A rare earth-containing microalloyed steel, its preparation method and application
By adding rare earth elements and optimizing the Cr and Sb content in 16Mn steel, a rare earth-containing microalloyed steel is formed, which solves the problem of insufficient corrosion resistance in high chlorine and high sulfur environments and enables its efficient application in petrochemical equipment.
Patent Information
- Application Number
- CN202211230094.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-08
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-10-08
AI Technical Summary
Existing ordinary carbon steel and carbon manganese steel have insufficient corrosion resistance in the high-chlorine and high-sulfur petroleum refining environment, and existing rare earth corrosion-resistant steels have insufficient performance or are too expensive in this environment, which cannot meet the service requirements of petrochemical equipment.
By adding appropriate amounts of rare earth elements La, Ce, and Y to 16Mn steel, optimizing the content of Cr and Sb, controlling the proportions of other components such as C, Si, Mn, P, and Cu, and employing a scientific and reasonable smelting process, rare earth microalloyed steel is formed, ensuring its corrosion resistance and mechanical properties in high-chlorine and high-sulfur environments.
It significantly improves the steel's resistance to chlorine and hydrogen sulfide corrosion, reduces the corrosion rate, maintains mechanical properties comparable to ordinary 16Mn steel, and has a lower cost, making it suitable for petrochemical equipment.
Abstract
Description
Technical Field
[0001] This invention relates to the field of metal smelting technology, specifically to a rare earth-containing microalloyed steel, its preparation method, and its application. Background Technology
[0002] Ordinary carbon steels such as Q245R, Q345R, and 20 steel, and carbon manganese steels such as 16Mn, are widely used in petrochemical equipment such as pipelines, pressure vessels, and storage tanks due to their low cost. However, because petrochemical equipment often faces highly corrosive environments with high sulfur, high chlorine, and high humidity, the aforementioned ordinary carbon and carbon manganese steels are far from meeting the corrosion resistance requirements of petrochemical equipment. Studies have shown that the domestic refining industry experiences over 1,000 leaks annually due to corrosion, resulting in over 50 unplanned shutdowns and economic losses amounting to tens of billions of yuan. To address this severe corrosion problem, the petrochemical industry has begun to replace ordinary carbon and carbon manganese steels with alloy steels containing high levels of alloying elements such as Cr, Ni, and Mo. However, this undoubtedly significantly increases the manufacturing costs of petrochemical equipment.
[0003] my country is a major rare earth resource country, with a severe oversupply of light rare earth elements, particularly lanthanum (La) and cerium (Ce). Adding light rare earth elements such as lanthanum and cerium to ordinary carbon steel and carbon-manganese steel can improve their corrosion resistance. Due to the low cost of rare earth elements and their ability to enhance the corrosion resistance of steel, corrosion-resistant steels containing rare earth elements are attracting increasing attention.
[0004] Patent application CN113737105A discloses a rare earth-containing weathering steel and its preparation method. This steel mainly adds a certain amount of rare earth to the base of weathering steel designed for atmospheric corrosion to improve the atmospheric corrosion resistance of traditional weathering steel. However, this rare earth-containing steel is still a weathering steel, and its corrosion resistance is only suitable for atmospheric environments with low corrosivity, and cannot cover the high-chlorine and high-sulfur petroleum refining environment.
[0005] Patent application CN110983156A discloses a rare earth corrosion-resistant steel rich in alloyed rare earth elements and its manufacturing method. The rare earth corrosion-resistant steel is formed by adding a small amount of rare earth to ordinary carbon steel Q235 and ordinary carbon manganese steel Q355 for rare earth alloying. However, this rare earth corrosion-resistant steel only achieves the atmospheric corrosion resistance of ordinary carbon steel Q235 or ordinary carbon manganese steel Q355 through rare earth alloying. The low Cr, Ni and Cu content makes it unable to meet the service requirements in the high chlorine and high sulfur petroleum refining environment.
[0006] Patent application CN114214558A discloses a low-alloy steel with super-strong resistance to sulfuric acid and hydrochloric acid corrosion and its preparation method. The method strictly limits the composition ratio of Si, Cr, Mo, Sb and Sn in the steel, which makes it difficult to control the actual content of these elements in the actual smelting process to meet the target requirements. The addition of many alloying elements (Cu, Mn, Cr, Ni, Mo, etc.) can easily lead to an increase in the brittleness of the steel and a decrease in its weldability, making it unable to meet the requirements for stress corrosion resistance and hydrogen embrittlement resistance when serving in a hydrogen sulfide-containing environment. Summary of the Invention
[0007] To address the shortcomings of existing technologies, this invention provides a rare earth-containing microalloyed steel, its preparation method, and its applications. This rare earth-containing microalloyed steel exhibits excellent resistance to corrosion in chlorine and hydrogen sulfide environments, meeting the corrosion resistance requirements of petrochemical equipment. Furthermore, it has a lower cost, and its yield strength and elongation are not lower than those of ordinary 16Mn steel.
[0008] To achieve the above objectives, the present invention provides a rare earth-containing microalloyed steel, wherein, based on the total mass of the rare earth-containing microalloyed steel, the mass fraction of its chemical composition is as follows: C: 0.065–0.20%, Si: 0.20–0.55%, Mn: 1.2–1.6%, P: ≤0.015%, S: ≤0.01%, Cr: 0.80–2.0%, Cu: ≤0.25%, Sb: 0.08–0.12%, rare earth elements: 0.01–0.05%, with the balance being Fe and unavoidable impurities.
[0009] Preferably, based on the total mass of the rare earth-containing microalloyed steel, the mass fraction of its chemical composition is as follows: C: 0.065–0.16%, Si: 0.25–0.50%, Mn: 1.2–1.5%, P: 0.007–0.013%, S: 0.001–0.01%, Cr: 1.20–2.0%, Cu: 0.01–0.18%, Sb: 0.09–0.12%, rare earth elements: 0.02–0.05%, with the balance being Fe and unavoidable impurities.
[0010] Preferably, the rare earth element is selected from one or more of La, Ce and Y.
[0011] Preferably, the corrosion rate of the rare earth-containing microalloyed steel in the atmospheric and vacuum distillation unit and the coking unit top circulation process environment is less than 0.8 mm / a, wherein the process environment is saturated with chloride ions, the humidity is 100%, and the hydrogen sulfide content is not less than 100 ppm.
[0012] A second aspect of this invention provides a method for preparing rare-earth-containing microalloyed steel, the method comprising the following steps:
[0013] S10. Add rare earth wire to the molten steel. After the rare earth wire melts, mix it evenly and continuously cast the resulting mixture to obtain a continuously cast billet.
[0014] S20. Roll the continuously cast billet to obtain rare earth microalloyed steel;
[0015] In step S10, the continuously cast billet comprises the following components by mass fraction: C: 0.065–0.20%, Si: 0.20–0.55%, Mn: 1.2–1.6%, P: ≤0.015%, S: ≤0.01%, Cr: 0.80–2.0%, Cu: ≤0.25%, Sb: 0.08–0.12%, and rare earth elements: 0.01–0.05%.
[0016] Preferably, in step S10, the preparation process of the molten steel includes:
[0017] A1. Desulfurize and remove slag from molten iron. When the temperature of the molten iron is ≥1300℃ and the S content in the molten iron is ≤0.007wt%, desulfurized molten iron is obtained.
[0018] A2. The desulfurized molten iron is introduced into the top and bottom of the converter for oxygen re-blowing. When the C content in the desulfurized molten iron is ≤0.05wt% and the P content is ≤0.01wt%, the blowing process ends.
[0019] A3. After tapping the steel and removing the slag, add SbFe alloy blocks and low-carbon CrFe alloy blocks to the obtained molten steel, then pour it into a ladle. Stir the ladle with argon, then transfer it to LF refining, add alloys, add slag, raise the temperature, and continuously adjust the composition to make the molten steel composition meet the target requirements.
[0020] Preferably, in step A3, slag is blocked during tapping, and a deoxidizing alloy is added during the tapping process.
[0021] Preferably, in step S10, the rare earth element in the continuously cast billet is selected from one or more of La, Ce and Y.
[0022] Preferably, in step S20, the rolling process includes: cutting the continuously cast billet to a fixed length, feeding it into a heating furnace and heating it to 1200-1250°C, removing phosphorus with high-pressure water when it exits the heating furnace, and then feeding it into a rolling mill for rolling and coiling.
[0023] Preferably, the final rolling temperature is 840–910°C.
[0024] Preferably, the winding temperature is 600–720°C.
[0025] Preferably, the rolling step further includes: cold rolling and annealing the steel obtained after coiling.
[0026] A third aspect of the present invention provides an application of the rare earth-containing microalloyed steel as described above, wherein the rare earth-containing microalloyed steel is used to manufacture petrochemical equipment.
[0027] The advantages and beneficial effects of this invention are:
[0028] (1) This invention uses rare earth alloying on 16Mn steel and scientifically and rationally optimizes the composition of 16Mn steel, limiting the Cr content and Sb content, thereby greatly improving its resistance to chlorine and hydrogen sulfide corrosion. The resulting rare earth microalloyed steel has excellent corrosion resistance in high chlorine and high hydrogen sulfide environments, and its corrosion rate is reduced by more than 50% compared with ordinary 16Mn steel.
[0029] (2) In the composition design of the present invention, Cr and Sb are added to 16Mn steel without changing the microstructure (ferrite) of 16Mn steel. Therefore, the yield strength and elongation of the rare earth microalloyed steel are not lower than those of ordinary 16Mn steel, which overcomes the problem that the existing ordinary carbon steel or carbon manganese steel will have its mechanical properties reduced while improving its corrosion resistance.
[0030] (3) The rare earth microalloyed steel provided by the present invention has a small amount of alloying elements added and a low cost. Its cost is no more than 1.3 times that of 16Mn steel, and it can widely replace ordinary carbon steel and carbon manganese steel in the application of petrochemical wet hydrogen sulfide environment. Detailed Implementation
[0031] The following provides a detailed description of specific embodiments of the present invention. It should be understood that the specific embodiments described herein are for illustrative and explanatory purposes only and are not intended to limit the scope of the invention.
[0032] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0033] This invention provides a rare earth-containing microalloyed steel, which, based on the total mass of the rare earth-containing microalloyed steel, contains the following chemical composition by mass fraction: C: 0.065–0.20%, Si: 0.20–0.55%, Mn: 1.2–1.6%, P: ≤0.015%, S: ≤0.01%, Cr: 0.80–2.0%, Cu: ≤0.25%, Sb: 0.08–0.12%, rare earth elements: 0.01–0.05%, with the balance being Fe and unavoidable impurities.
[0034] In this invention, the rare earth element is selected from one or more of La, Ce, and Y. La and Ce are readily available and inexpensive; therefore, the rare earth element is preferably La and / or Ce, and more preferably La and Ce.
[0035] The mechanisms of action of the above elements are as follows:
[0036] Rare Earth Elements (REM): The rare earth elements used in this invention are one or more of cerium (Ce), lanthanum (La), and yttrium (Y). By adding rare earth elements such as cerium (Ce), lanthanum (La), or yttrium (Y), the size of inclusions can be reduced, inclusions can be spheroidized, the distribution of inclusions can be improved, grain size can be refined, the interlamellar spacing of pearlite can be reduced, and the uniformity and toughness of the steel structure can be improved. In addition, rare earth elements such as cerium (Ce), lanthanum (La), and yttrium (Y) can reduce the sensitivity to pitting corrosion induced by inclusions, reduce the segregation of P at grain boundaries, and improve the corrosion resistance of grain boundaries. At the same time, rare earth elements can increase the proportion of α-FeOOH and amorphous phases in the rust layer, thereby increasing the density and uniformity of the rust layer, and thus improving the overall corrosion resistance of the steel. However, excessive rare earth element content can also have adverse effects on the steel. Therefore, in this invention, the content of rare earth elements is controlled between 0.01 and 0.05 wt%.
[0037] Carbon (C) is the most effective and economical strengthening element in steel, primarily improving its strength through solid solution strengthening and precipitation strengthening. However, C reduces the plasticity and toughness of steel. High C content easily leads to C combining with Cr and precipitating at grain boundaries, resulting in Cr depletion at grain boundaries and reducing the steel's resistance to intergranular corrosion and intergranular cracking. Therefore, in this invention, the C content is controlled between 0.065 and 0.2 wt%.
[0038] Silicon (Si): Generally added during smelting as a reducing agent and deoxidizer. Solid-solution Si can strengthen the steel, improve its hardenability and tempering resistance, and, when combined with Cr, effectively improve its weather resistance. However, excessive Si content can lead to decreased weldability and difficulty in removing surface oxide scale. Therefore, in this invention, the Si content is controlled between 0.20 and 0.55 wt%.
[0039] Manganese (Mn): As a desulfurization and deoxidation element, Mn can reduce the hot and cold brittleness caused by sulfur. Simultaneously, Mn has a solid solution strengthening effect, which can improve the tensile strength of materials and lower the austenite transformation initiation temperature Ar3, thus moderately improving hardenability. In this invention, the Mn content is controlled between 1.2 and 1.6 wt%.
[0040] Phosphorus (P): P is prone to segregation, which reduces the cold brittleness, toughness, and weldability of steel. Therefore, in this invention, the P content is controlled below 0.015 wt%.
[0041] Sulfur (S): It readily combines with Mn to form MnS inclusions, which deteriorate the mechanical properties of steel. Furthermore, large inclusions easily create a potential difference with the matrix, preferentially leading to pitting corrosion and further reducing the steel's corrosion resistance. Therefore, in this invention, the S content is controlled below 0.01 wt%.
[0042] Chromium (Cr): It can form a dense oxide film on the surface of steel plates, improving the passivation ability of the steel plates. It easily accumulates in rust layers, increasing the selective permeability of the rust layer to anions and improving the steel's resistance to chloride corrosion. For cost reasons and in this invention, the Cr content is controlled between 0.80 and 2.0 wt%.
[0043] Copper (Cu): It can form a Cu-based barrier layer between the substrate and the rust layer, which is firmly bonded to the substrate and provides good protection for the steel plate. At the same time, Cu can combine with S and Sb to form Cu2S and Cu2Sb layers, preventing further corrosion and improving corrosion resistance. In this invention, the Cu content is controlled below 0.25 wt%.
[0044] Antimony (Sb): A highly effective alloying element for improving the acid corrosion resistance of steel. Sb reacts with Cl to form a catalytic effect, promoting the formation of a composite compound on the steel surface, thereby enhancing the corrosion resistance of the substrate. Simultaneously, Sb effectively inhibits hydrogen penetration, reduces the poisoning effect of sulfur, and improves the steel's resistance to hydrogen sulfide stress corrosion. In this invention, the Sb content is controlled between 0.08 and 0.12 wt%.
[0045] In a preferred embodiment, based on the total mass of the rare earth-containing microalloyed steel, the mass fraction of its chemical composition is as follows: C: 0.065–0.16%, Si: 0.25–0.50%, Mn: 1.2–1.5%, P: 0.007–0.013%, S: 0.001–0.01%, Cr: 1.20–2.0%, Cu: 0.01–0.18%, Sb: 0.09–0.12%, rare earth elements: 0.02–0.05%, with the balance being Fe and unavoidable impurities.
[0046] The rare earth-containing microalloyed steel of the present invention has a corrosion rate of less than 0.8 mm / a in the atmospheric and vacuum distillation unit tower top circulation process environment (chloride ion saturation, humidity 100%, hydrogen sulfide content not less than 100 ppm). That is, the corrosion depth of the rare earth-containing microalloyed steel under this environment is less than 0.8 mm per year, and it has excellent corrosion resistance, which can meet the service requirements in the high chlorine and high sulfur petroleum refining environment.
[0047] This invention also proposes a method for preparing rare-earth-containing microalloyed steel as described above, the method comprising the following steps:
[0048] Step S10: Add rare earth wire to the molten steel. After the rare earth wire melts and is mixed evenly, the resulting mixture is continuously cast to obtain a continuously cast billet.
[0049] Step S20: Roll the continuously cast billet to obtain rare earth microalloyed steel.
[0050] In step S10, the continuously cast billet comprises the following components by mass fraction: C: 0.065–0.20%, Si: 0.20–0.55%, Mn: 1.2–1.6%, P: ≤0.015%, S: ≤0.01%, Cr: 0.80–2.0%, Cu: ≤0.25%, Sb: 0.08–0.12%, and rare earth elements: 0.01–0.05%.
[0051] In this invention, in step S10, the rare earth element in the continuously cast billet is selected from one or more of La, Ce and Y.
[0052] In a preferred embodiment, step S10, the preparation process of the molten steel includes:
[0053] Step A1: Hot metal pretreatment
[0054] Desulfurize and remove slag from molten iron. When the temperature of the molten iron is ≥1300℃ and the sulfur content in the molten iron is ≤0.007wt%, desulfurized molten iron is obtained.
[0055] Step A2, Converter blowing
[0056] After the desulfurized molten iron and scrap steel are mixed, oxygen is blown back into the top and bottom of the converter to remove phosphorus and carbon. The blowing process ends when the carbon content in the desulfurized molten iron is ≤0.05wt% and the phosphorus content is ≤0.01wt%.
[0057] Step A3, Ladle Refining
[0058] After tapping the steel and removing the slag, SbFe alloy blocks and low-carbon CrFe alloy blocks are added to the resulting molten steel, which is then poured into a ladle. The ladle is then stirred with argon, and the process is transferred to LF refining, where alloys are added, slag is added, and the temperature is increased. The composition is continuously adjusted to achieve the target requirements for the molten steel composition.
[0059] In a preferred embodiment, in step A1, desulfurization is carried out by blowing lime powder into the molten iron ladle.
[0060] In a preferred embodiment, a deoxidizing alloy is added during the tapping process to deoxidize the molten steel. The deoxidizing alloy is selected from SiFe particles, MnFe particles, and Al alloy particles.
[0061] In a preferred embodiment, step S20 includes: cutting the continuously cast billet to a fixed length, sending it into a heating furnace and heating it to 1200-1250°C, removing phosphorus with high-pressure water when it exits the heating furnace, and then sending it into a rolling mill for rolling and coiling.
[0062] More preferably, the final rolling temperature is 840–910°C, and more preferably 850–890°C.
[0063] More preferably, the winding temperature is 600–720°C, more preferably 660–680°C.
[0064] Of course, the design of the present invention is not limited to this. In one specific embodiment, the rolling step further includes: cold rolling and annealing the steel obtained after coiling. Through the above steps, the mechanical properties of the steel can be further improved.
[0065] Furthermore, this invention also proposes an application of the rare-earth-containing microalloyed steel described above, which is used to manufacture petrochemical equipment. The rare-earth-containing microalloyed steel exhibits excellent corrosion resistance in high-chlorine and high-hydrogen sulfide environments, good mechanical properties, and low cost, showing significant advantages compared to existing ordinary carbon steel and carbon-manganese steel.
[0066] The present invention will be described in detail below through embodiments, but the scope of protection of the present invention is not limited thereto. In the following examples, the selected low-carbon CrFe block has a Cr content (weight percentage) of 54.2% and the selected SbFe block has an Sb content (weight percentage) of 99.4%.
[0067] Example 1
[0068] This embodiment is used to illustrate the rare earth-containing microalloyed steel and its preparation method according to the present invention.
[0069] (1) Lime powder is injected into the ladle for desulfurization, and then slag is removed. When the temperature of the molten iron is ≥1300℃ and the S content in the molten iron is ≤0.007wt%, desulfurized molten iron is obtained. The desulfurized molten iron enters the converter for steelmaking. Lime is added to the top of the converter for oxygen blowing to remove P and C. When the C content in the desulfurized molten iron is ≤0.05wt% and the P content is ≤0.01wt%, the blowing ends. The slag is blocked when the steel is tapped from the converter, and deoxidizing alloy (Al particles) is added during the tapping process. Low carbon CrFe alloy blocks (addition amount 36.9kg / ton) and SbFe alloy blocks (addition amount 1.51kg / ton) are added to the obtained molten steel. Then it is put into the ladle. The ladle is blown with argon to stir and promote the floating of inclusions. Then it is transferred to LF for refining. Alloy is added, slag is added, the temperature is raised, and the composition is continuously adjusted to obtain molten steel with the target composition.
[0070] (2) After the molten steel obtained in step (1) enters the tundish, LaCe rare earth wire (addition amount is 0.52kg / ton) is added. After the rare earth wire melts and is mixed evenly, the resulting mixture is continuously cast to obtain a continuously cast billet.
[0071] (3) Cut the continuous casting billet obtained in step (2) into 150mm thick slabs and send them into a heating furnace to be heated to 1240℃. When exiting the heating furnace, use high-pressure water to remove phosphorus and then send them into the rolling mill for rough rolling and finish rolling. The rough rolling end temperature is 990℃, the finish rolling temperature is 890℃, and the coiling temperature is 680℃ to obtain rare earth microalloyed steel with a thickness of 8mm.
[0072] The rare earth microalloyed steel contains the following chemical composition by mass fraction: C: 0.112%, Si: 0.31%, Mn: 1.390%, P: 0.008%, S: 0.004%, Cr: 1.836%, Cu: 0.01%, Sb: 0.107%, La: 0.0195%, Ce: 0.014%, with the balance being Fe and unavoidable impurities.
[0073] Example 2
[0074] This embodiment is used to illustrate the rare earth-containing microalloyed steel and its preparation method according to the present invention.
[0075] (1) Lime powder is injected into the ladle for desulfurization, and then slag is removed. When the temperature of the molten iron is ≥1300℃ and the S content in the molten iron is ≤0.007wt%, desulfurized molten iron is obtained. The desulfurized molten iron enters the converter for steelmaking. Lime is added to the top of the converter for oxygen blowing to remove P and C. When the C content in the desulfurized molten iron is ≤0.05wt% and the P content is ≤0.01wt%, the blowing ends. The converter taps out the steel and removes slag. During the tapping process, deoxidizing alloy (Al particles) is added. Low carbon CrFe alloy blocks (addition amount 33.21kg / ton) and SbFe alloy blocks (addition amount 1.21kg / ton) are added to the obtained molten steel. Then it is put into the ladle. The ladle is blown with argon to stir and promote the floating of inclusions. Then it is transferred to LF for refining. Alloy is added, slag is added, the temperature is raised, and the composition is continuously adjusted to obtain molten steel with the target composition.
[0076] (2) After the molten steel obtained in step (1) enters the tundish, LaCe rare earth wire (addition amount is 0.64 kg / ton) is added. After the rare earth wire melts and is mixed evenly, the resulting mixture is continuously cast to obtain a continuously cast billet.
[0077] (3) Cut the continuous casting billet obtained in step (2) into 150mm thick slabs and send them into a heating furnace to be heated to 1230℃. When exiting the heating furnace, use high-pressure water to remove phosphorus and then send them into the rolling mill for rough rolling and finish rolling. The rough rolling end temperature is 980℃, the finish rolling temperature is 875℃, and the coiling temperature is 670℃ to obtain rare earth microalloyed steel with a thickness of 10mm.
[0078] The rare earth microalloyed steel contains the following chemical composition by mass fraction: C: 0.093%, Si: 0.46%, Mn: 1.507%, P: 0.010%, S: 0.008%, Cr: 1.519%, Cu: 0.13%, Sb: 0.091%, La: 0.0311%, Ce: 0.0105%, with the balance being Fe and unavoidable impurities.
[0079] Example 3
[0080] This embodiment is used to illustrate the rare earth-containing microalloyed steel and its preparation method according to the present invention.
[0081] (1) Lime powder is injected into the ladle for desulfurization, and then slag is removed. When the temperature of the molten iron is ≥1300℃ and the S content in the molten iron is ≤0.007wt%, desulfurized molten iron is obtained. The desulfurized molten iron enters the converter for steelmaking. Lime is added to the top of the converter for oxygen blowing to remove P and C. When the C content in the desulfurized molten iron is ≤0.05wt% and the P content is ≤0.01wt%, the blowing ends. The slag is blocked when the steel is tapped from the converter, and deoxidizing alloy (Al particles) is added during the tapping process. Low carbon CrFe alloy blocks (addition amount 22.14kg / ton) and SbFe alloy blocks (addition amount 1.81kg / ton) are added to the obtained molten steel. Then it is put into the ladle. The ladle is blown with argon to stir and promote the floating of inclusions. Then it is transferred to LF for refining. Alloy is added, slag is added, the temperature is raised, and the composition is continuously adjusted to obtain molten steel with the target composition.
[0082] (2) After the molten steel obtained in step (1) enters the tundish, LaCe rare earth wire (addition amount is 0.44 kg / ton) is added. After the rare earth wire melts and is mixed, the resulting mixture is continuously cast to obtain a continuously cast billet.
[0083] (3) Cut the continuous casting billet obtained in step (2) into 150mm thick slabs and send them into a heating furnace to be heated to 1220℃. When exiting the heating furnace, use high-pressure water to remove phosphorus and then send them into the rolling mill for rough rolling and finish rolling. The rough rolling end temperature is 970℃, the finish rolling temperature is 850℃, and the coiling temperature is 660℃ to obtain rare earth microalloyed steel with a thickness of 12mm.
[0084] The rare earth microalloyed steel contains the following chemical composition by mass fraction: C: 0.108%, Si: 0.29%, Mn: 1.299%, P: 0.012%, S: 0.007%, Cr: 1.322%, Cu: 0.09%, Sb: 0.12%, La: 0.0191%, Ce: 0.0095%, with the balance being Fe and unavoidable impurities.
[0085] Example 4
[0086] This embodiment is used to illustrate the rare earth-containing microalloyed steel and its preparation method according to the present invention.
[0087] (1) Lime powder is injected into the ladle for desulfurization, and then slag is removed. When the temperature of the molten iron is ≥1300℃ and the S content in the molten iron is ≤0.007wt%, desulfurized molten iron is obtained. The desulfurized molten iron enters the converter for steelmaking. Lime is added to the top of the converter for oxygen blowing to remove P and C. When the C content in the desulfurized molten iron is ≤0.05wt% and the P content is ≤0.01wt%, the blowing ends. The slag is blocked when the steel is tapped from the converter, and deoxidizing alloy (Al particles) is added during the tapping process. Low carbon CrFe alloy blocks (addition amount 37.4kg / ton) and SbFe alloy blocks (addition amount 1.13kg / ton) are added to the obtained molten steel. Then it is put into the ladle. The ladle is blown with argon to stir and promote the floating of inclusions. Then it is transferred to LF for refining. Alloy is added, slag is added, the temperature is raised, and the composition is continuously adjusted to obtain molten steel with the target composition.
[0088] (2) After the molten steel obtained in step (1) enters the tundish, LaCe rare earth wire (addition amount is 0.57kg / ton) is added. After the rare earth wire melts and is mixed evenly, the resulting mixture is continuously cast to obtain a continuously cast billet.
[0089] (3) Cut the continuous casting billet obtained in step (2) into 150mm thick slabs and send them into a heating furnace to be heated to 1200℃. When exiting the heating furnace, use high-pressure water to remove phosphorus and then send them into the rolling mill for rough rolling and finish rolling. The rough rolling end temperature is 990℃, the finish rolling temperature is 900℃, and the coiling temperature is 700℃ to obtain rare earth microalloyed steel with a thickness of 8mm.
[0090] The rare earth microalloyed steel contains the following chemical composition by mass fraction: C: 0.15%, Si: 0.22%, Mn: 1.215%, P: 0.008%, S: 0.005%, Cr: 1.92%, Cu: 0.05%, Sb: 0.087%, La: 0.0223%, Ce: 0.015%, with the balance being Fe and unavoidable impurities.
[0091] Example 5
[0092] This embodiment is used to illustrate the rare earth-containing microalloyed steel and its preparation method according to the present invention.
[0093] (1) Lime powder is injected into the ladle for desulfurization, and then slag is removed. When the temperature of the molten iron is ≥1300℃ and the S content in the molten iron is ≤0.007wt%, desulfurized molten iron is obtained. The desulfurized molten iron enters the converter for steelmaking. Lime is added to the top of the converter for oxygen blowing to remove P and C. When the C content in the desulfurized molten iron is ≤0.05wt% and the P content is ≤0.01wt%, the blowing ends. The slag is blocked when the steel is tapped from the converter, and deoxidizing alloy (Al particles) is added during the tapping process. Low carbon CrFe alloy blocks (addition amount 17.9kg / ton) and SbFe alloy blocks (addition amount 1.64kg / ton) are added to the obtained molten steel. Then it is put into the ladle. The ladle is blown with argon to stir and promote the floating of inclusions. Then it is transferred to LF for refining. Alloy is added, slag is added, the temperature is raised, and the composition is continuously adjusted to obtain molten steel with the target composition.
[0094] (2) After the molten steel obtained in step (1) enters the tundish, La rare earth wire (addition amount is 0.51 kg / ton) is added. After the rare earth wire melts and is mixed, the resulting mixture is continuously cast to obtain a continuously cast billet.
[0095] (3) Cut the continuous casting billet obtained in step (2) into 150mm thick slabs and send them into a heating furnace to be heated to 1250℃. When exiting the heating furnace, use high-pressure water to remove phosphorus and then send them into the rolling mill for rough rolling and finish rolling. The rough rolling end temperature is 990℃, the finish rolling temperature is 840℃, and the coiling temperature is 610℃ to obtain rare earth microalloyed steel with a thickness of 8mm.
[0096] The rare earth microalloyed steel contains the following chemical composition by mass fraction: C: 0.17%, Si: 0.53%, Mn: 1.55%, P: 0.011%, S: 0.009%, Cr: 1.12%, Cu: 0.17%, Sb: 0.113%, La: 0.0345%, with the balance being Fe and unavoidable impurities.
[0097] Comparative Example 1
[0098] The method described in Example 1 was implemented, except that in step (1), the amount of SbFe alloy block added was adjusted, and the content of Sb (by weight) in the final rare earth microalloyed steel was 0.043%, and the content of the other components was within the range required by the present invention, and was basically consistent with the rare earth microalloyed steel in Example 1.
[0099] Comparative Example 2
[0100] The method described in Example 1 was implemented, except that in step (1), the amount of low-carbon CrFe alloy block added was adjusted, and the Cr content (weight percentage) in the final rare earth microalloyed steel was 0.062%, and the content of the other components was within the range required by the present invention, and was basically consistent with the rare earth microalloyed steel in Example 1.
[0101] Comparative Example 3
[0102] The method described in Example 1 was implemented, except that in step (2), the amount of LaCe rare earth wire added was adjusted, and the content of La (by weight) in the final rare earth microalloyed steel was 0.042%, the content of Ce (by weight) was 0.0253%, and the content of the remaining components was within the range required by the present invention and was basically consistent with the rare earth microalloyed steel in Example 1.
[0103] Comparative Example 4
[0104] The method described in Example 1 was implemented, except that in step (2), the amount of LaCe rare earth wire added was adjusted, and the content of La (by weight) in the final rare earth microalloyed steel was 0.004%, the content of Ce (by weight) was 0.003%, and the content of the remaining components was within the range required by the present invention and was basically consistent with the rare earth microalloyed steel in Example 1.
[0105] Test Example 1
[0106] Corrosion resistance tests were conducted on the rare earth-containing microalloyed steels prepared in Examples 1-5 and Comparative Examples 1-4, as well as ordinary 16Mn steel. The test method was as follows: the rare earth-containing microalloyed steels were placed in the environment of the top circulation line of a coking unit with sludge (chloride ion saturation, humidity 100%, hydrogen sulfide content not less than 100ppm) and taken out after 180 days. The corrosion rate was detected and calculated. The results are shown in Table 1 below.
[0107] Table 1
[0108] Example number Uniform corrosion rate (mm / a) Relative reduction rate of 16Mn Example 1 0.53 68% Example 2 0.77 54% Example 3 0.66 61% Example 4 0.64 62% Example 5 0.79 53% Comparative Example 1 0.96 41% Comparative Example 2 1.42 16% Comparative Example 3 1.16 31% Comparative Example 4 1.57 7% 16Mn steel 1.69 0
[0109] As can be seen from the results in Table 1 above, the rare earth-containing microalloyed steels prepared in Examples 1-5 of this invention exhibit excellent resistance to chlorine and hydrogen sulfide corrosion. Meanwhile, a comparison between Example 1 and Comparative Examples 1-2 shows that excessively low Sb or Cr content in the rare earth-containing microalloyed steel leads to a significant reduction in the steel's corrosion resistance; a comparison between Example 1 and Comparative Examples 3-4 shows that both excessively low and excessively high rare earth element content in the rare earth-containing microalloyed steel result in a substantial reduction in the steel's corrosion resistance.
[0110] Test Example 2
[0111] The rare earth-containing microalloyed steels prepared in Examples 1-5 were subjected to yield strength, tensile strength and elongation tests using slow strain rate tensile tests. The results are shown in Table 2 below.
[0112] Table 2
[0113] Example number Yield strength (MPa) Tensile strength (MPa) Elongation after fracture Example 1 305 530 23.5 Example 2 295 497 24.7 Example 3 285 522 21.7 Example 4 314 524 22.4 Example 5 297 493 27.6 Requirements for 16Mn steel 275~345 470~660 ≥21%
[0114] As can be seen from the results in Table 2, the yield strength, tensile strength and elongation of the rare earth-containing microalloyed steels prepared in Examples 1-5 of the present invention are not lower than those of ordinary 16Mn steel, and the mechanical properties are good.
[0115] In summary, this invention significantly improves the resistance to chlorine and hydrogen sulfide corrosion of 16Mn steel by using rare earth alloying and scientifically optimizing the composition of 16Mn steel, thereby limiting the Cr and Sb contents, while ensuring its mechanical properties.
[0116] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.
Claims
1. A rare earth containing microalloyed steel, characterized in that, Based on the total mass of the rare earth-containing microalloyed steel, its chemical composition by mass fraction is as follows: C: 0.065~0.16%, Si: 0.25~0.50%, Mn: 1.2~1.5%, P: 0.007~0.013%, S: 0.001~0.01%, Cr: 1.20~2.0%, Cu: 0.01~0.18%, Sb: 0.09~0.12%, rare earth elements: 0.02~0.05%, with the balance being Fe and unavoidable impurities; wherein the rare earth elements are La and Ce; The corrosion rate of the rare earth-containing microalloyed steel in the atmospheric and vacuum distillation unit and the coking unit top circulation process environment is less than 0.8 mm / a, wherein the process environment is saturated with chloride ions, the humidity is 100%, and the hydrogen sulfide content is not less than 100 ppm. The preparation method of the rare earth-containing microalloyed steel includes the following steps: S10. Add rare earth wire to the molten steel. After the rare earth wire melts and is mixed, the resulting mixture is continuously cast to obtain a continuously cast billet. S20. Roll the continuously cast billet to obtain rare earth microalloyed steel; In step S20, the rolling process includes: cutting the continuously cast billet to a fixed length, sending it into a heating furnace and heating it to 1200~1250℃, removing phosphorus with high-pressure water when it exits the heating furnace, and then sending it into a rolling mill for rolling and coiling; wherein the final rolling temperature is 840~910℃ and the coiling temperature is 600~720℃.
2. A method of producing the rare earth containing microalloyed steel according to claim 1, characterized in that, The method includes the following steps: S10. Add rare earth wire to the molten steel. After the rare earth wire melts and is mixed, the resulting mixture is continuously cast to obtain a continuously cast billet. S20. Roll the continuously cast billet to obtain rare earth microalloyed steel; In step S10, the continuously cast billet comprises the following components by mass fraction: C: 0.065~0.16%, Si: 0.25~0.50%, Mn: 1.2~1.5%, P: ≤0.013%, S: ≤0.01%, Cr: 1.20~2.0%, Cu: ≤0.18%, Sb: 0.09~0.12%, and rare earth elements: 0.02~0.05%; wherein the rare earth elements are La and Ce. In step S20, the rolling process includes: cutting the continuously cast billet to a fixed length, sending it into a heating furnace to be heated to 1200~1250°C, removing phosphorus with high-pressure water when it exits the heating furnace, and then sending it into a rolling mill for rolling and coiling.
3. The method of claim 2, wherein, In step S10, the preparation process of the molten steel includes: A1. Desulfurize and remove slag from molten iron. When the temperature of the molten iron is ≥1300℃ and the S content in the molten iron is ≤0.007wt%, desulfurized molten iron is obtained. A2. The desulfurized molten iron is introduced into the top and bottom of the converter for oxygen re-blowing. When the C content in the desulfurized molten iron is ≤0.05wt% and the P content is ≤0.01wt%, the blowing process ends. A3. After tapping the steel and removing the slag, add SbFe alloy blocks and low-carbon CrFe alloy blocks to the obtained molten steel, then pour it into a ladle. Stir the ladle with argon, then transfer it to LF refining, add alloys, add slag, raise the temperature, and continuously adjust the composition to make the molten steel composition meet the target requirements.
4. The method of claim 3, wherein, In step A3, a deoxidizing alloy is added during the tapping process.
5. The method of claim 2, wherein, The rolling step further includes: cold rolling and annealing the steel obtained after coiling.
6. Use of the rare earth containing microalloyed steel according to claim 1, characterized in that, The rare earth-containing microalloyed steel is used to manufacture petrochemical equipment.
Citation Information
Patent Citations
Rare earth corrosion-resistant steel rich in alloyed rare earth elements and manufacturing method of rare earth corrosion-resistant steel
CN110983156A
Weathering steel containing rare earth and preparation method thereof
CN113737105A
Ultrastrong sulfuric acid and hydrochloric acid corrosion resistant low alloy steel and preparation method thereof
CN114214558A
Rare earth weathering steel rich in alloying rare earth elements and manufacturing method of rare earth weathering steel
CN110923572A
Corrosion resistant steel for crude oil and heavy oil storage speed
JP2001214236A