A processing method for homogeneous high-toughness copper-nickel-tin alloy

By adding microalloying elements Nb and/or Y to copper-nickel-tin alloys and employing a single hot and cold deformation processing method, combined with solution treatment, annealing, and aging heat treatment, the problems of high cost and uneven mechanical properties of copper-nickel-tin alloys are solved, achieving high toughness and uniform microstructure, making them suitable for the aerospace field.

CN117926152BActive Publication Date: 2026-11-10CENT SOUTH UNIV +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410021348.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-05
Publication Date
2026-11-10
Estimated Expiration
2044-01-05

AI Technical Summary

Technical Problem

Existing technologies for preparing copper-nickel-tin alloys are costly, have uneven mechanical properties, and lack sufficient toughness, making it difficult to meet the application requirements of the aerospace field.

Method used

A homogeneous, high-toughness copper-nickel-tin alloy was prepared by using microalloying elements Nb and/or Y, through a process involving one hot deformation and one cold deformation, combined with solution treatment, annealing, and aging heat treatment.

Benefits of technology

It improves the microstructure uniformity and toughness of copper-nickel-tin alloys, reduces processing costs, and increases the tensile strength, yield strength, and elongation of the material. It is suitable for copper-nickel-tin alloys of different sizes and solves the cracking problem caused by differences in internal and external properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117926152B_ABST
    Figure CN117926152B_ABST
Patent Text Reader

Abstract

A processing method for a homogeneous, high-toughness copper-nickel-tin alloy includes the following steps: (1) adding microalloying element additives, including Nb and / or Y, to the copper-nickel-tin alloy raw material and performing a solution treatment; (2) subjecting the copper-nickel-tin alloy billet to a hot deformation treatment at a temperature of 700℃~900℃; (3) subjecting the copper-nickel-tin alloy billet to a cold deformation treatment at a temperature of 20℃~50℃; (4) subjecting the copper-nickel-tin alloy billet to annealing and aging heat treatment in sequence to obtain a homogeneous, high-toughness copper-nickel-tin alloy. This method involves fewer deformation and heat treatment processes, reducing the amount of deformation per process. It avoids the inherent defect of copper-nickel-tin alloys being difficult to deform multiple times and achieves the requirements of uniform microstructure and high strength and toughness in copper-nickel-tin alloys.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of alloy processing, and particularly relates to a processing method for copper-nickel-tin alloys. Background Technology

[0002] Copper-nickel-tin alloys are widely used in national defense, building structures, and rail transportation due to their chemical stability, good corrosion resistance, and excellent mechanical properties. However, in aerospace applications such as aircraft landing gear bearings / bushings, copper-nickel-tin alloys are required to have uniform mechanical properties and high toughness, which current technologies cannot meet.

[0003] Refining the microstructure and reducing defects are among the most effective ways to improve the strength and toughness of copper alloys. Patent document CN106498322A discloses a static magnetic field deep cryogenic treatment method to improve the strength and toughness of copper or copper alloys. This method improves the toughness of copper alloys by coupling static magnetic field and deep cryogenic field. However, this method is only applicable to small-sized samples and is difficult to implement in industrial applications. Patent document CN110195170A discloses a preparation method to improve the strength and toughness of Cu-Ni-Si alloys. This production process includes: semi-continuous casting ingot → ingot heating → hot rolling → first solution treatment → milling → first cold rolling → trimming → annealing → second cold rolling → second solution treatment → third cold rolling → third solution treatment → fourth cold rolling → cleaning → aging heat treatment → cleaning → tension leveling → slitting. This process is extremely costly and has low processing efficiency.

[0004] Therefore, there is an urgent need for a new, lower-cost material processing method to improve the strength and toughness of copper-nickel-tin alloys and to solve the problem of uneven microstructure and mechanical properties, so as to meet the application requirements of copper-nickel-tin alloys in the aerospace industry. Summary of the Invention

[0005] The technical problem to be solved by the present invention is that the existing methods for preparing copper-nickel-tin alloys are costly, have uneven mechanical properties, and lack product toughness. To overcome the shortcomings and defects mentioned in the background art, the present invention provides a processing method for homogeneous and high-toughness copper-nickel-tin alloys.

[0006] To solve the above-mentioned technical problems, the technical solution proposed by this invention is as follows:

[0007] A method for processing a homogeneous, high-toughness copper-nickel-tin alloy includes the following steps:

[0008] (1) Add microalloying element additives to copper-nickel-tin alloy raw materials, wherein the microalloying elements include Nb and / or Y, to prepare copper-nickel-tin alloy billets, and perform solid solution treatment on the copper-nickel-tin alloy billets;

[0009] (2) Heat the copper-nickel-tin alloy billet after solution treatment in step (1) to 800℃~900℃ for hot deformation treatment.

[0010] (3) The copper-nickel-tin alloy billet after the hot deformation treatment in step (2) is subjected to cold deformation treatment; the temperature of the cold deformation treatment is 20℃~50℃;

[0011] (4) The copper-nickel-tin alloy billet after the secondary deformation treatment in step (3) is subjected to annealing and aging heat treatment in sequence to obtain a homogeneous high-toughness copper-nickel-tin alloy.

[0012] This patent employs a two-stage deformation process, consisting of a hot deformation followed by a cold deformation. This not only avoids the disadvantage that alloy materials cannot withstand large deformations, but also induces the recrystallization process during subsequent aging heat treatment. Recrystallization refines the grains, resulting in increased strength and toughness.

[0013] Preferably, the additive includes elemental Nb and / or Y, and the mass ratio of the microalloying element in the microalloying element additive to the copper-nickel-tin alloy billet is 0.05% to 1.00%.

[0014] Microalloying element additives enter the molten state of copper-nickel-tin alloy raw materials in elemental form, forming Ni3Nb and / or Ni3Y intermetallic compounds with Ni in the copper-nickel-tin alloy raw materials. After atomization and powdering, copper-nickel-tin metal powder containing microalloying elements is obtained, and then pressed and hot isostatically sintered to obtain copper-nickel-tin alloy billets.

[0015] The microalloying elements can form intermetallic compounds in copper, nickel, and tin, which have a pinning effect on grain growth and can ensure uniform crystalline structure and grain size during recrystallization.

[0016] During recrystallization, the timing and rate of grain recrystallization vary, which, if left untreated, can lead to uneven grain size and distribution. The pinning effect of microalloying elements refers to the phenomenon where, after grains grow to a certain size (around 8-10 micrometers), they are pinned by intermetallic compounds formed by the microalloying elements, thus maintaining their growth at that size. Simultaneously, grains that have not reached this size will continue to grow unaffected, ultimately resulting in all grains having similar sizes and achieving homogeneity. The pinning effect also prevents excessively large grains, ensuring grain refinement and making a significant contribution to the strength and toughness of the alloy.

[0017] Preferably, in step (2), the deformation amount of the hot deformation treatment is 10% to 20%, and the uniform deformation time is no more than 60s; in step (3), the deformation amount of the cold deformation treatment is 10% to 40%, and the uniform deformation time is 80s to 150s.

[0018] During cold deformation processing, copper-nickel-tin alloys, especially bars, rapidly achieve work hardening on the surface, while the core remains undeformed. This results in a significant difference in deformation between the inner and outer layers, leading to inhomogeneous microstructures and substantial performance differences between the core and edges. In practical applications, this mismatch in microstructures between the inner and outer layers easily causes cracking. This application addresses this issue by first employing hot deformation to maintain the billet at a high temperature during deformation, placing it in a solution state. The hot-deformed billet exhibits defects such as deformation twins. During cold deformation, the pinning effect of intermetallic compounds formed by added microalloying elements ensures that the grains in both the core and edges maintain a fixed size during recrystallization, resulting in a more uniform microstructure that meets the requirements of homogeneity and high toughness. Furthermore, because it involves two deformation processes, controlling the deformation amount slightly each time can induce subsequent recrystallization, thus avoiding the problem of poor deformability in copper-nickel-tin alloys, especially copper-nickel-tin bars.

[0019] Preferably, the starting deformation temperature is the temperature at which the deformation equipment contacts the alloy to begin the deformation process, the ending deformation temperature is the temperature at which the deformation equipment leaves the alloy to end the deformation process, and the uniform deformation means that the deformation equipment moves at a constant speed relative to the alloy during the deformation process.

[0020] Preferably, in step (2), the heat deformation treatment is followed by heat preservation for 20 min to 30 min; after heat preservation, cooling is performed at a rate greater than 20℃ / s.

[0021] Preferably, in step (1), the solution treatment specifically includes: heating the copper-nickel-tin alloy raw material to 800℃~900℃ at a heating rate of 10℃ / min~20℃ / min, holding it at that temperature for 150min~210min, and then cooling it after the holding period. More preferably, the cooling is water quenching cooling.

[0022] Preferably, in step (4), the annealing process specifically includes: holding at 700℃~900℃ for 20min~60min, and then cooling at a cooling rate greater than 20℃ / s.

[0023] Preferably, in step (4), the aging heat treatment specifically includes: holding at 350℃~450℃ for 1h~4h to obtain a homogeneous high-toughness copper-nickel-tin alloy.

[0024] Preferably, the performance data of the homogeneous high-toughness copper-nickel-tin alloy include: Rockwell hardness ≥30, tensile strength ≥1000MPa, yield strength ≥850MPa, and elongation ≥10%.

[0025] The preferred homogeneous high-toughness copper-nickel-tin alloy has the following mass fractions in the overall alloy: nickel 9%–21%, tin 6%–10%, microalloying elements 0.05%–1.0%, impurities 0%–0.15%, and the remaining component is copper. The grain size of the homogeneous high-toughness copper-nickel-tin alloy is 5–15 μm, and more preferably, the grain size is 8–10 μm.

[0026] Impurities are those that may be introduced during the preparation process due to minor oxidation of the powder surface or contamination by other carbide oxides, which may have a negative impact on the performance of the sample.

[0027] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0028] (1) This invention only involves heat treatment and deformation processing. The billet undergoes only one solution heat treatment, one annealing treatment, and one low-temperature aging heat treatment. The process steps are few, resulting in high industrial production efficiency. This scheme involves fewer deformation and heat treatment processes and reduces the amount of deformation per process. It avoids the inherent defect of copper-nickel-tin alloys being difficult to deform multiple times, while also meeting the requirements of uniform microstructure and high strength and toughness of copper-nickel-tin alloys. Furthermore, it greatly reduces energy consumption and has environmental benefits.

[0029] (2) The present invention adopts a deformation processing technology of one hot deformation followed by one cold deformation. The hot deformation followed by the cold deformation ensures that the first deformation can also maintain its solid solution state, minimizes the surface work hardening caused by deformation, and has low requirements for deformation processing equipment and low operation difficulty. It is applicable to copper-nickel-tin alloys of different sizes, with a wide range of applications and good engineering application prospects.

[0030] (3) The homogeneous high-toughness copper-nickel-tin alloy obtained by this invention improves the uniformity of the material's microstructure and its toughness while ensuring high strength and other properties. When manufacturing large products, the homogeneous alloy exhibits consistent internal and external properties, making it suitable for a wide range of applications. It solves the problem of cracking during application caused by uneven microstructure distribution and significant differences in surface and internal properties after multi-stage deformation of the alloy material. The homogeneous high-toughness copper-nickel-tin alloy product obtained by this invention achieves advanced levels in the industry in terms of tensile strength, yield strength, and elongation. Attached Figure Description

[0031] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0032] Figure 1This is a schematic diagram of the metallographic structure of the homogeneous high-toughness copper-nickel-tin alloy (edge ​​and core) of Example 1;

[0033] Figure 2 , 3 This is a SEM image of the edge of the homogeneous, high-toughness copper-nickel-tin alloy from Example 1; Detailed Implementation

[0034] To facilitate understanding of the present invention, the present invention will be described more fully and in detail below with reference to the accompanying drawings and preferred embodiments, but the scope of protection of the present invention is not limited to the following specific embodiments.

[0035] Unless otherwise defined, all technical terms used herein have the same meaning as commonly understood by those skilled in the art. The technical terms used herein are for the purpose of describing particular embodiments only and are not intended to limit the scope of the invention.

[0036] Unless otherwise specified, all raw materials, reagents, instruments and equipment used in this invention can be purchased from the market or prepared by existing methods.

[0037] Example 1:

[0038] The sintering raw material was Cu-15Ni-8Sn alloy rods sintered by powder metallurgy hot isostatic pressing. Table 1 shows the composition analysis of the Cu-15Ni-8Sn alloy rods:

[0039] Table 1. Composition of Cu-15Ni-8Sn alloy

[0040]

[0041] This embodiment provides a processing method for a homogeneous, high-toughness copper-nickel-tin alloy, including the following steps:

[0042] 1) Melt the original Cu-15Ni-8Sn metal raw material, add the microalloying element additive Nb, and let Nb enter the melt in elemental form. The amount of Nb added is 0.3wt% of the Cu-15Ni-8Sn metal raw material. After atomization powdering (Nb is uniformly distributed in the Cu-15Ni-8Sn alloy metal powder), pressing, and hot isostatic pressing sintering, Cu-15Ni-8Sn alloy rods (L=500mm, Φ=60mm) are obtained. Solution treatment is performed, and the temperature is raised to 850℃ in the furnace at a heating rate of 10℃ / min and held for 180min.

[0043] 2) After the Cu-15Ni-8Sn alloy bar has been held at the temperature for the required time after solution treatment, it is quenched in water and then subjected to hot deformation. The initial deformation temperature when the deformation equipment comes into contact with the alloy is 800℃, and the final deformation temperature when the deformation equipment leaves the alloy is 700℃. The deformation amount is 10% (Φ=57mm). The deformation equipment moves at a constant speed relative to the alloy billet during the deformation process, and the uniform deformation time is 60s. Then, it is returned to the furnace and held at 800℃ for 20min. After the holding time is completed, it is rapidly cooled with a cooling rate >20℃ / s.

[0044] 3) The Cu-15Ni-8Sn alloy bar after hot deformation treatment was subjected to cold deformation treatment at room temperature of 22-25℃, with a re-deformation amount of 14% (Φ=53mm), a uniform deformation time of 80s, and a cumulative deformation amount of 22% after the two deformations.

[0045] 4) Anneal the cold-deformed Cu-15Ni-8Sn alloy bars by holding them in a muffle furnace at 850℃ for 20 minutes, followed by rapid cooling at a rate >20℃ / s.

[0046] 5) The annealed Cu-15Ni-8Sn alloy bars were subjected to aging heat treatment in a muffle furnace at an aging temperature of 400℃ for 2 hours. After the aging time was reached, they were cooled by water quenching. The treatment was completed to obtain a homogeneous high-toughness copper-nickel-tin alloy.

[0047] Figure 1 Images showing the metallographic structure (edge ​​and core) of the homogeneous, high-toughness copper-nickel-tin alloy processed in this embodiment. Figure 2 , 3 This is a SEM image of the edge of the homogeneous, high-toughness copper-nickel-tin alloy from Example 1;

[0048] As can be seen from the figure, the copper-nickel-tin alloy processed by the method in this embodiment has a uniform microstructure, very few defects, and refined grains with a grain size range of 5-15μm, most of which are distributed around 8-10μm, thus possessing strong and tough microstructure.

[0049] Comparative Example 1:

[0050] The raw materials are the same as in Example 1, and the preparation steps are as follows:

[0051] 1) The original Cu-15Ni-8Sn alloy bar (L=500mm, Φ=60mm) was solution treated, water quenched and cooled, and then heated to 850℃ in the furnace at a heating rate of 10℃ / min and held for 180min.

[0052] 2) Aging heat treatment: Aging heat treatment is carried out in a muffle furnace at a temperature of 400℃ for 2 hours. After the aging time is reached, water quenching is performed to cool the furnace and the treatment is completed.

[0053] Comparative Example 2:

[0054] The raw materials are the same as in Example 1, and the preparation steps are as follows:

[0055] 1) The original Cu-15Ni-8Sn alloy bar (L=500mm, Φ=60mm) was solution treated, water quenched and cooled, and then heated to 850℃ in the furnace at a heating rate of 10℃ / min and held for 180min.

[0056] 2) After the Cu-15Ni-8Sn alloy bar has been held at the solution-treated temperature for the required time, hot deformation is immediately performed. The starting temperature for deformation is 800℃, the ending temperature is 700℃, the deformation amount is 10% (Φ=57mm), the uniform deformation time is 60s, and then it is returned to the furnace to be held at 800℃ for 20min. After the holding time is completed, it is rapidly cooled with a cooling rate >20℃ / s.

[0057] The Cu-15Ni-8Sn alloy bars after hot deformation were annealed and held in a muffle furnace at 850℃ for 20 min. After holding, they were rapidly cooled at a rate >20℃ / s.

[0058] 3) Aging heat treatment: Aging is carried out in a muffle furnace at an aging temperature of 400℃ for 2 hours. After the aging time is reached, water quenching is performed to cool the furnace and the treatment is completed.

[0059] The core and edge portions of the samples from Example 1 and Comparative Examples 1 and 2 were machined into 26mm × 8mm × 2mm plate-shaped tensile specimens using wire cutting. Alloy performance was then tested using the test scheme described in the national standard GB / T 228.1-2021. The parameters and results are shown in Table 2.

[0060] Table 2. Test Results of Cu-15Ni-8Sn Alloy

[0061]

[0062] Note: The uniformity value represents "core data / edge data", and the closer the value is to 1, the better the uniformity.

Claims

1. A processing method for a homogeneous, high-toughness copper-nickel-tin alloy, characterized in that, Includes the following steps: (1) Add microalloying element additives to copper-nickel-tin alloy raw materials, wherein the microalloying elements include Nb and / or Y, to prepare copper-nickel-tin alloy billets, and perform solid solution treatment on the copper-nickel-tin alloy billets; wherein the microalloying element additives include elemental Nb and / or Y, and the mass ratio of the microalloying element in the microalloying element additives to the copper-nickel-tin alloy billets is 0.05% to 1.00%; the solid solution treatment specifically includes: heating the copper-nickel-tin alloy raw materials to 800℃ to 900℃ at a heating rate of 10℃ / min to 20℃ / min, holding the temperature for 150min to 210min, and cooling the materials after the holding period; (2) The copper-nickel-tin alloy billet after solution treatment in step (1) is subjected to hot deformation treatment. The temperature of the hot deformation treatment is 700℃~900℃; the starting temperature of the hot deformation treatment is 800~900℃, the ending temperature is 700~800℃, the deformation amount is 10%~20%, and the uniform deformation time is no more than 60s. (3) The copper-nickel-tin alloy billet after the hot deformation treatment in step (2) is subjected to cold deformation treatment. The temperature of the cold deformation treatment is 20℃~50℃; the deformation amount of the cold deformation treatment is 10%~40%; and the uniform deformation time is 80s~150s. (4) The copper-nickel-tin alloy billet after the secondary deformation treatment in step (3) is subjected to annealing and aging heat treatment in sequence to obtain a homogeneous high-toughness copper-nickel-tin alloy; the annealing treatment specifically includes: holding at 700℃~900℃ for 20min~60min and cooling at a cooling rate greater than 20℃ / s; the aging heat treatment specifically includes: holding at 350℃~450℃ for 1h~4h; The mass fraction of each element in the homogeneous high-toughness copper-nickel-tin alloy is as follows: nickel 9%–21%, tin 6%–10%, microalloying elements 0.05%–1.0%, impurities 0%–0.15%, and the remaining component is copper. The grain size of the homogeneous high-toughness copper-nickel-tin alloy is 5–15 μm.

2. The processing method as described in claim 1, characterized in that, The starting deformation temperature is the temperature at which the deformation equipment contacts the alloy and begins the deformation process; the ending deformation temperature is the temperature at which the deformation equipment leaves the alloy and ends the deformation process; and the uniform deformation means that the deformation equipment moves at a constant speed relative to the alloy billet during the deformation process, with the moving speed being 1 mm / s to 10 mm / s.

3. The processing method as described in claim 1, characterized in that, In step (2), the heat deformation treatment is followed by heat preservation for 20 min to 30 min; after heat preservation, cooling is performed at a rate greater than 20℃ / s.

4. The processing method as described in claim 1, characterized in that, The performance data of the homogeneous high-toughness copper-nickel-tin alloy include: Rockwell hardness ≥30, tensile strength ≥1000MPa, yield strength ≥850MPa, and elongation ≥10%.

Citation Information

Patent Citations

  • Static magnetic field cryogenic treatment method for improving strength and toughness of copper or copper alloy

    CN106498322A

  • Preparing method capable of improving strength and toughness of Cu-Ni-Si alloy

    CN110195170A

  • Copper-nickel-tin alloy with high toughness

    CN105143480A

  • Copper-nickel-tin alloy with high toughness

    CN107881362A