2 parts by weight of caprolactam to every 100 parts by weight of tap water. The air gap is 10 cm. The cured hollow fibers are then transferred to 0.5% hydrochloric acid for 24 hours and then transferred to room temperature water. After washing and drying, an asymmetric thermotropic polyvinylidene fluoride hollow fiber membrane is obtained.
[0046] No finger-like pore structures were observed on the cross-section near the outer surface of the hollow fiber membrane obtained in Comparative Example 2.
[0047] Comparative Example 3 A hollow fiber membrane is prepared by the following steps: Step 1): Add 30% by mass of polyvinylidene fluoride, 47% by mass of caprolactam, 15% by mass of polyethylene glycol 10000, 6% by mass of nano zinc oxide, 1.5% by mass of antioxidant 1010 and 0.5% by mass of stearic acid to a high-speed mixer and mix evenly. Step 2): Set the temperature of each section of the twin-screw extruder to 165℃-185℃ and the twin-screw speed to 230 rpm. Feed the uniformly mixed mixture into the twin-screw extruder through the feeder and extrude it through the hollow fiber spinneret to produce hollow fibers. The core support is nitrogen. Step 3): The hollow fibers are introduced into a gel bath at 15°C for curing. The gel bath is prepared by adding 3 parts by weight of sodium dodecyl sulfate and 15 parts by weight of caprolactam to every 100 parts by weight of tap water. The air gap is 10 cm. The cured hollow fibers are then transferred to 0.5% hydrochloric acid for 24 hours and then transferred to room temperature water. After washing and drying, an asymmetric thermotropic polyvinylidene fluoride hollow fiber membrane is obtained.
[0048] No finger-like pore structures were observed on the cross-section near the outer surface of the hollow fiber membrane obtained in Comparative Example 3.
[0049] The polyvinylidene fluoride hollow fiber membranes prepared in the above examples and comparative examples were used for pure water flux testing, tensile testing and pore size testing, and the results are shown in Table 1.
[0050] Table 1. Performance of polyvinylidene fluoride hollow fiber membranes prepared in Examples 1-4 and Comparative Examples 1-3
[0051] In summary, the asymmetric thermotropic polyvinylidene fluoride hollow fiber membrane prepared by this invention retains excellent mechanical properties. Furthermore, the induced formation of finger-like pores connects the dense region between the separation layer and the support layer, significantly reducing the fluid resistance of the membrane material and resulting in a substantial increase in membrane water flux. Simultaneously, pore size testing shows that the separation accuracy of the membrane material obtained by this invention remains significantly unchanged.
[0052] In Comparative Example 1, the gel bath used water; in Comparative Example 2, the gel bath contained no surfactant; and in Comparative Example 3, the gel bath contained an excessively high amount of diluent. This resulted in the polyvinylidene fluoride hollow fiber membranes prepared in Comparative Examples 1-3 exhibiting excellent mechanical properties, but due to the extremely dense near-separation layer region, the membrane material suffered from high fluid resistance and very low water flux. This demonstrates that the gel bath of the present invention, through control of the gel interface characteristics, eliminates excessively thick near-surface dense deposits while retaining a high-precision thin separation layer, thus balancing high permeability and high separation accuracy of the membrane material.
Claims
1. A method for preparing an asymmetric thermally induced polyvinylidene fluoride hollow fiber membrane, characterized in that, The membrane includes an intermediate finger-shaped porous layer, a separation layer located on a first surface of the intermediate finger-shaped porous layer, and a supporting porous layer located on a second surface of the intermediate finger-shaped porous layer. The thickness of the finger-shaped porous layer accounts for less than 15% of the total thickness of the membrane, and the thickness of the supporting porous layer accounts for more than 85% of the total thickness of the membrane. The preparation of asymmetric thermally induced polyvinylidene fluoride hollow fiber membranes includes the following steps: S1. Mix polyvinylidene fluoride, water-soluble diluent, high molecular weight glycol condensate, nanoporous agent and processing aid evenly to obtain a mixture, wherein the high molecular weight glycol condensate is a glycol condensate with a molecular weight greater than 5000. S2. The mixture is extruded through a twin-screw extruder and supported by an inert material in the inner cavity to form a hollow fiber nascent membrane; S3. The hollow fiber nascent membrane is placed in a gel bath containing an interface-inducing component for curing, cleaning, and drying to obtain an asymmetric thermotropic polyvinylidene fluoride hollow fiber membrane. The gel bath containing the interface-inducing component is an aqueous solution containing 0.5-8% by mass of a surfactant and a water-soluble diluent. The water-soluble diluent has a mass fraction of >0% and ≤10%. The surfactant is one of sodium dodecyl sulfate and sodium dodecylbenzene sulfonate, and the water-soluble diluent is one of caprolactam, caprolactone, and γ-butyrolactone.
2. The preparation method according to claim 1, characterized in that, The thickness of the separation layer is less than 3 micrometers, and the average pore size of the separation layer is less than 300 nanometers.
3. The preparation method according to claim 1, characterized in that, The thickness of the asymmetric thermotropic polyvinylidene fluoride hollow fiber membrane is 100-300 micrometers, the tensile strength is greater than 6 MPa, and the elongation at break is greater than 100%.
4. The preparation method according to claim 1, characterized in that, In step S1, the mass percentage of the raw materials used to prepare the mixture is as follows: 25-40% polyvinylidene fluoride, 30-50% water-soluble diluent, 10-25% high molecular weight glycol condensate, 1-10% nanoporous agent, and 1-3% processing aid.
5. The preparation method according to claim 1 or 4, characterized in that, In S1, the nanoporous agent is an oxide nanomaterial.
6. The preparation method according to claim 1 or 4, characterized in that, In S1, the water-soluble diluent is one or more of cyclohexanone, caprolactam, and lactone; the processing aid is a mixture of antioxidant and lubricant, the lubricant is a fatty acid amide lubricant, and the mass ratio of antioxidant to lubricant is (2-8):
1.
7. The preparation method according to claim 1, characterized in that, In S2, the inert material support in the inner cavity is provided by an inert gas or an inert liquid grease; the inert gas is nitrogen or argon; the inert liquid grease is vegetable oil and / or mineral oil.
8. The preparation method according to claim 1, characterized in that, The preparation method further includes: S4, re-stretching and heat-setting the asymmetric thermo-induced polyvinylidene fluoride hollow fiber membrane obtained in S3.
Citation Information
Patent Citations
Method for preparation of polyvinylidene fluoride membrane by thermally induced phase separation
CN103252173A
Method for producing density and gradient sectional porous ultrafiltration membrane
CN101073750A
High-flux polyvinylidene fluoride hollow fiber membrane
CN103111189A
High-strength self-supporting polyvinylidene fluoride hollow fiber membrane and preparation method thereof