A method for preparing a large-area two-dimensional alkali metal chalcogenide network
By depositing and annealing selenium powder on a copper substrate and then depositing potassium elementals in a heating state, a large area two-dimensional potassium selenium compound network is solved, and the cyclic performance problem caused by volume changes in the electrochemical energy storage system is solved. , realizes high-energy and low-cost two-dimensional material preparation, suitable for two-dimensional electronic information devices.
Patent Information
- Application Number
- CN202410050469.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-12
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-01-12
AI Technical Summary
The existing polyselenides have large volume changes in electrochemical energy storage systems, resulting in poor circulation performance. We seek a selenide that does not meet the stoichiometric ratio as a replacement material to improve energy storage performance.
By depositing selenium powder on a copper substrate and annealing, and then depositing potassium element in a heating state, a large area two-dimensional potassium selenium compound network structure is formed. The method includes depositing selenium powder on a copper single crystal substrate under an ultra-high vacuum environment, heating and annealing to form a selenium-carrying copper substrate, and then depositing potassium element at room temperature to form a two-dimensional potassium-selenium compound network.
A new single-layer two-dimensional material was obtained, suitable for two-dimensional electronic information devices, with excellent energy and low cost characteristics, and improved the performance of energy storage systems.
Smart Images

Figure CN117865076B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a large-area two-dimensional alkali metal sulfide compound network, and belongs to the technical field of nanomaterials. Background Art
[0002] In recent decades, due to the rapid consumption of fossil energy and the increasingly serious energy crisis, the demand for high energy / power density and low-cost secondary batteries has been increasing. Therefore, the development of alternative electrochemical energy storage systems has attracted more and more attention. In recent years, alkali metal chalcogenides have been widely studied as electrodes and electrolytes in the energy field, especially with the participation of potassium ions, which have the characteristics of high energy and low cost and are considered to be an attractive candidate material in the next generation of energy storage systems. However, since most polyselenides often have the characteristics of large volume changes, their cycle performance is still not ideal. Therefore, finding a class of unconventional, non-stoichiometric selenides may provide a new option.
[0003] For potassium selenium compounds, most of them belong to the element ratio in the phase diagram. If the surface physical chemistry method is used to prepare materials with element ratios that do not exist in the phase diagram, the subsequent experimental methods can be understood and designed based on the morphology, thus providing a meaningful strategy for its practical application. Summary of the invention
[0004] In view of the problems and shortcomings of the above-mentioned prior art, the present invention provides a method for preparing a large-area two-dimensional alkali metal sulfide compound network. The present invention utilizes the strategy that selenium powder will chemically react with a copper substrate to form a compound, and deposits selenium powder on the surface of the copper substrate to obtain a sample having copper selenium compounds and selenium atoms on the copper substrate, and then heats the sample to a growth temperature and anneals the sample, and then deposits potassium on the sample surface, and heats the sample to room temperature and anneals the sample, and finally obtains a sample of a network structure composed of a large-area two-dimensional potassium selenium compound. The present invention is implemented by the following technical solutions.
[0005] A method for preparing a large-area two-dimensional alkali metal chalcogenide network, the steps comprising:
[0006] Step 1: In an ultra-high vacuum environment, selenium powder is deposited onto a clean copper single crystal substrate surface at 25-30°C;
[0007] Step 2: After the deposition in step 1 is completed, the copper single crystal substrate and the selenium powder deposited on the surface of the copper single crystal substrate are heated to the growth temperature, annealed, and then cooled to room temperature to obtain an annealed selenium-loaded copper single crystal substrate;
[0008] Step 3: evaporate potassium and deposit it onto the annealed selenium-loaded copper single crystal substrate obtained in step 2, and then maintain it at room temperature to obtain a large-area two-dimensional potassium-selenium compound network.
[0009] The preparation process of the copper single crystal substrate in step 1 comprises the following steps:
[0010] Step 1.1, in an ultra-high vacuum chamber, subjecting a copper single crystal to argon ion sputtering to obtain a copper substrate;
[0011] Step 1.2: Heat the copper substrate obtained in step 1.1 to 450° C. and maintain the temperature for 10-30 minutes to obtain a copper single crystal substrate.
[0012] In the step 1, selenium powder is evaporated at an evaporation temperature of 120° C. to 125° C. and deposited on the surface of a clean copper single crystal substrate for 15 to 20 minutes.
[0013] In step 2, the growth temperature is 100-400° C., and the annealing treatment (i.e., maintaining the growth temperature) is performed for 10-30 minutes. By performing this step, the deposited selenium atoms can interact with the potassium element and fully diffuse to form a large-area two-dimensional potassium-selenium compound network structure.
[0014] In the step 3, the potassium element is evaporated at a temperature of 620° C. to 630° C. and is deposited on the annealed selenium-loaded copper single crystal substrate for 10 min to 15 min.
[0015] In the step 3, the mixture is kept at room temperature for 15 to 30 minutes.
[0016] The step of evaporating the selenium powder and potassium element is to evaporate the selenium powder and potassium element and deposit them on the copper single crystal substrate by thermal resistance heating and direct current heating.
[0017] The beneficial effects of the present invention are:
[0018] The network structure composed of large-area two-dimensional potassium-selenium compounds prepared by the present invention is a new type of single-layer two-dimensional material, which may be directly used in two-dimensional electronic information devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a scanning tunneling microscope image of a large-area two-dimensional potassium-selenium compound network prepared in Example 1 of the present invention;
[0020] Figure 2 The scanning tunneling microscope atomic resolution image, cellular structure and periodic diagram of the large-area two-dimensional potassium selenide compound network prepared in Example 1 of the present invention;
[0021] Figure 3It is a scanning tunneling microscope image of a large-area two-dimensional potassium-selenide compound network prepared in Example 1 of the present invention, a scanning tunneling microscope image of a large-area two-dimensional potassium-selenide compound network simulated by a computational method, and a corresponding optimized atomic configuration image of the potassium-selenide compound network. DETAILED DESCRIPTION
[0022] The present invention will be further described below in conjunction with the accompanying drawings and specific implementation methods.
[0023] Test instruments and equipment:
[0024] Low-temperature scanning tunneling microscope: purchased from Omicron, Germany.
[0025] K-cell molecular evaporation source: purchased from Omicron, Germany.
[0026] Argon ion gun: purchased from Omicron, Germany.
[0027] raw material:
[0028] Selenium powder: purchased from Sigma-Aldrich, purity 99.99%.
[0029] Copper single crystal: purchased from MaTecK, purity 99.999%.
[0030] Potassium element: purchased from SAES, purity 99.99%.
[0031] Example 1
[0032] The method for preparing the large-area two-dimensional alkali metal sulfide compound network comprises the following steps:
[0033] Step 1: In ultra-high vacuum environment (vacuum degree better than 1x10 -9 mbar), using a thermal resistance K-cell molecular evaporation source, the selenium powder was deposited at an evaporation temperature of 125°C for 15 min onto a clean copper single crystal substrate surface at 30°C;
[0034] The clean copper single crystal substrate preparation process comprises the following specific steps:
[0035] Step 1.1: In an ultra-high vacuum chamber (vacuum degree better than 1x10 -9 mbar), using an argon ion gun to perform argon ion sputtering on the copper single crystal to obtain a copper substrate;
[0036] Step 1.2, heating the copper substrate obtained in step 1.1 to 450° C. and maintaining the temperature for 10 min to obtain a copper single crystal substrate;
[0037] Step 2: After the deposition in step 1 is completed, the copper single crystal substrate and the selenium powder deposited on the surface of the copper single crystal substrate are heated to a growth temperature of 400° C., annealed for 30 minutes, and then cooled to room temperature to obtain an annealed selenium-loaded copper single crystal substrate;
[0038] Step 3: evaporate potassium at 630° C., deposit it on the annealed selenium-loaded copper single crystal substrate obtained in step 2 for 10 minutes, and then keep it at room temperature for 30 minutes to obtain a large-area two-dimensional potassium-selenium compound network.
[0039] The large-area two-dimensional potassium selenide compound network prepared by the present invention is observed by scanning tunneling microscopy. Figure 1 shown.
[0040] Figure 2 The atomic resolution image of the large-area two-dimensional potassium selenide compound network prepared by the present invention, as well as its cell size and period, is shown in the scanning tunneling microscope. Figure 2 It can be seen that the cell size of this large-area two-dimensional potassium-selenide compound network is 1.51nm.
[0041] Figure 3 The scanning tunneling microscope atomic resolution images of the large-area two-dimensional potassium selenide compound network structure prepared according to the preparation method of the embodiment of the present invention are experimentally and computationally simulated. It can be directly and effectively proved that the large-area two-dimensional potassium selenide compound network structure prepared by the preparation method of the embodiment of the present invention is composed of selenium atoms and potassium atoms.
[0042] Example 2
[0043] The method for preparing the large-area two-dimensional alkali metal sulfide compound network comprises the following steps:
[0044] Step 1: In ultra-high vacuum environment (vacuum degree is better than 1x10 -9 mbar), using a thermal resistance K-cell molecular evaporation source, the selenium powder was deposited on a clean copper single crystal substrate surface at 25°C at an evaporation temperature of 120°C for 20 min;
[0045] The clean copper single crystal substrate preparation process comprises the following specific steps:
[0046] Step 1.1: In an ultra-high vacuum chamber (vacuum degree better than 1x10 -9 mbar), using an argon ion gun to perform argon ion sputtering on the copper single crystal to obtain a copper substrate;
[0047] Step 1.2, heating the copper substrate obtained in step 1.1 to 450° C. and maintaining the temperature for 30 min to obtain a copper single crystal substrate;
[0048] Step 2: After the deposition in step 1 is completed, the copper single crystal substrate and the selenium powder deposited on the surface of the copper single crystal substrate are heated to a growth temperature of 100° C., annealed for 10 minutes, and then cooled to room temperature to obtain an annealed selenium-loaded copper single crystal substrate;
[0049] Step 3: evaporate potassium at 620° C., deposit it on the annealed selenium-loaded copper single crystal substrate obtained in step 2 for 15 minutes, and then keep it at room temperature for 30 minutes to obtain a large-area two-dimensional potassium-selenium compound network.
[0050] Example 3
[0051] The method for preparing the large-area two-dimensional alkali metal sulfide compound network comprises the following steps:
[0052] Step 1: In ultra-high vacuum environment (vacuum degree is better than 1x10 -9 mbar unit), using a thermal resistance K-cell molecular evaporation source, the selenium powder was deposited on a clean copper single crystal substrate surface at 28°C for 18 min at an evaporation temperature of 122°C;
[0053] The clean copper single crystal substrate preparation process comprises the following specific steps:
[0054] Step 1.1: In an ultra-high vacuum chamber (vacuum degree better than 1x10 -9 mbar), using an argon ion gun to perform argon ion sputtering on the copper single crystal to obtain a copper substrate;
[0055] Step 1.2, heating the copper substrate obtained in step 1.1 to 450° C. and maintaining the temperature for 20 min to obtain a copper single crystal substrate;
[0056] Step 2: After the deposition in step 1 is completed, the copper single crystal substrate and the selenium powder deposited on the surface of the copper single crystal substrate are heated to a growth temperature of 300° C., annealed for 20 minutes, and then cooled to room temperature to obtain an annealed selenium-loaded copper single crystal substrate;
[0057] Step 3: evaporate potassium at 625° C., deposit it on the annealed selenium-loaded copper single crystal substrate obtained in step 2 for 13 minutes, and then keep it at room temperature for 25 minutes to obtain a large-area two-dimensional potassium-selenium compound network.
[0058] The specific implementation modes of the present invention are described in detail above in conjunction with the accompanying drawings, but the present invention is not limited to the above implementation modes, and various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.
Claims
1. A method for preparing a large-area two-dimensional alkali metal sulfide network, characterized in that the steps include: Step 1: In an ultra-high vacuum environment, deposit selenium powder onto a clean copper single crystal substrate surface at 25-30°C; Step 2: After the deposition in step 1 is completed, the copper single crystal substrate and the selenium powder deposited on the surface of the copper single crystal substrate are heated to the growth temperature, annealed, and then cooled to room temperature to obtain an annealed selenium-loaded copper single crystal substrate; Step 3, evaporating potassium and depositing it onto the annealed selenium-loaded copper single crystal substrate obtained in step 2, and then maintaining it at room temperature to obtain a large-area two-dimensional potassium-selenium compound network; The preparation process of the copper single crystal substrate in step 1 comprises the following steps: Step 1.1, in an ultra-high vacuum chamber, subjecting a copper single crystal to argon ion sputtering to obtain a copper substrate; Step 1.2, heating the copper substrate obtained in step 1.1 to 450° C. and maintaining the temperature for 10-30 minutes to obtain a copper single crystal substrate; In the step 1, selenium powder is evaporated at an evaporation temperature of 120° C. to 125° C. and deposited on the surface of a clean copper single crystal substrate for 15 to 20 minutes; In step 2, the growth temperature is 100-400° C., and the annealing treatment is 10-30 minutes; In the step 3, the potassium element is evaporated at a temperature of 620° C. to 630° C. and is deposited on the annealed selenium-loaded copper single crystal substrate for 10 min to 15 min.
2. The method for preparing a large-area two-dimensional alkali metal chalcogenide network according to claim 1, characterized in that: In step 3, the mixture is kept at room temperature for 15 to 30 minutes.
Citation Information
Patent Citations
A group 6a / group 3a ink and methods of making and using same
CN102344714A
Method for simultaneously preparing, regulating and controlling three types of single-layer copper selenide superstructures