Polyester impact modifier

By using polyester composed of isosorbide, dicarboxylic acid or anhydride and polyol as an impact modifier in biopolymers, the problem that petroleum-based polymers are not easy to degrade is solved and the impact resistance of biopolymers is improved. and environmental friendliness, achieving compostability.

CN117897429BActive Publication Date: 2024-10-29丹尼米尔知识产权有限责任公司
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202280048740.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-13
Publication Date
2024-10-29
Estimated Expiration
2042-05-13

AI Technical Summary

Technical Problem

Existing petroleum-based polymers do not degrade easily in landfills or home composting, leading to environmental pollution, and existing biopolymers require non-biodegradable additives to improve physical properties, reducing environmental benefits.

Method used

A polyester composed of isosorbide, dicarboxylic acid or anhydride and polyol was developed as an impact modifier for use in compositions with biodegradable polymers to improve their physical properties and meet the requirements of Composting Requirements.

Benefits of technology

The polyester adds improved impact resistance and toughness to the polymer while meeting biodegradable and compostable requirements, reducing the risk of environmental pollution.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention discloses a polyester composed of: (1) about 15% to about 40% by weight of isosorbide monomer repeating units; (2) about 25% to about 60% by weight of dicarboxylic acids or anhydrides such as succinic acid or anhydrides; and (3) about 10% to about 20% by weight of monomer repeating units of polyols such as 1,3-propylene glycol. In some cases, the polymer may also include monomer repeating units of methyl nadic anhydride or nadic anhydride. The present invention also discloses a polymer composition comprising a polyester and a biodegradable polymer selected from the group consisting of polylactic acid, polyhydroxyalkanoate, and mixtures thereof.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to polyesters suitable for use as impact modifiers and biodegradable polymer compositions comprising such impact modifiers. Background Art

[0002] Petroleum-based polymers, such as polyethylene (PE), polypropylene (PP), or polyethylene terephthalate (PET), have been used for decades in a wide variety of applications. While these polymers can provide good strength, barrier, and / or printability properties, unfortunately, these polymers do not readily degrade or break down after disposal in landfills or through home composting techniques. As a result, films, bags, and other materials made from these polymers can remain in landfills for centuries after disposal.

[0003] Therefore, there is an increasing demand for alternative polymers that are bioderived, biodegradable and / or compostable. Examples of such polymers include polylactic acid and polyhydroxyalkanoates. Although these biopolymers offer significant advantages in terms of biodegradability and / or compostability, it is often necessary to mix various additives with the biopolymers to improve the physical properties of the biopolymers.

[0004] If the additives mixed into the biopolymer are not biodegradable and / or compostable, the environmental benefits of the biopolymer are reduced. Therefore, there is a need to provide additives for use with biopolymers, such as polylactic acid and polyhydroxyalkanoates, that are themselves biodegradable and / or compostable. Summary of the invention

[0005] The compostable polyesters according to the present invention meet the above-mentioned and other needs.

[0006] In a first aspect, the present invention provides a polyester. According to a specific embodiment, the polyester is composed of: (1) about 15% to about 40% by weight of monomer repeating units of isosorbide; (2) about 25% to about 60% by weight of monomer repeating units of dicarboxylic acid or anhydride; and (3) about 10% to about 20% by weight of monomer repeating units of polyol. All of these weight percentages are based on the total weight of the polyester.

[0007] The polyester also has a weight average molecular weight of at least 8,000 Daltons as determined by ASTM D5296-05. More preferably, the polyester has a weight average molecular weight of from about 10,000 to about 15,000 Daltons as determined by ASTM D5296-05.

[0008] In a specific embodiment, the dicarboxylic acid or anhydride is preferably selected from the group consisting of succinic acid, succinic anhydride, glutaric acid, pimelic acid, undecanoic acid, dodecanoic acid, dodecanedioic acid, suberic acid, azelaic acid, sebacic acid, adipic acid, phthalic anhydride, dimethyl terephthalate, terephthalic acid, isophthalic acid, 1,8-naphthalene dicarboxylic anhydride, 1,8-naphthalene dicarboxylic acid, dimethyl 1,8-naphthalene dicarboxylate, dimethyl isophthalate, phthalic acid, pyromellitic anhydride, mellitic anhydride, The group consisting of mellitic acid, trimellitic anhydride, 3,3'4,4'-benzophenonetetracarboxylic anhydride, 3,3'4,4'-benzophenonetetracarboxylic acid, trimellitic acid, nadic anhydride, methyl nadic anhydride, C36 dimer acid, partially hydrogenated C36 dimer acid, polyethylene terephthalate recycled polymer, polybutylene terephthalate recycled polymer, polyethylene terephthalate virgin polymer, polybutylene terephthalate virgin polymer, and mixtures thereof.

[0009] More preferably, the dicarboxylic acid or anhydride is selected from the group consisting of succinic acid, succinic anhydride, nadic anhydride, methyl nadic anhydride, sebacic acid, C36 dimer acid, partially hydrogenated C36 dimer acid, and mixtures thereof.

[0010] In a particularly preferred embodiment, the dicarboxylic acid or anhydride is composed of a mixture of (1) succinic acid or succinic anhydride and (2) nadic anhydride, methyl nadic anhydride, C36 dimer acid or partially hydrogenated C36 dimer acid, and mixtures thereof. For this embodiment, the polyester is preferably about 25% to about 35% by weight succinic acid or succinic anhydride and about 10% to about 25% by weight nadic anhydride, methyl nadic anhydride, C36 dimer acid or partially hydrogenated C36 dimer acid.

[0011] In some embodiments, the polyol is preferably selected from the group consisting of glycerol, ethylene glycol, diethylene glycol, 1,3-propylene glycol, 1,4-butylene glycol, 1,5-pentanediol, 1,6-hexanediol, 2-methyl, neopentyl glycol, propylene glycol, triethylene glycol, tetraethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, tetrapropylene glycol, trimethylene glycol, 1,1,1-trimethylolethane, 1,2,3-trimethylolpropane, methylpropylene glycol, pentaerythritol, and polyoxyalkylene polyols comprising monomer repeating units of ethylene oxide, propylene oxide or butylene oxide, and mixtures thereof.

[0012] More preferably, the polyol is selected from the group consisting of 1,3-propylene glycol, 1,4-butylene glycol, 1,6-hexanediol, methylpropylene glycol, and mixtures thereof. Even more preferably, the polyol comprises 1,3-propylene glycol.

[0013] In some cases, the dicarboxylic acid or anhydride preferably comprises succinic acid or anhydride, and the polyol preferably comprises 1,3-propylene glycol.

[0014] In an alternative embodiment, the isosorbide may be omitted from the polyester. In this case, the polyester is composed of: (1) about 35% to about 65% by weight of monomer repeating units of a dicarboxylic acid or anhydride selected from the group consisting of succinic acid, succinic anhydride, nadic anhydride, methyl nadic anhydride, sebacic acid, C36 dimer acid or partially hydrogenated C36 dimer acid, and mixtures thereof; and (2) about 35% to about 65% by weight of monomer repeating units of a polyol.

[0015] In a preferred embodiment, the dicarboxylic acid or anhydride is composed of (1) succinic acid or succinic anhydride and (2) nadic anhydride, methyl nadic anhydride, C36 dimer acid or partially hydrogenated C36 dimer acid, and mixtures thereof. For this embodiment, the polyester is preferably about 30% to about 40% by weight of succinic acid or succinic anhydride, and about 10% to about 20% by weight of nadic anhydride, methyl nadic anhydride, C36 dimer acid or partially hydrogenated C36 dimer acid.

[0016] Suitable polyols for use in the substituted polyester are the same as those mentioned above for the polyester, including isosorbide. In addition, for the substituted polyester, the weight average molecular weight of the polyester is at least 8,000 Daltons as determined by ASTM D5296-05. More preferably, the polyester has a weight average molecular weight of about 10,000 to about 15,000 Daltons as determined by ASTM D5296-05.

[0017] In a second aspect, the present invention provides a polymer composition. The polymer composition generally comprises from about 50% to about 95% by weight of a biodegradable polymer selected from the group consisting of polylactic acid, polyhydroxyalkanoate and mixtures thereof. The polymer composition also comprises from about 5% to about 50% by weight of an impact-modified polyester. The impact-modified polyester is composed, in sequence, of: (1) from about 15% to about 40% by weight of isosorbide monomer repeating units based on the total weight of the polyester; (2) from about 25% to about 60% by weight of dicarboxylic acid or anhydride monomer repeating units based on the total weight of the polyester; and (3) from about 10% to about 20% by weight of polyol monomer repeating units based on the total weight of the polyester. The impact-modified polyester also has a weight average molecular weight of at least 8,000 Daltons as determined by ASTM D5296-05.

[0018] In a specific embodiment, the dicarboxylic acid or anhydride is preferably selected from succinic acid, succinic anhydride, glutaric acid, pimelic acid, undecanoic acid, dodecanoic acid, dodecanedioic acid, suberic acid, azelaic acid, sebacic acid, adipic acid, phthalic anhydride, dimethyl terephthalate, terephthalic acid, isophthalic acid, 1,8-naphthalene dicarboxylic anhydride, 1,8-naphthalene dicarboxylic acid, 1,8-naphthalene dicarboxylic acid dimethyl ester, dimethyl isophthalate, phthalic acid, pyromellitic anhydride, mellitic anhydride, The group consisting of mellitic acid, trimellitic anhydride, 3,3'4,4'-benzophenonetetracarboxylic anhydride, 3,3'4,4'-benzophenonetetracarboxylic acid, trimellitic acid, nadic anhydride, methyl nadic anhydride, C36 dimer acid, partially hydrogenated C36 dimer acid, polyethylene terephthalate recycled polymer, polybutylene terephthalate recycled polymer, polyethylene terephthalate virgin polymer, polybutylene terephthalate virgin polymer, and mixtures thereof.

[0019] More preferably, the dicarboxylic acid or anhydride is selected from the group consisting of succinic acid, succinic anhydride, nadic anhydride, methyl nadic anhydride, sebacic acid, C36 dimer acid, partially hydrogenated C36 dimer acid, and mixtures thereof.

[0020] In a particularly preferred embodiment, the dicarboxylic acid or anhydride is composed of a mixture of (1) succinic acid or succinic anhydride and (2) nadic anhydride, methyl nadic anhydride, C36 dimer acid or partially hydrogenated C36 dimer acid, and mixtures thereof. For this embodiment, the polyester is preferably about 25% to about 35% by weight succinic acid or succinic anhydride and about 10% to about 25% by weight nadic anhydride, methyl nadic anhydride, C36 dimer acid or partially hydrogenated C36 dimer acid.

[0021] In some embodiments, the polyol is preferably selected from the group consisting of glycerol, ethylene glycol, diethylene glycol, 1,3-propylene glycol, 1,4-butylene glycol, 1,5-pentanediol, 1,6-hexanediol, 2-methyl, neopentyl glycol, propylene glycol, triethylene glycol, tetraethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, tetrapropylene glycol, trimethylene glycol, 1,1,1-trimethylolethane, 1,2,3-trimethylolpropane, methylpropylene glycol, pentaerythritol, and polyoxyalkylene polyols comprising monomer repeating units of ethylene oxide, propylene oxide or butylene oxide, and mixtures thereof.

[0022] More preferably, the polyol is selected from the group consisting of 1,3-propylene glycol, 1,4-butylene glycol, 1,6-hexanediol, methylpropylene glycol, and mixtures thereof. Even more preferably, the polyol comprises 1,3-propylene glycol.

[0023] In some cases, the dicarboxylic acid or anhydride preferably comprises succinic acid or anhydride, and the polyol preferably comprises 1,3-propylene glycol.

[0024] According to a specific embodiment, the polymer composition more preferably comprises about 60% to about 85% by weight of the biodegradable polymer and about 5% to about 30% by weight of the impact-modified polyester. Even more preferably, the polymer composition comprises about 7.5% to about 15% by weight of the impact-modified polyester.

[0025] In some cases, the biodegradable polymer preferably comprises polylactic acid. In other embodiments, the biodegradable polymer preferably comprises at least one polyhydroxyalkanoate. In some embodiments, the biodegradable polymer preferably comprises a mixture of polylactic acid and polyhydroxyalkanoate. For example, in some embodiments, based on the total weight of the polymer composition, the polymer composition may include about 5% to about 25% by weight of polylactic acid and about 70% to about 90% by weight of at least one polyhydroxyalkanoate.

[0026] According to a specific embodiment, wherein the polymer composition comprises a polyhydroxyalkanoate, the at least one polyhydroxyalkanoate preferably consists of poly-3-hydroxybutyrate-co-3-hydroxyhexanoate ("P(3HB-co-3HHx)").

[0027] In some cases, the (3HB-co-3HHx) preferably consists of about 75% to about 99% hydroxybutyric acid by mole and about 1% to about 25% hydroxyhexanoate by mole. More preferably, the (3HB-co-3HHx) consists of about 93% to about 98% hydroxybutyric acid by mole and about 2% to about 7% hydroxyhexanoate by mole.

[0028] In other embodiments, the at least one polyhydroxyalkanoate may include a terpolymer consisting of about 75% to about 99.9% mole percent monomer repeating units of 3-hydroxybutyric acid, about 0.1% to about 25% mole percent monomer repeating units of 3-hydroxyhexanoate, and about 0.1% to about 25% mole percent monomer repeating units of a third 3-hydroxyalkanoate having 5 to 12 carbon atoms.

[0029] According to a specific embodiment, the at least one polyhydroxyalkanoate preferably has a weight average molecular weight of about 50,000 Daltons to about 2.5 million Daltons as determined by ASTM D5296-05. More preferably, the at least one polyhydroxyalkanoate has a weight average molecular weight of about 500,000 Daltons to about 750,000 Daltons as determined by ASTM D5296-05.

[0030] The polymer composition may also include further additives. In some embodiments, the polymer composition further includes about 1% to about 10% by weight of at least one plasticizer; about 0.1% to about 5% by weight of at least one nucleating agent; and about 0.1% to about 10% by weight of a filler.

[0031] In some cases, in addition to polylactic acid and / or polyhydroxyalkanoate, the polymer composition may also include additional biodegradable polymers. Thus, in a particular embodiment, the polymer composition may also include about 5% to about 50% by weight of at least one biodegradable polymer selected from the group consisting of polycaprolactone, polyvinyl sebacate, polybutylene succinate, polybutylene succinate-adipate, polybutylene adipate, polyvinyl acetate, and mixtures thereof.

[0032] According to certain embodiments, the polymer composition is preferably biodegradable as determined using ASTM standard D5988. Additionally, in some embodiments, the polymer composition is preferably home compostable as determined using ASTM standard D6868.

[0033] The present invention also provides various end-use products that can be formed from the above-mentioned polymer composition. Therefore, according to one embodiment, the present invention provides a molded sheet consisting of the polymer composition. In a second embodiment, the present invention provides a molded article consisting of the polymer composition, wherein the molded article is formed by thermoforming, injection molding or blow molding. In another embodiment, the present invention provides a film consisting of the polymer composition, wherein the film is a blown film or a cast film. In another embodiment, the present invention provides a fiber consisting of the polymer composition. DETAILED DESCRIPTION

[0034] The present invention first provides novel polyesters which are suitable for use as impact modifiers in biodegradable and / or compostable polymer compositions.

[0035] Typically, the polyester is composed of at least three different types of monomer repeating units derived from: (1) isosorbide; (2) succinic acid or anhydride; and (3) 1,3-propylene glycol. In terms of amount, the polyester is typically composed of: (1) about 15% to about 40% by weight of monomer repeating units of isosorbide; (2) about 25% to about 60% by weight of monomer repeating units of dicarboxylic acid or anhydride; and (3) about 10% to about 20% by weight of monomer repeating units of polyols.

[0036] A variety of dicarboxylic acids and anhydrides are considered suitable for use in the preparation of polyesters. For example, the dicarboxylic acids and anhydrides may be suitably selected from succinic acid, succinic anhydride, glutaric acid, pimelic acid, undecanoic acid, dodecanoic acid, dodecanedioic acid, suberic acid, azelaic acid, sebacic acid, adipic acid, phthalic anhydride, dimethyl terephthalate, terephthalic acid, isophthalic acid, 1,8-naphthalene dicarboxylic anhydride, 1,8-naphthalene dicarboxylic acid, dimethyl 1,8-naphthalene dicarboxylate, dimethyl isophthalate, phthalic acid, pyromellitic anhydride, mellitic anhydride, mellitic acid, phthalic acid, pyromellitic anhydride, mellitic acid, phthalic ... The present invention is a group consisting of a polyol, ...

[0037] More preferably, the dicarboxylic acid or anhydride is selected from the group consisting of succinic acid, succinic anhydride, nadic anhydride, methyl nadic anhydride, sebacic acid, C36 dimer acid, partially hydrogenated C36 dimer acid, and mixtures thereof.

[0038] In a particularly preferred embodiment, the dicarboxylic acid or anhydride is composed of a mixture of (1) succinic acid or succinic anhydride and (2) nadic anhydride, methyl nadic anhydride, C36 dimer acid or partially hydrogenated C36 dimer acid, and mixtures thereof. For this embodiment, the polyester is preferably about 25% to about 35% by weight succinic acid or succinic anhydride, and about 10% to about 25% by weight nadic anhydride, methyl nadic anhydride, C36 dimer acid or partially hydrogenated C36 dimer acid.

[0039] A range of polyols are also considered suitable for polyesters. Examples of suitable polyols may be selected from the group consisting of glycerol, ethylene glycol, diethylene glycol, 1,3-propylene glycol, 1,4-butylene glycol, 1,5-pentanediol, 1,6-hexanediol, 2-methyl, neopentyl glycol, propylene glycol, triethylene glycol, tetraethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, tetrapropylene glycol, trimethylene glycol, 1,1,1-trimethylolethane, 1,2,3-trimethylolpropane, methylpropylene glycol, pentaerythritol, and polyoxyalkylene polyols comprising monomer repeating units of ethylene oxide, propylene oxide or butylene oxide, and mixtures thereof.

[0040] More preferably, the polyol is selected from the group consisting of 1,3-propylene glycol, 1,4-butylene glycol, 1,6-hexanediol, methylpropylene glycol, and mixtures thereof. Even more preferably, the polyol comprises 1,3-propylene glycol.

[0041] In a particularly preferred embodiment, the dicarboxylic acid or anhydride preferably includes succinic acid or anhydride, and the polyol preferably includes 1,3-propylene glycol.

[0042] The polyester also has a weight average molecular weight of at least 8,000 Daltons as determined by ASTM D5296-05. More preferably, the polyester has a weight average molecular weight of from about 10,000 to about 15,000 Daltons as determined by ASTM D5296-05.

[0043] Typically, polyesters can be prepared by charging isosorbide to a reaction flask or other reactor equipped with a nitrogen inlet, vacuum capability, heating and stirring. First, the isosorbide is melted and the molten material is then vacuum degassed. Subsequently, the diacid is added and the contents of the flask are reacted at a temperature up to 220°C until the evolution of water slows, at which point all remaining diols are charged. Esterification is accomplished at temperatures up to 220°C and vacuum pressures as low as 3.3 kPa.

[0044] In an alternative embodiment, isosorbide may be omitted from the polyester. In this case, the polyester is composed of: (1) about 35% to about 65% by weight of monomer repeating units of a dicarboxylic acid or anhydride selected from the group consisting of succinic acid, succinic anhydride, nadic anhydride, methyl nadic anhydride, sebacic acid, C36 dimer acid, partially hydrogenated C36 dimer acid, and mixtures thereof; and (2) about 35% to about 65% by weight of monomer repeating units of a polyol.

[0045] In a preferred embodiment, the dicarboxylic acid or anhydride is composed of (1) succinic acid or succinic anhydride and (2) nadic anhydride, methyl nadic anhydride, C36 dimer acid or partially hydrogenated C36 dimer acid, and mixtures thereof. For this embodiment, the polyester is preferably about 30% to about 40% by weight of succinic acid or succinic anhydride and about 10% to about 20% by weight of nadic anhydride, methyl nadic anhydride, C36 dimer acid or partially hydrogenated C36 dimer acid.

[0046] Suitable polyols for use in the substituted polyester are the same as those mentioned above for the polyester, including isosorbide. In addition, for the substituted polyester, the weight average molecular weight of the polyester is at least 8,000 Daltons as determined by ASTM D5296-05. More preferably, the polyester has a weight average molecular weight of about 10,000 to about 15,000 Daltons as determined by ASTM D5296-05.

[0047] The polyesters according to the present invention are suitable for use as impact modifiers in polymer compositions. "Impact modifiers" as used in the present invention are additives used to increase the durability and toughness of polymer resins, wherein toughness is measured by the area under the stress-strain curve of a standard tensile elongation and modulus test. In addition, the toughness of a polymer can be correlated by a notched Izod test. Polymers that exhibit higher impact numbers will indicate increased toughness.

[0048] The polyesters according to the present invention are also preferably biodegradable as determined using ASTM standard D5511. In addition, in some embodiments, the polyesters are preferably home compostable as determined using ASTM standard D6868.

[0049] The present invention also provides a polymer composition comprising the polyester as described. Typically, the polymer composition combines the impact modifier polyester with at least one biodegradable polymer selected from the group consisting of polylactic acid, polyhydroxyalkanoate, and mixtures thereof. Typically, the polymer composition comprises about 5% to about 50% by weight of the impact modified polyester and about 50% to about 95% by weight of the biodegradable polymer selected from the group consisting of polylactic acid, polyhydroxyalkanoate, and mixtures thereof.

[0050] The polymer composition more preferably comprises about 60% to about 85% by weight of the biodegradable polymer and about 5% to about 30% by weight of the impact-modified polyester. Even more preferably, the polymer composition comprises about 7.5% to about 15% by weight of the impact-modified polyester.

[0051] Likewise, the impact modifier used in the polymer composition is a polyester according to the aforementioned disclosure. Thus, the impact-modified polyester is composed of: (1) about 15% to about 40% by weight of monomer repeating units of isosorbide; (2) about 25% to about 60% by weight of monomer repeating units of a dicarboxylic acid or anhydride; and (3) about 10% to about 20% by weight of monomer repeating units of a polyol. The weight average molecular weight of the impact-modified polyester is at least 8,000 Daltons as determined by ASTM D5296-05.

[0052] In some cases, the biodegradable polymer preferably includes polylactic acid. In other embodiments, the biodegradable polymer preferably includes at least one polyhydroxyalkanoate. In addition, in a specific embodiment, the biodegradable polymer preferably includes a mixture of polylactic acid and polyhydroxyalkanoate. For example, in some embodiments, based on the total weight of the polymer composition, the polymer composition can include about 5% to about 25% by weight of polylactic acid and about 70% to about 90% by weight of at least one polyhydroxyalkanoate.

[0053] According to a specific embodiment, wherein the polymer composition comprises a polyhydroxyalkanoate, the at least one polyhydroxyalkanoate preferably consists of poly-3-hydroxybutyrate-co-3-hydroxyhexanoate ("P(3HB-co-3HHx)").

[0054] In some embodiments, the 3HB-co-3HHx is preferably composed of about 75% to about 99% hydroxybutyric acid and about 1% to about 25% hydroxyhexanoate by mole. More preferably, the 3HB-co-3HHx is composed of about 93% to about 98% hydroxybutyric acid and about 2% to about 7% hydroxyhexanoate by mole.

[0055] In other embodiments, at least one polyhydroxyalkanoate may include a terpolymer consisting of about 75% to about 99.9% mole percent monomer repeating units of 3-hydroxybutyric acid, about 0.1% to about 25% mole percent monomer repeating units of 3-hydroxyhexanoate, and about 0.1% to about 25% mole percent monomer repeating units of a third 3-hydroxyalkanoate having 5 to 12 carbon atoms.

[0056] According to a specific embodiment, at least one polyhydroxyalkanoate preferably has a weight average molecular weight of about 50,000 Daltons to about 2.5 million Daltons as determined by ASTM D5296-05. More preferably, at least one polyhydroxyalkanoate has a weight average molecular weight of about 500,000 Daltons to about 750,000 Daltons as determined by ASTM D5296-05.

[0057] The polymer composition may also include further additives. For example, the polymer composition may include a plasticizer, a nucleating agent, and / or a filler. In some embodiments, the polymer composition may also include about 1% to about 10% by weight of at least one plasticizer; about 0.1% to about 5% by weight of at least one nucleating agent; and about 0.1% to about 10% by weight of a filler.

[0058] Suitable nucleating agents for use in the polymer composition may, for example, be selected from the group consisting of pentaerythritol, boron nitride, polyhydroxybutyrate, inositol, clay, dipentaerythritol, sorbitol, and mixtures thereof.

[0059] Suitable fillers for use in the polymer composition may, for example, be selected from the group consisting of aragonite, clay, calcium carbonate, cellulose, nanocellulose, talc, kaolinite, montmorillonite, bentonite, silica, chitin, starch, diatomaceous earth, titanium dioxide, nanoclay, mica, and mixtures thereof.

[0060] Suitable plasticizers for use in the polymer composition can be selected, for example, from the group consisting of sebacate, citrate, fatty esters of adipic acid, succinic acid and gluconic acid, lactates, alkyl diesters, citrates, alkyl methyl esters, dibenzoates, propylene carbonate, caprolactone diols having an average molecular weight of 200-10000 g / mol, poly(ethylene) glycols having an average molecular weight of 400-10000 g / mol, esters of vegetable oils, long chain alkyl acids, adipic acid esters, glycerol, isosorbide derivatives or mixtures thereof, HALLGREEN IM-8830 esters, HALLGREEN R-8010 esters, polyhydroxyalkanoate copolymers containing at least 18 mol% of monomer repeating units of hydroxyalkanoates other than hydroxybutyrate, and mixtures thereof.

[0061] In addition, in a particular embodiment, the polymer composition may also include an additional biodegradable polymer in addition to polylactic acid and / or polyhydroxyalkanoate. Therefore, in a particular embodiment, the polymer composition may also include about 5% to about 50% by weight of at least one biodegradable polymer selected from the group consisting of polycaprolactone, polyvinyl sebacate, polybutylene succinate, polybutylene succinate-adipate, polybutylene adipate, polyvinyl acetate, and mixtures thereof.

[0062] According to certain embodiments, the polymer composition as a whole is preferably biodegradable as determined using ASTM standard D5988. Additionally, in some embodiments, the polymer composition is preferably home compostable as determined using ASTM standard D6868.

[0063] A variety of end products can be formed from the polymer composition according to the present invention. Therefore, according to one embodiment, the present invention provides a molded sheet made from the polymer composition. In a second embodiment, the present invention provides a molded article consisting of the polymer composition, wherein the molded article is formed by thermoforming, injection molding or blow molding. In another embodiment, the present invention provides a film consisting of the polymer composition, wherein the film is a blown film or a cast film. In another embodiment, the present invention provides a fiber consisting of the polymer composition.

[0064] Implementation

[0065] The present invention is further described by the following embodiments:

[0066] Embodiment 1. A polyester comprising: monomer repeating units of isosorbide in an amount of about 15% to about 40% by weight, based on the total weight of the polyester; monomer repeating units of a dicarboxylic acid or anhydride in an amount of about 25% to about 60% by weight, based on the total weight of the polyester; and monomer repeating units of a polyol in an amount of about 10% to about 20% by weight, based on the total weight of the polyester, wherein the polyester has a weight average molecular weight of at least 8,000 Daltons as determined by ASTM D5296-05.

[0067] Embodiment 2. The polyester of embodiment 1, wherein the dicarboxylic acid or anhydride is selected from the group consisting of succinic acid, succinic anhydride, glutaric acid, pimelic acid, undecanoic acid, dodecanoic acid, dodecanedioic acid, suberic acid, azelaic acid, sebacic acid, adipic acid, phthalic anhydride, dimethyl terephthalate, terephthalic acid, isophthalic acid, 1,8-naphthalene dicarboxylic anhydride, 1,8-naphthalene dicarboxylic acid, dimethyl 1,8-naphthalene dicarboxylate, dimethyl isophthalate, phthalic acid, pyromellitic anhydride, mellitic acid The present invention is a group consisting of anhydride, mellitic acid, trimellitic anhydride, 3,3'4,4'-benzophenonetetracarboxylic anhydride, 3,3'4,4'-benzophenonetetracarboxylic acid, trimellitic acid, nadic anhydride, methyl nadic anhydride, C36 dimer acid, partially hydrogenated C36 dimer acid, polyethylene terephthalate recycled polymer, polybutylene terephthalate recycled polymer, polyethylene terephthalate virgin polymer, polybutylene terephthalate virgin polymer, and mixtures thereof.

[0068] Embodiment 3. The polyester of embodiment 1 or 2, wherein the dicarboxylic acid or anhydride is selected from the group consisting of succinic acid, succinic anhydride, nadic anhydride, methyl nadic anhydride, sebacic acid, C36 dimer acid, partially hydrogenated C36 dimer acid, and mixtures thereof.

[0069] Embodiment 4. The polyester of any of the preceding embodiments, wherein the dicarboxylic acid or anhydride comprises a mixture of (1) succinic acid or succinic anhydride and (2) nadic anhydride, methyl nadic anhydride, C36 dimer acid, or partially hydrogenated C36 dimer acid, and mixtures thereof.

[0070] Embodiment 5. The polyester of any of the preceding embodiments, wherein the polyester comprises about 25% to about 35% by weight of succinic acid or succinic anhydride, and about 10% to about 25% by weight of nadic anhydride, methyl nadic anhydride, C36 dimer acid, or partially hydrogenated C36 dimer acid.

[0071] Embodiment 6. The polyester of any of the preceding embodiments, wherein the polyol is selected from the group consisting of glycerol, ethylene glycol, diethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 2-methyl, neopentyl glycol, propylene glycol, triethylene glycol, tetraethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, tetrapropylene glycol, trimethylene glycol, 1,1,1-trimethylolethane, 1,2,3-trimethylolpropane, methylpropylene glycol, pentaerythritol, and polyoxyalkylene polyols comprising monomer repeating units of ethylene oxide, propylene oxide or butylene oxide, and mixtures thereof.

[0072] Embodiment 7. The polyester of any of the preceding embodiments, wherein the polyol is selected from the group consisting of 1,3-propylene glycol, 1,4-butylene glycol, 1,6-hexanediol, methylpropylene glycol, and mixtures thereof.

[0073] Embodiment 8. The polyester of any of the preceding embodiments, wherein the polyol comprises 1,3-propylene glycol.

[0074] Embodiment 9. The polyester of any of the preceding embodiments, wherein the dicarboxylic acid or anhydride comprises succinic acid or anhydride and the polyol comprises 1,3-propylene glycol.

[0075] Embodiment 10. The polyester of any of the preceding embodiments, wherein the polyester has a weight average molecular weight of about 10,000 to about 15,000 Daltons as determined by ASTM D5296-05.

[0076] Embodiment 11. A polymer composition comprising: about 50% to about 95% by weight of a biodegradable polymer selected from the group consisting of polylactic acid, polyhydroxyalkanoates and mixtures thereof; about 5% to about 50% by weight of an impact-modified polyester, wherein the impact-modified polyester comprises: about 15% to about 40% by weight of isosorbide monomer repeating units based on the total weight of the polyester; about 25% to about 60% by weight of dicarboxylic acid or anhydride monomer repeating units based on the total weight of the polyester; about 10% to about 20% by weight of polyol monomer repeating units based on the total weight of the polyester, wherein the polyester has a weight average molecular weight of at least 8000 Daltons as determined by ASTM D5296-05.

[0077] Embodiment 12. The polymer composition of embodiment 11, wherein the dicarboxylic acid or anhydride is selected from the group consisting of succinic acid, succinic anhydride, glutaric acid, pimelic acid, undecanoic acid, dodecanoic acid, dodecanedioic acid, suberic acid, azelaic acid, sebacic acid, adipic acid, phthalic anhydride, dimethyl terephthalate, terephthalic acid, isophthalic acid, 1,8-naphthalene dicarboxylic anhydride, 1,8-naphthalene dicarboxylic acid, dimethyl 1,8-naphthalene dicarboxylate, dimethyl isophthalate, phthalic acid, pyromellitic anhydride, benzene dicarboxylic acid, 1,8-naphthalene dicarboxylic acid, 1,8-naphthalene dicarboxylic acid, 1,8-naphthalene dicarboxylic acid, 1,8-naphthalene dicarboxylic acid, 1,8-naphthalene dicarboxylic acid, 1,8-naphthalene dicarboxylic acid, 1,8-naphthalene dicarboxylic acid, 1,8-naphthalene dicarboxylic acid, 1,8-naphthalene dicarboxylic acid, 1,8-naphthalene dicarboxylic acid, 1,8-naphthalene dicarboxylic acid methyl ester ... The group consisting of hexacarboxylic anhydride, mellitic acid, trimellitic anhydride, 3,3'4,4'-benzophenonetetracarboxylic anhydride, 3,3'4,4'-benzophenonetetracarboxylic acid, trimellitic acid, nadic anhydride, methyl nadic anhydride, C36 dimer acid, partially hydrogenated C36 dimer acid, polyethylene terephthalate recycled polymer, polybutylene terephthalate recycled polymer, polyethylene terephthalate virgin polymer, polybutylene terephthalate virgin polymer, and mixtures thereof.

[0078] Embodiment 13. The polymer composition of embodiment 11 or 12, wherein the dicarboxylic acid or anhydride is selected from the group consisting of succinic acid, succinic anhydride, nadic anhydride, methyl nadic anhydride, sebacic acid, C36 dimer acid, partially hydrogenated C36 dimer acid, and mixtures thereof.

[0079] Embodiment 14. The polymer composition of any of embodiments 11-13, wherein the dicarboxylic acid or anhydride comprises a mixture of (1) succinic acid or succinic anhydride and (2) nadic anhydride, methyl nadic anhydride, C36 dimer acid, or partially hydrogenated C36 dimer acid, and mixtures thereof.

[0080] Embodiment 15. The polymer composition of any one of embodiments 11-14, wherein the polyester comprises about 25% to about 35% by weight of succinic acid or succinic anhydride, and about 10% to about 25% by weight of nadic anhydride, methyl nadic anhydride, C36 dimer acid, or partially hydrogenated C36 dimer acid.

[0081] Embodiment 16. The polymer composition of any one of embodiments 11-15, wherein the polyol is selected from the group consisting of glycerol, ethylene glycol, diethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 2-methyl, neopentyl glycol, propylene glycol, triethylene glycol, tetraethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, tetrapropylene glycol, trimethylene glycol, 1,1,1-trimethylolethane, 1,2,3-trimethylolpropane, methylpropylene glycol, pentaerythritol, and polyoxyalkylene polyols comprising monomer repeating units of ethylene oxide, propylene oxide or butylene oxide, and mixtures thereof.

[0082] Embodiment 17. The polymer composition of any of embodiments 11-16, wherein the polyol is selected from the group consisting of 1,3-propylene glycol, 1,4-butanediol, 1,6-hexanediol, methylpropylene glycol, and mixtures thereof.

[0083] Embodiment 18. The polymer composition of any of Embodiments 11-17, wherein the polyol comprises 1,3-propylene glycol.

[0084] Embodiment 19. The polymer composition of any of embodiments 11-18, wherein the dicarboxylic acid or anhydride comprises succinic acid or anhydride and the polyol comprises 1,3-propylene glycol.

[0085] Embodiment 20. The polymer composition of any of embodiments 11-19, wherein the impact-modified polyester has a weight average molecular weight of about 10,000 to about 15,000 Daltons as determined by ASTM D5296-05.

[0086] Embodiment 21. The polymer composition of any one of embodiments 11-20, wherein the polymer composition comprises about 60% to about 85% by weight of the biodegradable polymer and about 5% to about 30% by weight of the impact-modified polyester.

[0087] Embodiment 22. The polymer composition of any of embodiments 11-21, wherein the biodegradable polymer comprises polylactic acid.

[0088] Embodiment 23. The polymer composition of any of embodiments 11-22, wherein the biodegradable polymer comprises at least one polyhydroxyalkanoate.

[0089] Embodiment 24. The polymer composition of embodiment 23, wherein the at least one polyhydroxyalkanoate comprises poly-3-hydroxybutyrate-co-3-hydroxyhexanoate ("P(3HB-co-3HHx)").

[0090] Embodiment 25. The polymer composition of embodiment 24, wherein P(3HB-co-3HHx) comprises about 75% to about 99% by mole of hydroxybutyric acid and about 1% to about 25% by mole of hydroxyhexanoate.

[0091] Embodiment 26. The polymer composition of embodiment 24, wherein P(3HB-co-3HHx) comprises about 93 to about 98 mole percent hydroxybutyric acid and about 2 to about 7 mole percent hydroxyhexanoate.

[0092] Embodiment 27. The polymer composition of embodiment 23, wherein at least one polyhydroxyalkanoate comprises a terpolymer consisting of monomer repeating units of about 75% to about 99.9% by mole of 3-hydroxybutyric acid, about 0.1% to about 25% by mole of 3-hydroxyhexanoate, and about 0.1% to about 25% by mole of a third 3-hydroxyalkanoate having 5 to 12 carbon atoms.

[0093] Embodiment 28. The polymer composition of embodiment 23, wherein the at least one polyhydroxyalkanoate has a weight average molecular weight of about 50,000 Daltons to about 2.5 million Daltons as determined by ASTM D5296-05.

[0094] Embodiment 29. The polymer composition of embodiment 23, wherein the at least one polyhydroxyalkanoate has a weight average molecular weight of about 500,000 Daltons to about 750,000 Daltons as determined by ASTM D5296-05.

[0095] Embodiment 30. The polymer composition of embodiments 11-29, wherein the polymer composition comprises from about 5% to about 25% by weight of polylactic acid and from about 70% to about 90% by weight of at least one polyhydroxyalkanoate.

[0096] Embodiment 31. The polymer composition of embodiments 11-30, further comprising:

[0097] From about 1% to about 10% by weight of at least one plasticizer;

[0098] From about 0.1% to about 5% by weight of at least one nucleating agent; and

[0099] From about 0.1% to about 10% by weight of filler.

[0100] Embodiment 32. The polymer composition of embodiments 11-31, wherein the polymer composition is biodegradable as determined using ASTM standard D5988.

[0101] Embodiment 33. The polymer composition of embodiments 11-32, wherein the polymer composition is home compostable as determined using ASTM standard D6868.

[0102] Embodiment 34. The polymer composition of embodiments 11-33 further comprises about 5% to about 50% by weight of at least one biodegradable polymer selected from the group consisting of polycaprolactone, polyvinyl sebacate, polybutylene succinate, polybutylene succinate-adipate, polybutylene adipate, polyvinyl acetate, and mixtures thereof.

[0103] Embodiment 35. A molded sheet comprising the polymer composition of any of Embodiments 11-34.

[0104] Embodiment 36. A molded article comprising the polymer composition of any one of embodiments 11-34, wherein the molded article is formed by thermoforming, injection molding, or blow molding.

[0105] Embodiment 37. A film comprising the polymer composition of any of embodiments 11-34, wherein the film is a blown film or a cast film.

[0106] Embodiment 38. A fiber comprising the polymer composition of any of embodiments 11-34.

[0107] Example

[0108] The following non-limiting examples illustrate various additional aspects of the invention. Unless otherwise indicated, temperatures are in degrees Celsius and percentages are in weight based on the dry weight of the formulation.

[0109] Example 1

[0110] 800g of isosorbide and 5g of phosphoric acid are charged to a reaction bottle equipped with a nitrogen inlet and vacuum capacity. The reaction temperature is raised to 100°C, and three vacuum cycles are performed by pulling the contents in the reaction bottle to maximum vacuum, and then releasing the vacuum with an inert gas (such as nitrogen). Subsequently, 1279g of succinic acid is charged, and another vacuum cycle is performed. Next, the reactor temperature is raised to a maximum of 220°C, and water is continuously distilled into a receiver. When the precipitation of water slows down, 416g of propylene glycol is charged to the reactor. The temperature is slowly raised to a maximum of 210°C again. Near the end of the reaction, 1g of stannous (II) ethylhexanoate is added, and vacuum is applied. The material is kept until the appropriate molecular weight specification is obtained.

[0111] Example 2

[0112] 416kg of isosorbide and 2.27kg of phosphoric acid are loaded into a 1514L stainless steel reactor equipped with a nitrogen inlet and vacuum capability. The reaction temperature is raised to 100°C, and three vacuum cycles are performed by pulling the contents in the reactor to maximum vacuum and then releasing the vacuum with an inert gas (such as nitrogen). Subsequently, 590kg of succinic acid is loaded and another vacuum cycle is performed. Next, the reactor temperature is raised to a maximum of 220°C, and water is continuously distilled into a receiver. When the precipitation of water slows down, 216kg of propylene glycol is loaded into the reactor. The temperature is slowly raised to a maximum of 210°C again. Near the end of the reaction, 453g of stannous (II) ethylhexanoate is added. The material is kept until the appropriate molecular weight specification is obtained.

[0113] Example 3

[0114] 575g of isosorbide, 888g of partially hydrogenated distilled dimer acid and 5g of phosphoric acid are charged to a reaction flask equipped with a nitrogen inlet and vacuum capacity. The reaction temperature is raised to 100°C, and three vacuum cycles are performed by pulling the contents in the reaction flask to maximum vacuum, and then releasing the vacuum with an inert gas (such as nitrogen). Subsequently, 733g of succinic acid is charged, and a vacuum cycle is performed again. Next, the reactor temperature is raised to a maximum of 220°C, and water is continuously distilled into a receiver. When the precipitation of water slows down, 299g of propylene glycol is charged to the reactor. The temperature is slowly raised to a maximum of 220°C again. Near the end of the reaction, 1g of stannous (II) ethylhexanoate is added, and vacuum is applied. The material is kept until the appropriate molecular weight specification is obtained.

[0115] Example 4

[0116] 2314 g of polyester from Example 2 and 186 g of methyl nadic anhydride were charged to a reaction flask equipped with a nitrogen inlet and vacuum capability. The reactor temperature was raised to a maximum of 220° C., with water being continuously distilled into a receiver. Near the end of the reaction, 0.63 g of stannous (II) ethylhexanoate was added. The material was maintained until the appropriate molecular weight specification was obtained.

[0117] Example 5

[0118] 1124 g of 1,6-hexanediol, 548 g of succinic acid and 827 g of methyl nadic anhydride were charged to a reaction flask equipped with a nitrogen inlet and vacuum capability. Next, the reactor temperature was raised to a maximum of 210°C, and water was continuously distilled into a receiver. Near the end of the reaction, 0.63 g of stannous (II) ethylhexanoate was added. The material was maintained until the appropriate molecular weight specification was obtained.

[0119] Example 6

[0120] 1155 g of 1,6-hexanediol, 563 g of succinic acid and 783 g of nadic anhydride were charged to a reaction flask equipped with a nitrogen inlet and vacuum capability. Next, the reactor temperature was raised to a maximum of 210°C, with water continuously distilled into a receiver. Near the end of the reaction, 0.63 g of tin(II) ethylhexanoate was added. The material was maintained until the appropriate molecular weight specification was obtained.

[0121] Example 7

[0122] 1191 g of 1,6-hexanediol, 871 g of succinic acid and 438 g of methyl nadic anhydride were charged to a reaction flask equipped with a nitrogen inlet and vacuum capability. Next, the reactor temperature was raised to a maximum of 210°C, with water continuously distilled into a receiver. Near the end of the reaction, 0.63 g of stannous (II) ethylhexanoate was added. The material was maintained until the appropriate molecular weight specification was obtained.

[0123] Embodiment 8-20

[0124] In each such example, a polymer composition comprising one of the impact-modified polyesters of Examples 1-7 was prepared. The polymer composition was extruded on a 27 mm twin screw Entek extruder. In Examples 8-15, 19 and 20, the tensile strength and elongation of the extruded material samples were tested using an Instron 34TM-10 according to ATSM D638 (Type I specimen). The impact strength test was conducted using an Instron 9050 tester according to ATSM D256 (Test Method A). In Examples 16-18, the resilience of the extruded material samples was tested using an Instron CEAST 9050 Pendulum Impact System test equipment according to ASTM D4812-19.

[0125] For each example, a control sample was prepared, extruded, and tested similarly to the test sample. In each example, the composition of the control sample was identical to the test sample except that the impact-modified polyester was omitted from the polymer composition.

[0126] Example 8

[0127] In a 27 mm extruder, 2.27 kg of the reaction product of Example 1 was added to 42.5 kg of PHA, 453 g of pentaerythritol and 172 g of Joncryl 4468 and passed through the extruder. The plastic was tested and showed a tensile strength of 26379 kPa (relative to the control 24097 kPa); an elongation of 8.9% (relative to the control 10.6%), and an impact strength of 0.344 J / cm (relative to the control 0.288 J / cm).

[0128] Example 9

[0129] In a 27 mm extruder, 4.53 kg of the reaction product of Example 1 was added to 40 kg of PHA, 453 g of pentaerythritol and 340 g of Joncryl 4468 and passed through the extruder. The plastic was tested and showed a tensile strength of 24242 kPa (relative to 24097 kPa for the control); an elongation of 11.3% (relative to 10.6% for the control), and an impact strength of 0.408 J / cm (relative to 0.288 J / cm for the control).

[0130] Example 10

[0131] In a 27 mm extruder, 4.5 kg of the reaction product of Example 1 was added to 40 kg of PHA, 317 g of Joncryl 4468 and 453 g of pentaerythritol and passed through the extruder. The plastic was tested and showed a tensile strength of 19981 kPa (relative to 27303 kPa for the control); an elongation of 2.2% (relative to 9.3% for the control), and an impact strength of 0.259 J / cm (relative to 0.301 J / cm for the control).

[0132] Embodiment 11

[0133] In a 27 mm extruder, 6.8 kg of the reaction product of Example 1 was added to 37.6 kg of PHA, 498 g of Joncryl 4468 and 453 g of pentaerythritol and passed through the extruder. The plastic was tested and showed a tensile strength of 26745 kPa (relative to 27303 kPa for the control); an elongation of 11.5% (relative to 9.3% for the control), and an impact strength of 0.256 J / cm (relative to 0.301 J / cm for the control).

[0134] Example 12

[0135] In a 27 mm extruder, 4.53 kg of the reaction product of Example 1 was added to 40.6 kg of PHA and 227 kg of boron nitride and passed through the extruder. The plastic was tested and showed a tensile strength of 19960 kPa (relative to 24097 kPa for the control); an elongation of 11.8% (relative to 10.6% for the control), and an impact strength of 0.232 J / cm (relative to 0.288 J / cm for the control).

[0136] Example 13

[0137] In a 27 mm extruder, 2.27 kg of the reaction product of Example 6 was added to 42.9 kg of PHA and 227 g of boron nitride and passed through the extruder. The plastic was tested and showed a tensile strength of 16899 kPa (relative to the control 24097 kPa); an elongation of 15.5% (relative to the control 10.6%), and an impact strength of 0.275 J / cm (relative to the control 0.288 J / cm).

[0138] Embodiment 14

[0139] In a 27 mm extruder, 4.53 kg of the reaction product of Example 6 was added to 40.6 kg of PHA and 227 g of boron nitride and passed through the extruder. The plastic was tested and showed a tensile strength of 12941 kPa (relative to 24097 kPa for the control); an elongation of 16.6% (relative to 10.6% for the control), and an impact strength of 0.324 J / cm (relative to 0.288 J / cm for the control).

[0140] Embodiment 15

[0141] In a 27 mm extruder, 4.53 kg of the reaction product of Example 5 was added to 40.6 kg of PHA and 227 g of boron nitride and passed through the extruder. The plastic was tested and showed a tensile strength of 19167 kPa (relative to the control 24097 kPa); an elongation of 18.4% (relative to the control 10.6%), and an impact strength of 0.277 J / cm (relative to the control 0.288 J / cm).

[0142] Example 16

[0143] In a 27 mm extruder, 2.27 kg of the reaction product of Example 6 was added to 42.87 kg of PHA and 227 g of boron nitride and passed through the extruder. The plastic was tested and showed 66.9 kJ / m 2 The rebound resilience is 14.5 kJ / m 2 .

[0144] Embodiment 17

[0145] In a 27 mm extruder, 4.53 kg of the reaction product of Example 6 was added to 40.6 kg of PHA and 227 g of boron nitride and passed through the extruder. The plastic was tested and showed 67.1 kJ / m 2 The rebound resilience is 14.5 kJ / m 2 .

[0146] Embodiment 18

[0147] In a 27 mm extruder, 4.53 kg of the reaction product of Example 7 was added to 40.6 kg of PHA and 227 g of boron nitride and passed through the extruder. The plastic was tested and showed 39.5 kJ / m 2 The rebound resilience is 14.5 kJ / m 2 .

[0148] Embodiment 19

[0149] In a 27 mm extruder, 4.53 kg of the reaction product of Example 4 was added to 40.6 kg of PHA and 227 g of boron nitride and passed through the extruder. The plastic was tested and showed 11.1 kJ / m 2 The rebound resilience is 2.34 kJ / m 2 .

[0150] Embodiment 20

[0151] In a 27 mm extruder, 1.36 kg of the reaction product of Example 3 was added to 44 kg of PHA and passed through the extruder. The plastic was tested and showed a tensile strength of 1386 kPa, relative to the control 1572 kPa; an elongation of 5.3%, relative to the control 5.6%; and an impact strength of 0.167 J / cm, relative to the control 0.301 J / cm.

[0152] As can be seen from the above, the impact-modified polyesters according to the present invention can provide a variety of mechanical property improvements to bioplastic systems. For example, a four-fold increase in impact strength or an 11% increase in elongation can be achieved without a corresponding loss in tensile strength. Thus, the impact-modified polyesters of the present invention allow the mechanical properties of bioplastic systems to be tailored to specific end-use applications.

[0153] The above description of the preferred embodiments of the present invention is presented for the purpose of illustration and description. It is not intended to be exhaustive or to limit the invention to the precise form disclosed. Obvious modifications or variations are possible in light of the above teachings. The embodiments selected and described are intended to provide the best illustration of the principles of the present invention and its practical application, and thus enable one of ordinary skill in the art to utilize the present invention in various embodiments and with various modifications suitable for the particular use contemplated. All such modifications and variations are within the scope of the present invention as determined by the appended claims when interpreted in accordance with their fair, legal and equally entitled scope.

Claims

1. A polyester comprising: 15 wt % to 40 wt % of monomer repeating units of isosorbide, based on the total weight of the polyester; 25 wt % to 60 wt % of monomer repeating units of dicarboxylic acid or anhydride, based on the total weight of the polyester; and 10 to 20 wt% of monomer repeating units of a polyol, based on the total weight of the polyester, wherein the polyester has a weight average molecular weight of at least 8000 Daltons as determined by ASTM D5296-05; and The dicarboxylic acid or anhydride is selected from the group consisting of (1) succinic acid or succinic anhydride and (2) nadic anhydride, methyl nadic anhydride, C36 dimer acid, or partially hydrogenated C36 dimer acid, and mixtures thereof.

2. The polyester of claim 1, wherein the polyester comprises 25 to 35 weight percent of succinic acid or succinic anhydride, and 10 to 25 weight percent of nadic anhydride, methyl nadic anhydride, C36 dimer acid, or partially hydrogenated C36 dimer acid.

3. The polyester according to claim 1, wherein the polyol is selected from the group consisting of glycerol, ethylene glycol, diethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, propylene glycol, triethylene glycol, tetraethylene glycol, dipropylene glycol, tripropylene glycol, tetrapropylene glycol, trimethylene glycol, 1,1,1-trimethylolethane, 1,2,3-trimethylolpropane, methylpropylene glycol, pentaerythritol, and polyoxyalkylene polyols comprising monomer repeating units of ethylene oxide, propylene oxide or butylene oxide, and mixtures thereof.

4. The polyester according to claim 1, wherein the polyol is selected from the group consisting of 1,3-propylene glycol, 1,4-butylene glycol, 1,6-hexanediol, methylpropylene glycol, and mixtures thereof.

5. The polyester of claim 1, wherein the polyol comprises 1,3-propylene glycol.

6. The polyester according to claim 1, wherein The polyester has a weight average molecular weight of 10,000 to 15,000 Daltons as determined by ASTM D5296-05.

7. A polymer composition comprising: 50 to 95 weight percent of a biodegradable polymer selected from the group consisting of polylactic acid, polyhydroxyalkanoate, and mixtures thereof; 5 to 50 weight percent of an impact-modified polyester, wherein the impact-modified polyester comprises: 15 wt % to 40 wt % of monomer repeating units of isosorbide, based on the total weight of the polyester; 25 wt % to 60 wt % of monomer repeating units of dicarboxylic acid or anhydride, based on the total weight of the polyester; 10 wt % to 20 wt % of the monomer repeating units of the polyol, based on the total weight of the polyester, wherein the polyester has a weight average molecular weight of at least 8000 Daltons as determined by ASTM D5296-05; and The dicarboxylic acid or anhydride is selected from the group consisting of (1) succinic acid or succinic anhydride and (2) nadic anhydride, methyl nadic anhydride, C36 dimer acid, or partially hydrogenated C36 dimer acid, and mixtures thereof.

8. The polymer composition of claim 7, wherein the polyester comprises 25 to 35 weight percent succinic acid or succinic anhydride, and 10 to 25 weight percent nadic anhydride, methyl nadic anhydride, C36 dimer acid, or partially hydrogenated C36 dimer acid.

9. The polymer composition of claim 7, wherein the polyol is selected from the group consisting of glycerol, ethylene glycol, diethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, propylene glycol, triethylene glycol, tetraethylene glycol, dipropylene glycol, tripropylene glycol, tetrapropylene glycol, trimethylene glycol, 1,1,1-trimethylolethane, 1,2,3-trimethylolpropane, methylpropylene glycol, pentaerythritol, and polyoxyalkylene polyols comprising monomer repeating units of ethylene oxide, propylene oxide or butylene oxide, and mixtures thereof.

10. The polymer composition of claim 7, wherein the polyol is selected from the group consisting of 1,3-propylene glycol, 1,4-butanediol, 1,6-hexanediol, methylpropylene glycol, and mixtures thereof.

11. The polymer composition of claim 7, wherein the polyol comprises 1,3-propylene glycol.

12. The polymer composition according to claim 7, wherein The impact-modified polyester has a weight average molecular weight of 10,000 to 15,000 Daltons as determined by ASTM D5296-05.

13. The polymer composition of claim 7, wherein the polymer composition comprises 60 to 85 weight percent of the biodegradable polymer and 5 to 30 weight percent of the impact-modified polyester.

14. The polymer composition of claim 7, wherein the biodegradable polymer comprises polylactic acid.

15. The polymer composition of claim 7, wherein the biodegradable polymer comprises at least one polyhydroxyalkanoate.

16. The polymer composition of claim 15, wherein the at least one polyhydroxyalkanoate comprises poly-3-hydroxybutyrate-co-3-hydroxyhexanoate P (3HB-co-3HHx).

17. The polymer composition of claim 16, wherein the P(3HB-co-3HHx) comprises 75 to 99 mol% of hydroxybutyrate and 1 to 25 mol% of hydroxyhexanoate.

18. The polymer composition of claim 16, wherein the P(3HB-co-3HHx) comprises 93 to 98 mol% of hydroxybutyrate and 2 to 7 mol% of hydroxyhexanoate.

19. The polymer composition of claim 15, wherein the at least one polyhydroxyalkanoate comprises a terpolymer consisting of 75 mol% to 99.9 mol% monomer repeating units of 3-hydroxybutyrate, 0.1 mol% to 25 mol% monomer repeating units of 3-hydroxyhexanoate, and 0.1 mol% to 25 mol% monomer repeating units of a third 3-hydroxyalkanoate having 5 to 12 carbon atoms.

20. The polymer composition according to claim 15, wherein The at least one polyhydroxyalkanoate has a weight average molecular weight of 50,000 Daltons to 2.5 million Daltons as determined by ASTM D5296-05.

21. The polymer composition according to claim 15, wherein The at least one polyhydroxyalkanoate has a weight average molecular weight of 500,000 to 750,000 Daltons as determined by ASTM D5296-05.

22. The polymer composition of claim 7, wherein the polymer composition comprises 5 to 25 wt% of polylactic acid and 70 to 90 wt% of at least one polyhydroxyalkanoate, based on the total weight of the polymer composition.

23. The polymer composition of claim 7, further comprising: 1 to 10 wt. % of at least one plasticizer; 0.1 wt % to 5 wt % of at least one nucleating agent; and 0.1 wt % to 10 wt % filler.

24. The polymer composition of claim 7, wherein the polymer composition is biodegradable as determined using ASTM standard D5988.

25. The polymer composition of claim 7, wherein the polymer composition is home compostable as determined using ASTM standard D6868.

26. The polymer composition of claim 7, further comprising 5 to 50 weight percent of at least one biodegradable polymer selected from the group consisting of polycaprolactone, polyvinyl sebacate, polybutylene succinate, polybutylene succinate-co-adipate, polybutylene adipate, polyvinyl acetate, and mixtures thereof.

27. A molded sheet comprising the polymer composition of claim 7.

28. A molded article comprising the polymer composition of claim 7, wherein the molded article is formed by thermoforming, injection molding, or blow molding.

29. A film comprising the polymer composition of claim 7, wherein the film is a blown film or a cast film.

30. A fiber comprising the polymer composition of claim 7.

Citation Information

Patent Citations

  • Polylactic acid resin and copolymer polyester resin blend, and molded product using same

    CN103946307A