A method for preparing low-temperature lithium iron phosphate positive electrode material
Through niobium, molybdenum doping and secondary carbon coating technology, combined with the characteristics of tannic acid and PTCDA, the problem of transmission efficiency of lithium iron phosphate at low temperatures is solved, forming a uniform carbon coating layer, significantly improving its conductivity and performance , achieving efficient electrochemical performance at low temperatures.
Patent Information
- Application Number
- CN202311691668.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-11
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-12-11
AI Technical Summary
The electron and ion transmission efficiency of lithium iron phosphate is limited at low temperatures. Existing modification methods such as the one-step carbon coating method have problems with uneven carbon coating and loss of metal doping, making it difficult to meet low-temperature performance requirements.
Using niobium and molybdenum doping and secondary carbon coating methods, combined with the complexing properties of tannic acid and the polyphenyl ring structure of PTCDA, the lithium iron phosphate cathode material is prepared through sand grinding, spray drying, calcination and other steps to form a uniform and continuous lithium iron phosphate cathode material. Carbon coating layer widens lithium ion diffusion channels and improves conductivity.
It significantly improves the electronic and ionic conductivity of lithium iron phosphate, ensuring comprehensive electrochemical performance at low temperatures. The process is simple, green and environmentally friendly, and is suitable for industrial development.
Smart Images

Figure CN117865101B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of electrochemical energy storage, and in particular to a method for preparing a low-temperature lithium iron phosphate positive electrode material. Background Art
[0002] Lithium iron phosphate (LiFePO4) is widely used in portable electronic devices and new energy vehicles due to its high safety, long cycle life, green environmental protection and low preparation cost. However, the performance of lithium iron phosphate at low temperature is far from meeting daily needs, and the electron and ion transmission efficiency of lithium iron phosphate at low temperature is greatly limited. Among the common modification methods, carbon coating can improve the electronic conductivity of the material, and ion doping can improve the ion conductivity. The currently widely used one-step carbon coating method is to coat the carbon layer on the surface of lithium iron phosphate particles at one time to improve the electronic conductivity, but the one-step carbon coating method has the disadvantage of uneven and discontinuous carbon coating. Chinese invention patent CN103456924B discloses a method for preparing a secondary carbon-coated lithium iron phosphate composite with a polymer as a carbon source. The method uses glucose to coat the precursor first, then mixes it with the polymer and the compatibilizer at high speed, and then uses a plastic extruder to melt granulate, and finally calcines at high temperature to obtain secondary carbon-coated lithium iron phosphate. Chinese invention patent CN109860530 B discloses a titanium- and niobium-doped ammonium iron phosphate, lithium iron phosphate / carbon composite material, and its preparation method and application. The titanium and niobium co-doped lithium iron phosphate prepared by the invention has good low-temperature performance, but the carbon coating layer is not optimized. Chinese invention patent CN106554003 A discloses a synthesis method for improving the low-temperature performance of lithium iron phosphate. The method mixes the primary coated material with the carbon source for a second time, dries, and sinters to obtain a double-layer carbon-coated lithium iron phosphate. Although metal doping can improve ionic conductivity, there is an inconsistency between the doping amount of the final product and the feed amount. This is because some metal ions are in a free state during the slurry grinding and spraying process, which will cause unnecessary loss accompanied by the loss of solvent. Summary of the invention
[0003] The present invention aims to improve the electronic / ionic conductivity of lithium iron phosphate to improve the comprehensive electrochemical performance of the material at low temperature, and provides a method for preparing a low-temperature lithium iron phosphate positive electrode material. The lithium iron phosphate coating and doping modification strategy have a good effect on improving the low-temperature performance of lithium iron phosphate. The lithium iron phosphate is modified by niobium and molybdenum doping and secondary carbon coating, and the strong complexing property of tannic acid itself is used to reduce the loss of doped metal ions. The method has a simple process flow, the synthetic material is green and environmentally friendly, and it is easy to develop industrialization.
[0004] The method for solving the problem in the present invention is achieved by the following technical solution:
[0005] A low-temperature lithium iron phosphate positive electrode material and a preparation method thereof are prepared by the following steps:
[0006] Step (1): putting iron phosphate, lithium carbonate, tannic acid, niobium source and molybdenum source into a sand mill according to a certain molar ratio and using water as solvent for sand grinding;
[0007] Step (2): After sand grinding to a certain particle size, take out the slurry;
[0008] Step (3): spray drying the slurry of step (2) to obtain yellow material;
[0009] Step (4): placing the yellow material in step (3) into an inert atmosphere tube furnace for calcination to obtain carbon-coated lithium iron phosphate;
[0010] Step (5): placing the carbon-coated lithium iron phosphate and a certain amount of PTCDA in step (4) into an ethanol solution, stirring and dispersing them with ultrasonic stirring for a certain period of time, and then filtering to obtain a precursor;
[0011] Step (6): drying the precursor obtained in step (5) and placing it in an inert atmosphere tube furnace for calcination to obtain a lithium iron phosphate positive electrode material.
[0012] Specifically, the carbon source used in step (1) is tannic acid, and the molar ratio of added carbon to iron is (0.1-0.4):1;
[0013] Specifically, the molar ratio of niobium to iron added in step (1) is (0.01-0.06):1, and the molar ratio of molybdenum to iron added is (0.004-0.02):1.
[0014] Specifically, in step (4), the calcination temperature is 500-600°C, the holding time is 3-5 h, the heating rate is 2-5°C / min, and the protective gas is one of nitrogen or argon.
[0015] Specifically, the amount of PTCDA added in step (5) is 10-18% of the mass of the added lithium iron phosphate.
[0016] Specifically, in step (5), ultrasonication is performed for 20-40 mins and stirring is performed for 6-12 h.
[0017] Specifically, in step (6), the calcination temperature is 600-800°C, the heating rate is 2-5°C / min, the holding time is 5-9 h, and the protective gas is one of N2 and Ar.
[0018] Compared with other lithium iron phosphate modification methods, the beneficial effects of the present invention are:
[0019] 1. The co-doping of niobium and molybdenum causes the crystal structure of lithium iron phosphate to be distorted, which can broaden the original one-dimensional diffusion channel of lithium iron phosphate, facilitate the diffusion of lithium ions, improve the electronic conductivity of the material, and reduce resistance and polarization.
[0020] 2. Tannic acid has good film-forming properties in a neutral environment. Its molecules contain rich phenolic hydroxyl groups that can form a film on the surface of lithium iron phosphate particle precursors. The carbon coating layer formed by carbonization after calcination has good uniformity and continuity, which increases the contact area between particles and facilitates the transmission of electrons.
[0021] 3. Low-temperature carbonization can inhibit the growth of lithium iron phosphate primary particles while forming a carbon layer and refine the particles; high-temperature carbonization can increase the graphitization degree of the carbon layer and the conductivity of the material.
[0022] 4. PTCDA as a carbon source can further form a carbon layer on lithium iron phosphate. Due to the presence of multiple benzene ring structures in the carbon source, it can be converted into a uniform, ultra-thin, highly graphitized carbon coating layer during the calcination process without the need to add a catalyst, thereby improving the conductivity of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The scanning electron microscope of Example 1 at different magnifications Figure 1 ;
[0024] Figure 2 The scanning electron microscope of Example 1 at different magnifications Figure 2 ;
[0025] Figure 3 The scanning electron microscope of comparative example 1 at different magnifications Figure 1 ;
[0026] Figure 4 The scanning electron microscope of comparative example 1 at different magnifications Figure 2 . DETAILED DESCRIPTION
[0027] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments.
[0028] The present invention discloses a low-temperature lithium iron phosphate positive electrode material and a preparation method thereof. The invention ideas are further described below in conjunction with specific embodiments. These embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. It should be understood that based on the content of the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application.
[0029] Example 1
[0030] 150.82 g of anhydrous iron phosphate, 38.19 g of lithium carbonate, 4.66 g of tannic acid, 1.18 g of niobium pentoxide, 0.753 g of molybdenum trioxide and 335 g of deionized water were put into a sand mill for sand grinding. After sand grinding for 60 mins, the slurry was taken out for spray drying. After spray drying, the yellow material was obtained. The yellow material was placed in an inert atmosphere tube furnace, heated to 600 ° C for 330 mins, and kept warm for 200 mins. The protective gas was nitrogen. Lithium iron phosphate was sintered for standby use. 0.13 g of PTCDA was placed in 100 g of ethanol solution and then placed in 1 g of lithium iron phosphate for ultrasonic 20 mins. The ultrasonic power was 120W. After stirring for 6 h, the powder was filtered and dried and placed in an inert atmosphere tube furnace. The temperature was raised to 700 ° C for 200 mins, and the temperature was kept warm for 400 mins. After cooling to room temperature, the lithium iron phosphate positive electrode material was obtained.
[0031] Example 2
[0032] 150.82 g of anhydrous iron phosphate, 38.76 g of lithium carbonate, 1.03 g of tannic acid, 1.67 g of niobium pentoxide, 1.01 g of molybdenum trioxide and 340 g of deionized water were put into a sand mill for sand grinding. After sand grinding for 70 mins, the slurry was taken out for spray drying. After spray drying, the yellow material was obtained. The yellow material was placed in an inert atmosphere tube furnace, heated to 580 ° C for 300 mins, and kept warm for 220 mins. The protective gas was nitrogen. Lithium iron phosphate was sintered for standby use. 0.10 g of PTCDA was placed in 100 g of ethanol solution, and 1 g of lithium iron phosphate was placed in a tannic acid solution for ultrasonic 25 mins, with an ultrasonic power of 120 W and stirred for 7 h. After suction filtration and drying, the precursor was obtained. The precursor was placed in an inert atmosphere tube furnace, with nitrogen as the protective gas, heated to 650 ° C for 320 mins, kept warm for 500 mins, and then cooled to room temperature to obtain lithium iron phosphate positive electrode material.
[0033] Example 3
[0034] 150.82 g of anhydrous iron phosphate, 38.19 g of lithium carbonate, 2.18 g of tannic acid, 1.43 g of niobium pentoxide, 1.51 g of molybdenum trioxide and 350 g of deionized water were put into a sand mill for sand grinding. After sand grinding for 65 mins, the slurry was taken out for spray drying to obtain yellow material. The yellow material was placed in an inert atmosphere tube furnace, heated to 580 ° C for 330 mins, kept warm for 240 mins, and the protective gas was nitrogen. Lithium iron phosphate was sintered for standby use. 0.15 g of PTCDA was placed in 100 g of ethanol solution, and 1 g of lithium iron phosphate was placed in a tannic acid solution for ultrasonic 30 mins, with an ultrasonic power of 120 W. After stirring for 10 h, the precursor was filtered and dried to obtain the precursor. The precursor was placed in an inert atmosphere tube furnace, with nitrogen as the protective gas, heated to 680 ° C for 310 mins, kept warm for 480 mins, and then cooled to room temperature to obtain the lithium iron phosphate positive electrode material.
[0035] Comparative Example 1
[0036] 150.82 g of anhydrous iron phosphate, 38.19 g of lithium carbonate, 7.05 g of glucose, 1.18 g of niobium pentoxide, 0.753 g of molybdenum trioxide and 335 g of deionized water were put into a sand mill for sand grinding. After sand grinding for 60 mins, the slurry was taken out for spray drying. After spray drying, the yellow material was obtained. The yellow material was placed in an inert atmosphere tube furnace, heated to 600 ° C for 330 mins, and kept warm for 200 mins. The protective gas was nitrogen. Lithium iron phosphate was sintered for standby use. 6 g of monohydrated glucose was placed in 100 g of ethanol solution, and then 1 g of lithium iron phosphate solution was ultrasonicated for 20 mins, with an ultrasonic power of 100 W. After stirring for 6 h, the powder was filtered and dried, and placed in an inert atmosphere tube furnace, heated to 700 ° C for 200 mins, kept warm for 400 mins, and cooled to room temperature to obtain lithium iron phosphate positive electrode material.
[0037] Comparative Example 2
[0038] 150.82 g of anhydrous iron phosphate, 38.19 g of lithium carbonate, 7.05 g of fructose, 1.18 g of niobium pentoxide, 0.753 g of molybdenum trioxide and 335 g of deionized water were put into a sand mill for sand grinding. After sand grinding for 60 mins, the slurry was taken out for spray drying. After spray drying, the yellow material was obtained. The yellow material was placed in an inert atmosphere tube furnace, heated to 600 ° C for 330 mins, and kept warm for 200 mins. The protective gas was nitrogen. Lithium iron phosphate was sintered for standby use. 6 g of fructose was placed in 100 g of ethanol solution, and then 1 g of lithium iron phosphate solution was ultrasonicated for 20 mins. The ultrasonic power was 100 W. After stirring for 6 h, the powder was filtered and dried, and placed in an inert atmosphere tube furnace. The temperature was raised to 700 ° C for 200 mins, and the temperature was kept warm for 400 mins. After cooling to room temperature, the lithium iron phosphate positive electrode material was obtained.
[0039] Comparative Example 3
[0040] 150.82 g of anhydrous iron phosphate, 38.19 g of lithium carbonate, 3.55 g of sucrose, 1.18 g of niobium pentoxide, 0.753 g of molybdenum trioxide and 335 g of deionized water were put into a sand mill for sand grinding. After sand grinding for 60 mins, the slurry was taken out for spray drying. After spray drying, the yellow material was obtained. The yellow material was placed in an inert atmosphere tube furnace, heated to 600 ° C for 330 mins, and kept warm for 200 mins. The protective gas was nitrogen. Lithium iron phosphate was sintered for standby use. 3 g of sucrose was placed in 100 g of ethanol solution, and then 1 g of lithium iron phosphate solution was ultrasonicated for 20 mins. The ultrasonic power was 100 W. After stirring for 6 h, the powder was filtered and dried, and placed in an inert atmosphere tube furnace. The temperature was raised to 700 ° C for 200 mins, and the temperature was kept warm for 400 mins. After cooling to room temperature, the lithium iron phosphate positive electrode material was obtained.
[0041] Comparative Example 4
[0042] 150.82 g of anhydrous iron phosphate, 38.19 g of lithium carbonate, 4.66 g of tannic acid, 0.753 g of molybdenum trioxide and 335 g of deionized water were put into a sand mill for sand grinding. After sand grinding for 60 mins, the slurry was taken out for spray drying. After spray drying, the yellow material was obtained. The yellow material was placed in an inert atmosphere tube furnace, heated to 600 ° C for 330 mins, and kept warm for 200 mins. The protective gas was nitrogen. Lithium iron phosphate was sintered for standby use. 0.13 g of tannic acid was placed in 100 g of ethanol solution, and then 1 g of lithium iron phosphate solution was ultrasonicated for 20 mins. The ultrasonic power was 100 W. After stirring for 6 h, the powder was filtered and dried, and placed in an inert atmosphere tube furnace. The temperature was raised to 700 ° C for 200 mins, and the temperature was kept warm for 400 mins. After cooling to room temperature, the lithium iron phosphate positive electrode material was obtained.
[0043] Comparative Example 5
[0044] 150.82 g of anhydrous iron phosphate, 38.19 g of lithium carbonate, 4.66 g of tannic acid, 0.24 g of niobium pentoxide, 0.25 g of molybdenum trioxide and 335 g of deionized water were put into a sand mill for sand grinding. After sand grinding for 65 mins, the slurry was taken out for spray drying to obtain yellow material. The yellow material was placed in an inert atmosphere tube furnace, heated to 580 ° C for 330 mins, kept warm for 240 mins, and the protective gas was nitrogen. Lithium iron phosphate was sintered for standby use. 0.15 g of tannic acid was placed in 100 g of ethanol solution, and 1 g of lithium iron phosphate was placed in the tannic acid solution for ultrasonic 30 mins, with an ultrasonic power of 100 W. After stirring for 10 h, the precursor was filtered and dried to obtain the precursor. The precursor was placed in an inert atmosphere tube furnace, with nitrogen as the protective gas, heated to 680 ° C for 310 mins, kept warm for 480 mins, and then cooled to room temperature to obtain the lithium iron phosphate positive electrode material.
[0045] Comparative Example 6
[0046] 150.82 g of anhydrous iron phosphate, 38.19 g of lithium carbonate, 4.66 g of tannic acid, 3.36 g of niobium pentoxide, 0.23 g of molybdenum trioxide and 335 g of deionized water were put into a sand mill for sand grinding. After sand grinding for 60 mins, the slurry was taken out for spray drying. After spray drying, the yellow material was obtained. The yellow material was placed in an inert atmosphere tube furnace, heated to 600 ° C for 330 mins, and kept warm for 200 mins. The protective gas was nitrogen. Lithium iron phosphate was sintered for standby use. 0.13 g of tannic acid was placed in 100 g of ethanol solution, and then 1 g of lithium iron phosphate solution was ultrasonicated for 20 mins. The ultrasonic power was 100 W. After stirring for 6 h, the powder was filtered and dried and placed in an inert atmosphere tube furnace. The temperature was raised to 700 ° C for 200 mins, and the temperature was kept warm for 400 mins. After cooling to room temperature, the lithium iron phosphate positive electrode material was obtained.
[0047] Comparative Example 7
[0048] 150.82 g of anhydrous iron phosphate, 38.19 g of lithium carbonate, 4.66 g of tannic acid, 1.18 g of niobium pentoxide, 0.753 g of molybdenum trioxide and 335 g of deionized water were put into a sand mill for sand grinding. After sand grinding for 60 mins, the slurry was taken out for spray drying. After spray drying, the yellow material was obtained. The yellow material was placed in an inert atmosphere tube furnace, heated to 600 ° C for 330 mins, and kept warm for 200 mins. The protective gas was nitrogen. Lithium iron phosphate was sintered for standby use. 0.13 g of glucose was placed in 100 g of ethanol solution and then placed in 1 g of lithium iron phosphate for ultrasonic 20 mins. The ultrasonic power was 120 W. After stirring for 6 h, the powder was filtered and dried and placed in an inert atmosphere tube furnace. The temperature was raised to 700 ° C for 200 mins, and the temperature was kept warm for 400 mins. After cooling to room temperature, the lithium iron phosphate positive electrode material was obtained.
[0049] Comparative Example 8
[0050] 150.82 g of anhydrous iron phosphate, 38.19 g of lithium carbonate, 4.66 g of tannic acid, 1.18 g of niobium pentoxide, 0.753 g of molybdenum trioxide and 335 g of deionized water were put into a sand mill for sand grinding. After sand grinding for 60 mins, the slurry was taken out for spray drying. After spray drying, the yellow material was obtained. The yellow material was placed in an inert atmosphere tube furnace, heated to 600 ° C for 330 mins, and kept warm for 200 mins. The protective gas was nitrogen. Lithium iron phosphate was sintered for standby use. 0.13 g of fructose was placed in 100 g of ethanol solution and then placed in 1 g of lithium iron phosphate for ultrasonic 20 mins. The ultrasonic power was 120 W. After stirring for 6 h, the powder was filtered and dried and placed in an inert atmosphere tube furnace. The temperature was raised to 700 ° C for 200 mins, and the temperature was kept warm for 400 mins. After cooling to room temperature, the lithium iron phosphate positive electrode material was obtained.
[0051] Comparative Example 9
[0052] 150.82 g of anhydrous iron phosphate, 38.19 g of lithium carbonate, 4.66 g of tannic acid, 1.18 g of niobium pentoxide, 0.753 g of molybdenum trioxide and 335 g of deionized water were put into a sand mill for sand grinding. After sand grinding for 60 mins, the slurry was taken out for spray drying. After spray drying, the yellow material was obtained. The yellow material was placed in an inert atmosphere tube furnace, heated to 600 ° C for 330 mins, and kept warm for 200 mins. The protective gas was nitrogen. Lithium iron phosphate was sintered for standby use. 0.13 g of sucrose was placed in 100 g of ethanol solution and then placed in 1 g of lithium iron phosphate for ultrasonic 20 mins. The ultrasonic power was 120 W. After stirring for 6 h, the powder was filtered and dried and placed in an inert atmosphere tube furnace. The temperature was raised to 700 ° C for 200 mins, and the temperature was kept warm for 400 mins. After cooling to room temperature, the lithium iron phosphate positive electrode material was obtained.
[0053] Table 1 Changes in the amount of doped metal and the second addition of carbon source in the examples and comparative examples
[0054]
[0055] Low temperature discharge test
[0056] The materials of each embodiment and comparative example were mixed with a conductive agent (Super P) and a PVDF solution dissolved in NMP in a ratio of 90:5:5, respectively, and then coated on a carbon-coated aluminum foil. After vacuum drying at 110°C, they were pressed into a disc with a diameter of 12 mm as the positive electrode, a metal lithium sheet as the negative electrode, a Celgard 2300 microporous membrane as the separator, and a solution of 1.0 mol / L LiPF6 in ethylene carbonate (EC): dimethyl carbonate (DMC) = 1:1 as the electrolyte. The cells were assembled into R2025 button cells in a glove box, and after standing at room temperature of 25°C for 8 h, a low-temperature test was performed using a Xinwei 3008 battery testing system: first, the charging capacity was recorded after charging to 3.75 V at 0.1 C, the battery was placed in a -10°C constant temperature box for 1 h, and then taken out for a discharge test at 0.1 C, and the discharge specific capacity was recorded. The normal temperature discharge efficiency is the discharge capacity at normal temperature / the normal temperature charge capacity, and the low temperature discharge efficiency is the discharge capacity after low temperature standing / the normal temperature charge capacity.
[0057] Table 2 Performance comparison of the examples and comparative examples
[0058]
[0059] 1. Table 1 shows the changes in the amount of doped metal and the secondary addition of carbon source in the examples and comparative examples. Table 2 shows the performance comparison of the examples and comparative examples. By comparison, it can be seen that the low-temperature performance of the lithium iron phosphate composite material doped with niobium and molybdenum combined with carbon coating in the examples is higher than that in the comparative examples.
[0060] 2. Low-temperature lithium iron phosphate requires higher electronic and ionic conductivity. Although increasing the carbon content can improve the electronic conductivity, the higher the carbon content, the higher the requirement for the carbon layer. The carbon layer formed by the traditional common carbon source is not uniform enough and has poor continuity, and cannot play the role of a conductive medium. Tannic acid has good self-filming properties. It can be evenly coated on the surface of lithium iron phosphate in aqueous solution. After calcination, it forms a uniform and continuous carbon layer, which greatly increases the effective contact area between lithium iron phosphate, improves the efficiency of electron transmission, and ensures a higher conductivity at low temperature. In addition, tannic acid can form a film independently in a neutral environment and has good universality; the polybenzene ring structure of PTCDA can be converted into a uniform ultra-thin high-graphitization carbon coating layer without the addition of a catalyst during the heat treatment process. At the same time, the appropriate amount of niobium and molybdenum doping can cause lattice distortion, broaden the lithium ion deintercalation channel, and accelerate the transmission of lithium ions. The advantage of this method over other double-layer carbon coating technologies lies in simpler process costs and excellent carbon coating effects.
[0061] The above embodiments only express the preferred implementation modes of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims.
Claims
1. A method for preparing a low-temperature lithium iron phosphate positive electrode material, It is characterized in that Prepared by the following steps: Step (1): mixing iron phosphate, lithium carbonate, tannic acid, niobium source, and molybdenum source with deionized water in a certain molar ratio and then putting the mixture into a sand mill for sand grinding, wherein the carbon source is tannic acid, the molar ratio of the added carbon to the iron is (0.1-0.4):1, the molar ratio of the added niobium to the iron is (0.01-0.06):1, and the molar ratio of the added molybdenum to the iron is (0.004-0.02):1; Step (2): After sand grinding to a certain particle size, take out the slurry; Step (3): spray drying the slurry of step (2) to obtain yellow material; Step (4): placing the yellow material in step (3) into an inert atmosphere tube furnace for calcination to obtain carbon-coated lithium iron phosphate; Step (5): Place the lithium iron phosphate and PTCDA in step (4) in an ethanol solution, stir and disperse them with ultrasonic waves for a certain period of time, and then filter and dry to obtain a precursor. The amount of PTCDA added is 10-18% of the mass of the lithium iron phosphate. Ultrasonic waves are applied for 20-40 mins at a power of 100 W-300 W and stirred for 6-12 h. Step (6): drying the precursor obtained in step (5) and placing it in an inert atmosphere tube furnace for calcination to obtain a lithium iron phosphate positive electrode material.
2. The method for preparing a low-temperature lithium iron phosphate positive electrode material according to claim 1, It is characterized in that In step (4), the calcination conditions are 500-600 °C, the heating rate is 2-5 °C / min, the holding time is 3-5 h, and the protective gas is N 2 ,Ar one of them.
3. The method for preparing a low-temperature lithium iron phosphate positive electrode material according to claim 1, It is characterized in that In step (7), the calcination temperature is 600-800 °C, the heating rate is 2-5 °C / min, the holding time is 5-9 h, and the protective gas is N 2 ,Ar one of them.
Citation Information
Patent Citations
Preparation method of secondary carbon-coated lithium iron phosphate composite using polymer as carbon source
CN103456924B
Synthetic method capable of increasing low-temperature performance of lithium iron phosphate
CN106554003A
A titanium- and niobium-doped basic ammonium iron phosphate, lithium iron phosphate / carbon composite material, its preparation method and application
CN109860530B
A preparation method of a double-layer carbon-coated lithium iron phosphate material
CN109037659A
Preparation method of three-layer carbon-coated composite lithium iron phosphate cathode material
CN109920989A