A drawing friction protection surface treatment composition with good lubricity and its preparation method and application
By using a combination of grease, phosphate and other ingredients during the drawing process, a protective film layer is formed, which solves the problem of wire damage and water absorption during the drawing process, achieves efficient lubrication and anti-rust effects, and replaces Traditional phosphating liquid and saponification liquid improve the efficiency and environmental protection of cold plastic processing.
Patent Information
- Application Number
- CN202311727866.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-15
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-12-15
AI Technical Summary
In the existing technology, the wire is easily damaged and the mold is scratched during the drawing process, and the wire is easy to absorb water after surface treatment with coating agents on the market, which is not conducive to subsequent processing. There is a lack of good coating and drawing friction surface treatment agents that can replace phosphorus saponification. .
Provides a drawing friction protection surface treatment composition with good lubricity, including grease substances, phosphate esters, organic molybdenum salts, succinimide, hydroxyethyl acrylate and other ingredients, prepared through specific mixing and stirring steps , forming a protective film layer that can be directly adsorbed on the wire to increase lubricity and rust prevention.
The composition increases the lubricity and rust resistance of the wire, reduces the process and cost, has a pulling force of 100-130N, and a salt spray resistance time of more than 180 minutes. It is better than traditional phosphorus saponification and wire drawing powder, and improves processing efficiency. and reduce dust generation.
Smart Images

Figure BDA0004609184460000011 
Figure BDA0004609184460000021 
Figure BDA0004609184460000051
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal surface treatment, and in particular to a drawing friction protection surface treatment composition with good lubricity, a preparation method and application thereof. Background Art
[0002] In the application of cold plastic processing, the wire needs to be surface treated before it can be drawn. During the drawing process, the wire rubs against the mold. If the surface of the wire is not surface treated, the wire will be damaged during the drawing process and will scratch the mold. There are many types of surface treatment agents, including phosphorus saponification and direct treatment coating agents, but phosphorus saponification treatment requires multiple troughs, and the coating agent on the market is easy to absorb water on the wire surface after surface treatment, which is not conducive to subsequent processing. Therefore, the development of a drawing friction surface treatment agent that can replace phosphorus saponification and has a good coating is a demand in the current market. Summary of the invention
[0003] In order to overcome the shortcomings and deficiencies in the prior art, the purpose of the present invention is to provide a drawing friction protection surface treatment composition with good lubricity and a preparation method and application thereof, wherein the composition replaces the use of traditional phosphating solution and saponification solution, as well as subsequent wire drawing powder, and the composition can be directly adsorbed on the wire for drawing, thereby saving process and cost.
[0004] The purpose of the present invention is achieved through the following technical solutions:
[0005] The first object of the present application is to provide a surface treatment composition for pulling friction protection with good lubricity, which comprises the following raw materials in weight percentage:
[0006]
[0007]
[0008] The balance is water.
[0009] Furthermore, the lubricant is a grease substance; the grease substance is at least one of oleic acid glyceryl ester, pentaerythritol ester, and trimethylolpropane ester.
[0010] Furthermore, the extreme pressure additive includes phosphate ester; specifically, the phosphate ester is at least one of butyl phosphate ester, diethyl phenyl phosphate ester, aryl phosphate ester, amino phosphoroester, and tricresyl phosphate.
[0011] Furthermore, the anti-wear agent includes an organic molybdenum salt.
[0012] Furthermore, the dispersant is at least one of succinimide, polyimide and polyacrylamide.
[0013] Furthermore, the viscosity additive is at least one of hydroxyethyl acrylate and ether-containing methacrylate.
[0014] Furthermore, the corrosion inhibitor includes an alkylamine.
[0015] Furthermore, the rust inhibitor includes an alkyl succinic acid derivative.
[0016] The second object of the present application is to provide a method for preparing a drawing friction protection surface treatment composition with good lubricity, comprising the following steps:
[0017] (1) preparing materials according to the weight percentage of each raw material of the drawing friction protection surface treatment composition; taking a lubricant, adding a surfactant, mixing at 70° C. for 20 minutes, slowly adding an appropriate amount of water, and stirring for 30 minutes to obtain a mixture A;
[0018] (2) In another reactor, add an appropriate amount of extreme pressure additive to an appropriate amount of water, add a corrosion inhibitor; then add an anti-wear agent and a viscosity additive, mix well, and obtain a mixture B;
[0019] (3) Mixing mixture A and mixture B, stirring evenly, then adding a rust inhibitor and a dispersant; stirring until uniform, to obtain a drawing friction protection surface treatment composition.
[0020] The third purpose of the present application is to provide an application of a drawing friction protection surface treatment composition with good lubricity, and to apply the drawing friction protection surface treatment composition to cold plastic processing.
[0021] The beneficial effects of the present invention are:
[0022] 1. The composition described in the present application uses an extreme pressure additive and a lubricant together to increase the lubrication effect, because the phosphate ester substance forms a film layer on the surface of the wire, which increases the lubricity and anti-rust protective layer. At the same time, the phosphate ester substance can also maintain the stability of the solution; the dispersant and the viscosity additive work together, in addition to increasing the stability of the solution, and can also play an anti-rust role. The amide structure of the dispersant can enhance the stability of the viscosity additive, and together form a strong intermolecular force and a network structure on the surface of the wire, thereby enhancing the corrosion resistance of the wire.
[0023] 2. The composition described in this application replaces the traditional phosphating solution and saponifying solution, as well as the subsequent use of wire drawing powder, and can be directly adsorbed on the wire for drawing, saving process and cost. The composition is used in the cold plastic processing process, and the maximum drawing force after drawing is 100-130N, and the corrosion is titrated by salt spray test, and the salt spray resistance time is more than 180min; while the maximum drawing force of conventional phosphating saponification and wire drawing powder is 135-150N, and the salt spray resistance time of normal phosphating soap and wire drawing powder is 60-120min.
[0024] 3. By using the composition, the phosphorus saponification process is directly updated to surface treatment, which improves efficiency, and the composition is environmentally friendly, and can be directly drawn. The surface of the wire after soaking is smooth with a film layer and the tank liquid is easy to control. Moreover, when used, the composition is in liquid form and does not need to be dissolved, which saves the time of dissolving powder substances and does not generate dust. DETAILED DESCRIPTION
[0025] In order to facilitate the understanding of those skilled in the art, the present invention is further described below in conjunction with embodiments, and the contents mentioned in the implementation modes are not intended to limit the present invention.
[0026] As used herein, "and / or" includes the term of any and all combinations of one or more associated listed items. The terms used herein are only used to describe specific embodiments and are not intended to limit the present invention. As used herein, the singular forms "a", "an", "an" and "the" are also intended to include the plural forms, unless the context clearly indicates otherwise. It is further understood that "including", when used in this specification, specifies the stated features, integers, steps, operations, elements and / or compositions, but does not exclude the existence or addition of one or more other features, integers, steps, operations, elements, compositions and / or combinations thereof.
[0027] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs. It is further understood that terms, such as defined in commonly used dictionaries, are interpreted in accordance with their meanings in the context of the relevant art and are not in an idealized or overly formal sense unless explicitly so defined herein.
[0028] The exemplary invention described herein may appropriately lack any one or more element limitations that are not specifically disclosed herein. Therefore, the terms "comprise", "include", "contain", etc. should be understood broadly and non-restrictively. In addition, the terminology used herein is used as a description, not a limitation, and it is unintentional to use these terminology expressions that do not include any equivalent characteristics, but only describe some of their characteristics, but various modifications are possible within the scope of the present invention according to the rights. Therefore, although the present invention has been specifically disclosed by preferred embodiments and optional features, the modifications disclosed herein to embody the changes of the present invention may be recorded by those skilled in the art, and such modifications and changes will be considered to be within the scope of the present invention.
[0029] The raw materials or reagents used in the embodiments of the present invention and the comparative examples are all purchased from mainstream manufacturers in the market. The manufacturer or concentration is not specified, and they are all analytically pure raw materials or reagents that can be routinely obtained. As long as the expected effect can be played, there is no particular restriction. The instruments and equipment involved in reactions, mixing, etc. in the present embodiment are all purchased from major manufacturers in the market. As long as the expected effect can be played, there is no particular restriction. If specific techniques or conditions are not specified in the present embodiment, the techniques or conditions described in the literature in this area or according to the product specification are carried out.
[0030] In order to develop a drawing friction surface treatment agent that can replace phosphorus saponification and has a good coating, the present application provides a drawing friction protection surface treatment composition with good lubricity, which includes the following raw materials in weight percentage:
[0031]
[0032] The balance is water.
[0033] In one embodiment, the lubricant is a grease-like substance; the lubricant is at least one of oleic acid glyceride (for example, CAS No.: 25496-72-4, or CAS No.: 2442-61-7), pentaerythritol ester, and trimethylolpropane ester. The lubricant (grease-like substance) is mainly adsorbed on the surface of the wire by intermolecular forces, and plays a good lubricating role. The weight percentage of the lubricant in the composition is 20-35%, for example, it can be any value of 10%, 15%, 20%, 25%, 30%, and 35%, and it is sufficient to meet 20-35%.
[0034] In one embodiment, the extreme pressure additive includes phosphate ester; specifically, the phosphate ester is at least one of butyl phosphate (CAS No.: 947601-92-5), diethylphenyl phosphate (CAS No.: 6231-03-4), aryl phosphate (CAS No.: 26967-76-0), amino phosphate (CAS No.: 2015-56-7), and tricresyl phosphate (CAS No.: 1330-78-5); the phosphate ester can be oxidized on the surface of the wire to generate anionic phosphate, which serves as a connecting ligand of the polyferric chelate, and generates a thin high-viscosity film layer under high temperature and high pressure during the wire drawing process, thereby increasing the thickness of the film, thereby better protecting the wire and the mold. The weight percentage of the extreme pressure additive in the composition is 8-15%, for example, it can be any value of 8%, 9%, 10%, 11%, 12%, and 15%, and it is sufficient to meet 8-15%.
[0035] In one embodiment, the anti-wear agent includes an organic molybdenum salt; the anti-wear agent is at least one of dialkylphosphodithiomolybdenum salt (CAS No.: 72030-25-2), dialkyldithiocarbamate molybdenum (CAS No.: 71342-89-7), and epoxy acid molybdenum (for example, CAS No.: 90901-24-9); the organic molybdenum salts are all nanometers. The molybdenum atoms in the organic molybdenum salt are parallelepiped structures. When the organic matter formed by it is strongly applied, the weak strength between the planes causes the crystals to shear, forming a lubricated layered distribution, which plays a good wear-resistant role. The weight percentage of the anti-wear agent in the composition is 2-6%, for example, it can be any value of 2%, 3%, 4%, 5%, 6%, and 8%, and it is sufficient to meet 2-6%.
[0036] In one embodiment, the dispersant is at least one of succinimide (molecular weight 8000), polyimide (molecular weight 6000), and polyacrylamide (molecular weight 4000); succinimide, polyimide, or polyacrylamide can be well dissolved in water and can associate well with polar oily substances to ensure the stability of the solution. The weight percentage of the dispersant in the composition is 3-9%, for example, it can be any value of 3%, 4%, 5%, 6%, 8%, 9%, and it is sufficient to meet 3-9%.
[0037] In one embodiment, the viscosity additive is at least one of hydroxyethyl acrylate and ether-containing methacrylate (CAS No.: 951244-55-6). Hydroxyethyl acrylate or ether-containing methacrylate has good thermal stability and oxidative stability, and the stability of the solution is ensured by the network structure of the alkyl side chains and the lubricant.
[0038] The weight percentage of the viscosity additive in the composition is 2.8-7.2%, for example, it can be any value of 2.8%, 3%, 4.2%, 5.5%, 6.1%, 7.2%, as long as it satisfies 2.8-7.2%.
[0039] In one embodiment, the corrosion inhibitor includes an alkylamine; the alkylamine is at least one of monoamine (monohexanolamine, CAS No.: 141-43-5), diamine (diethanolamine, CAS No.: 111-42-2), triamine (triethanolamine: 102-71-6), ethylenediamine, triethylenetetramine and tetraethylenepentamine. The alkylamine is mainly used to protect the stability of the emulsion, adjust the pH of the solution, and reduce the production of bacteria. The weight percentage of the corrosion inhibitor in the composition is 3-8%, for example, it can be any value of 3%, 4%, 5%, 6%, 8%, and it is sufficient to meet 3-8%.
[0040] In one embodiment, the rust inhibitor includes an alkyl succinic acid derivative; the alkyl succinic acid derivative is at least one of metal sulfonates (such as calcium methanesulfonate CAS No.: 58131-47-8, magnesium taurate), ethanolamine borate (CAS No.: 283-56-7), and sulfonic acid amine (CAS No.: 7773-06-0); the alkyl succinic acid derivative can first replace the water molecules adsorbed on the metal surface, and then the lone pair of electrons on N can form a certain chemical bond with the empty orbital formed by the metal atom at the surface defect of the oxide layer, so a protective layer can be formed on the metal surface, and good cathode corrosion inhibition performance can also be formed on the metal surface. The weight percentage of the rust inhibitor in the composition is 1-7%, for example, it can be any value of 1%, 2%, 3%, 4%, 5%, 6%, and 7%, and it is sufficient to meet 1-7%.
[0041] In one embodiment, the surfactant includes a nonionic surfactant and an anionic emulsifier, and the surfactant is used to emulsify esters; the surfactant is at least one of alkylphenol polyoxyethylene ether (Tx-10), lauryl alcohol polyoxyethylene ether (CAS No.: 9002-92-0), sodium lauryl sulfate (CAS No.: 73296-89-6), and triethanolamine oleate (CAS No.: 88107-10-2). The surfactant is mainly used to emulsify lubricating substances that are not easily soluble. The weight percentage of the surfactant in the composition is 8-15%, for example, it can be any value of 8%, 9%, 10%, 11%, 12%, and 15%, and it is sufficient to meet 8-15%.
[0042] The technical solution of the present application is described below through specific embodiments:
[0043] Example 1
[0044] A method for preparing a drawing friction protection surface treatment composition with good lubricity comprises the following steps:
[0045] (1) According to the weight percentage of each raw material of the drawing friction protection surface treatment composition, the materials are prepared; the composition, in units of weight percentage, includes the following raw materials:
[0046]
[0047] Lauryl polyoxyethylene ether 6%;
[0048] The balance is water;
[0049] Take lubricant, add surfactant, mix at 70°C for 20 min, slowly add appropriate amount of water, stir for 30 min, and obtain mixture A;
[0050] (2) In another reactor, add an appropriate amount of extreme pressure additive to an appropriate amount of water, add a corrosion inhibitor; then add an anti-wear agent and a viscosity additive, mix well, and obtain a mixture B;
[0051] (3) Mixing mixture A and mixture B, stirring evenly, then adding a rust inhibitor and a dispersant; stirring until uniform, to obtain a drawing friction protection surface treatment composition.
[0052] Example 2
[0053] A method for preparing a surface treatment composition for pulling friction protection with good lubricity, wherein the composition comprises the following raw materials in terms of weight percentage:
[0054]
[0055] Sodium lauryl sulfate 6%;
[0056] The balance is water;
[0057] The remaining steps are consistent with Example 1.
[0058] Example 3
[0059] A method for preparing a surface treatment composition for pulling friction protection with good lubricity, wherein the composition comprises the following raw materials in terms of weight percentage:
[0060]
[0061] Lauryl polyoxyethylene ether 3%;
[0062] The balance is water;
[0063] The remaining steps are consistent with Example 1.
[0064] Example 4
[0065] A method for preparing a surface treatment composition for pulling friction protection with good lubricity, wherein the composition comprises the following raw materials in terms of weight percentage:
[0066]
[0067] The balance is water;
[0068] The remaining steps are consistent with Example 1.
[0069] The compositions of Examples 1 to 4 were subjected to corresponding performance tests according to the following test methods:
[0070] The test process is: pickling → water washing → surface treatment → drying → drawing; wherein, the surface treatment is to immerse the wire (such as 8A, 10A, 18A, etc., or alloy steel, such as SCM435) in the tank liquid for 1-5 minutes, take it out and dry it;
[0071] Drawing: The wire diameter of 6.0mm is drawn to 1.8mm through multiple dies;
[0072] Bath liquid: Take the composition and prepare a bath liquid with a mass concentration of 10-15%, heat it to 70-80°C, and the test data requires a sugar content of 5-6 and a solid content of 5-8%;
[0073] Sugar content is tested with a refractometer; dynamic viscosity is tested with a digital viscometer;
[0074] The detection method after wire processing is: corrosion resistance is salt spray test, temperature 35℃, 5% sodium chloride solution, using salt spray machine test.
[0075] The test results are shown in Table 1 below:
[0076] Table 1
[0077]
[0078] From Table 1, it can be found that the composition described in the present application has a maximum pull-out force of 100-130N after drawing when the composition is used in the cold plastic processing process, and the corrosiveness is titrated by the salt spray test, and the salt spray resistance time is more than 180min; while the maximum pull-out force of conventional phosphating soap and drawing powder is 135-150N, and the salt spray resistance time of normal phosphating soap and drawing powder is 60-120min.
[0079] The above embodiments are preferred implementation schemes of the present invention. In addition, the present invention may also be implemented in other ways. Any obvious replacement without departing from the concept of the present invention is within the protection scope of the present invention.
Claims
1. A surface treatment composition for pulling friction protection with good lubricity, It is characterized in that In units of weight percentage, it includes the following raw materials: Oleic acid glyceride is 15%, trimethylolpropane ester is 20%; diethyl phenyl phosphate is 6%, and aryl phosphate with CAS number 26967-76-0 is 2%; Molybdenum dialkyl dithiocarbamate with CAS number 71342-89-7 is 6%; Polyimide is 3%; Ether methacrylate with CAS number 951244-55-6 is 2.80%; triethanolamine, 6%; Magnesium sulfonate is 3%; Alkylphenol polyoxyethylene ether Tx-10 is 4%, sodium lauryl sulfate is 6%; The balance is water.
2. The method for preparing the drawing friction protection surface treatment composition according to claim 1, It is characterized in that The following steps are involved: (1) preparing materials according to the weight percentage of each raw material of the drawing friction protection surface treatment composition; taking oleic acid glyceryl ester and trimethylolpropane ester, adding alkylphenol polyoxyethylene ether Tx-10 and sodium lauryl sulfate, mixing at 70° C. for 20 minutes, slowly adding an appropriate amount of water, and stirring for 30 minutes to obtain a mixture A; (2) In another reactor, add diethylphenyl phosphate and aryl phosphate to an appropriate amount of water, add triethanolamine; then add molybdenum dialkyl dithiocarbamate and ether-containing methacrylate, mix well, and obtain mixture B; (3) Mixing mixture A and mixture B, stirring evenly, then adding magnesium sulfonate and polyimide; stirring until uniform, to obtain a drawing friction protection surface treatment composition.
3. An application of the drawing friction protection surface treatment composition according to claim 1 or the drawing friction protection surface treatment composition prepared by the preparation method according to claim 2, It is characterized in that The drawing friction protection surface treatment composition is applied to cold plastic processing.