Preparation method of barium ferrite / (aniline-co-6-(2-aminophenoxy)hexane-1-ol) copolymer conductive polymer nanocomposite microwave absorbing medium
By introducing 6-(2-aminophenoxy)hexane-1-ol and aniline monomers into the surface of hexagonal barium ferrite and forming a micro-protrusion/short rod-shaped copolymer conductive polymer layer, the problem of narrow electromagnetic wave absorption bandwidth of hexagonal barium ferrite is solved, and a wide-band electromagnetic wave absorption effect is achieved.
Patent Information
- Application Number
- CN202410220156.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-28
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-02-28
AI Technical Summary
Existing hexagonal barium ferrites have a high electromagnetic wave absorption frequency band and a narrow bandwidth, making it difficult to effectively extend the transmission and attenuation path of electromagnetic waves.
By introducing 6-(2-aminophenoxy)hexane-1-ol into the carboxylated Ba1-xLaxFe12O19 surface and polymerizing it in situ with aniline monomers, a micro-protrusion/short rod-shaped copolymer conductive polymer layer is formed, enriching the surface polyaniline morphology.
It extends the dissipation path of electromagnetic waves, improves the absorption performance of electromagnetic waves, and realizes wideband electromagnetic wave absorption.
Smart Images

Figure CN117946619B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of microwave absorbing materials, specifically relating to a method for preparing nanoparticles that improve the microwave absorption performance of functionalized lanthanum-doped barium ferrite by coating it with a (aniline-co-6-(2-aminophenoxy)hexane-1-ol) copolymer conductive polymer. Background Technology
[0002] M-type hexagonal barium ferrite (BaM) with permanent magnet properties exhibits good microwave absorption characteristics and is often used as a magnetic loss medium for electromagnetic wave absorption. However, due to its high ferromagnetic resonance frequency band, hexagonal barium ferrite has a high absorption frequency band and a narrow bandwidth. Therefore, it is necessary to composite it with ceramic-based materials, carbon-based materials, conductive polymers, etc. Conductive polymers have been widely studied due to their good conductivity, low cost, and good environmental stability. Composites of BaM with conductive polymers can effectively integrate magnetic and electrical losses, which is an effective method to improve the electromagnetic wave absorption performance of barium ferrite.
[0003] In recent years, many studies have focused on the morphology design of polyaniline on ferrite surfaces. The morphology of conductive polymers on ferrite surfaces significantly affects the scattering effect of electromagnetic waves. The presence of conductive polymers with morphologies resembling micro-protrusions, micro-cones, or rods can extend the transmission and attenuation paths of electromagnetic waves, effectively improving electromagnetic wave absorption. Studies have shown that rare-earth doping can increase the surface activity of hexagonal ferrites, inducing the growth of polyaniline with a micro-protrusion morphology. Furthermore, due to the presence of hydroxyl groups on the surface of hexagonal barium ferrites, oleic acid can be used as a surfactant to modify the surface of nano-hexagonal ferrites through esterification, resulting in a short rod-like structure for the surface polyaniline. Both methods can effectively alter the morphology of polyaniline on hexagonal barium ferrite surfaces, thereby significantly improving the electromagnetic wave absorption performance of the composite material.
[0004] This invention is based on rare earth doping and surface carboxylation of BaM, by partially replacing the aniline monomer with 6-(2-aminophenoxy)hexane-1-ol in the carboxylation of BaM. 1-x La x Fe 12 O 19 In-situ polymerization is performed on the surface to form a copolymer conductive polymer layer. This results in the conductive polymer exhibiting a micro-protrusion / short rod-like morphology, which can effectively extend the dissipation path of electromagnetic waves and improve their dissipation capability. Summary of the Invention
[0005] The technical problem to be solved by the present invention is to provide a method for enabling 6-(2-aminophenoxy)hexane-1-ol to successfully participate in in-situ polymerization by forming a micro-protrusion / rod-like and loosely porous surface polyaniline layer on the surface of lanthanum carboxylated barium ferrite.
[0006] This invention is achieved through the following technical solution: A method for preparing a barium ferrite / (aniline-co-6-(2-aminophenoxy)hexane-1-ol) copolymer conductive polymer nanocomposite microwave absorbing medium involves introducing 6-(2-aminophenoxy)hexane-1-ol as a second monomer, and co-treating it with the aniline monomer in a carboxylated Ba... 1-x La x Fe 12 O 19 In-situ polymerization is performed on the surface to enrich the morphology of the polyaniline, including the following steps: (1) Prepare hydrochloric acid solution; (2) Carboxylated Ba 1-x La x Fe 12 O 19 Dispersed in hydrochloric acid solution, the mixture was processed in a cell disruptor to obtain suspension I; (3) Add aniline monomer and 6-(2-aminophenoxy)hexane-1-ol to suspension I, and treat with a cell disruptor to obtain suspension II; (4) Prepare an ammonium persulfate hydrochloric acid solution as an initiator; (5) After transferring suspension II into a low-temperature water bath and stirring and pre-cooling for a period of time, slowly add the prepared initiator dropwise and react for a period of time to obtain suspension III; (6) The suspension III was centrifuged to obtain the precipitate, which was then washed by centrifugation with an alcohol-water solution. The resulting product was dried, ground, and sieved to finally obtain carboxylated Ba. 1-x La x Fe 12 O 19 / (aniline-co-6-(2-aminophenoxy)hexane-1-ol) copolymer conductive polymer nanocomposite microwave absorbing medium Where x = 0.05~0.20, in step (3) carboxylation of Ba 1-x La x Fe 12 O 19 The mass ratio of the copolymer to the comonomer is 10:1 to 10:3.
[0007] The concentration of hydrochloric acid solution in step (1) is 1 mol / L.
[0008] In step (2), Ba 1-x La x Fe 12 O 19 The preparation method is as follows: A mixed metal salt solution of ferric nitrate, barium nitrate, and lanthanum nitrate was prepared with a molar ratio of 12:(1-x):x, so that the iron ion concentration was 0.5 mol / L. The amount of sodium hydroxide used is 3n (Fe 3+ )*120%, sodium carbonate dosage is (n(Ba 2+ )+n(La 3+ Prepare a mixed precipitant solution by multiplying the concentration of sodium hydroxide by 150% to achieve a sodium hydroxide concentration of 5 mol / L. The prepared metal salt solution was added to the mixed precipitant solution, stirred for 2 hours, and then filtered to obtain the precursor precipitate. The precursor, sodium chloride, and potassium chloride were mixed in a 1:1:1 mass ratio, ball-milled at 400 rpm for 4 hours, calcined at 800℃ for 2 hours, and then washed to obtain Ba. 1-x La x Fe 12 O 19 Nanoparticles.
[0009] In step (2), carboxylation of Ba 1-x La x Fe 12 O 19 The preparation method is as follows: Will Ba 1-x La x Fe 12 O 19 Nanoparticles and oleic acid were dispersed in deionized water at a mass ratio of 1:1 and reacted at 70°C for 1 h. After washing away excess oleic acid by centrifugation with ethanol, the nanoparticles were redispersed in an ethanol solution. Hydrogen peroxide was added at a molar ratio of n(OA):n(H2O2)=1:2 and reacted for 8 h to obtain the carboxylated product.
[0010] The preparation method of 6-(2-aminophenoxy)hexane-1-ol in step (3) is as follows: 5g of 2-aminophenol was dissolved in 100mL of dichloromethane as solution 1, and di-tert-butyl ester solution was added to 50mL of dichloromethane as solution 2. Solution 2 was slowly added dropwise to solution 1. After the addition was completed, the mixture was stirred at 23℃ for 22h. Then, the solvent was removed under negative pressure and the mixture was ground with glacial pentane to obtain product 1. 9.58 g of product 1 was dissolved in 100 mL of DMF solution, and 9.5 g of potassium carbonate and 8.7 g of hexanol bromide were added. The mixture was stirred at 23 °C for 17 h. Subsequently, the reaction mixture was filtered and the filtrate was concentrated under negative pressure. The residue was dissolved in 100 mL of LEtoAc solution, washed with water and brine, dried on MgSO4, and the solvent was removed under negative pressure. The primary product was purified by column chromatography to obtain product 2. 1.39 g of product 2 was dissolved in 6 mL of dichloromethane. A mixed solution of 2.8 mL of trifluoroacetic acid and 2.8 mL of dichloromethane was added dropwise. The mixture was stirred at 23 °C for 45 min. The solvent was removed under negative pressure. 50 mL of 1 mol / L NaOH solution was added. The aqueous phase was extracted with Et2O. The solution was then dried on MgSO4 and the solvent was removed under negative pressure. The final product, 6-(2-aminophenoxy)hexane-1-ol, was obtained by column chromatography.
[0011] In step (3), the molar ratio of aniline monomer to 6-(2-aminophenoxy)hexane-1-ol is 9:1.
[0012] In step (4), the molar ratio of the copolymer monomer to ammonium persulfate is 1:1.2, and the concentration of the prepared ammonium persulfate hydrochloric acid solution is 0.5 mol / L.
[0013] In step (5), the initiator is added at a rate of 0.2 to 0.4 mL / min, the reaction temperature is 0°C, and the reaction time is 20 h.
[0014] Compared with the prior art, the beneficial effects of the present invention are: This invention utilizes the aniline structure to modify the rare earth doping and surface functionalization of ferrites, forming a matching relationship of active sites, thereby more effectively inducing the diversity of polymer morphology on the ferrite surface, making the surface copolymer exhibit a convex rod shape, and improving the electromagnetic wave absorption performance of the material. This structure can effectively extend the dissipation path of electromagnetic waves and improve the electromagnetic wave dissipation capability. This invention provides a new technical means for the morphology of conductive polymers on ferrite surfaces. Attached Figure Description
[0015] Figure 1 The (aniline-co-6-(2-aminophenoxy)hexane-1-ol) copolymer conductive polymer synthesized in Example 1 is coated with carboxylated Ba 0.95 La 0.05 Fe 12 O 19 Transmission electron microscopy image of nanoparticles; Figure 2 The (aniline-co-6-(2-aminophenoxy)hexane-1-ol) copolymer conductive polymer in Example 1 is coated with carboxylated Ba 0.95 La 0.05 Fe 12 O 19 Reflection loss diagram of nanoparticles; Figure 3 The (aniline-co-6-(2-aminophenoxy)hexane-1-ol) copolymer conductive polymer in Example 1 is coated with carboxylated Ba 0.95 La 0.05 Fe12 O 19 Contour plot of nanoparticles; Figure 4 The (aniline-co-6-(2-aminophenoxy)hexane-1-ol) copolymer conductive polymer coated with carboxylated Ba in Example 2 is used. 0.90 La 0.10 Fe 12 O 19 Transmission electron microscopy image of nanoparticles; Figure 5 The (aniline-co-6-(2-aminophenoxy)hexane-1-ol) copolymer conductive polymer in Example 2 is coated with carboxylated Ba 0.90 La 0.10 Fe 12 O 19 Reflection loss diagram of nanoparticles; Figure 6 The (aniline-co-6-(2-aminophenoxy)hexane-1-ol) copolymer conductive polymer in Example 2 is coated with carboxylated Ba 0.90 La 0.10 Fe 12 O 19 Contour plot of nanoparticles. Detailed Implementation
[0016] The present invention will be further described below with reference to the accompanying drawings: Unless otherwise specified, the experimental methods used in the following examples are conventional methods. Unless otherwise specified, the experimental materials used in the following examples were all purchased from commercial sources. Example 1
[0017] Prepare a 1 mol / L hydrochloric acid solution; weigh 1.6 g of carboxylated Ba. 0.95 La 0.05 Fe 12 O 19 Transfer the powder to a beaker, add 80 mL of prepared hydrochloric acid solution to the beaker, and then add the carboxylated Ba... 0.95 La 0.05 Fe 12 O 19 The powder was dispersed in hydrochloric acid solution and then processed in a cell disruptor for 30 minutes to obtain suspension I; Add 0.2899 g of aniline monomer and 0.0725 g of 6-(2-aminophenoxy)hexane-1-ol to suspension I, and then treat with a cell disruptor for 30 min to obtain suspension II; 0.9410 g of ammonium persulfate was added to 8.2 mL of hydrochloric acid solution and ultrasonically dispersed and dissolved to obtain a 0.5 mol / L ammonium persulfate hydrochloric acid solution. Suspension II was transferred to a low-temperature water bath and pre-cooled at 0°C with stirring at 400 rpm for 30 min. A 0.5 mol / L ammonium persulfate hydrochloric acid solution was added to the suspension using a peristaltic pump at a flow rate of 0.2 mL / min. After the addition was completed, the reaction was allowed to proceed for 20 h. The solution was then washed multiple times by centrifugation with anhydrous ethanol:water = 1:1 until the supernatant was free of dark green color. After drying, the final product was obtained.
[0018] The (aniline-co-6-(2-aminophenoxy)hexane-1-ol) copolymer conductive polymer prepared by this method is coated with carboxylated Ba 0.95 La 0.05 Fe 12 O 19 Nanoparticles were successfully prepared.
[0019] Transmission electron microscopy images show that the prepared powder surface is uniformly coated with copolymers, exhibiting a small number of microprotrusions and rod-like structures (such as...). Figure 1 As shown in the figure). From its reflection loss diagram and two-dimensional reflection loss diagram, it can be seen that the fabrication of a highly efficient electromagnetic wave absorbing material has been achieved (e.g., Figure 2 and Figure 3 (As shown). Example 2
[0020] Prepare a 1 mol / L hydrochloric acid solution; weigh 1.6 g of carboxylated Ba. 0.90 La 0.10 Fe 12 O 19 Transfer the powder to a beaker, add 80 mL of prepared hydrochloric acid solution to the beaker, and then add the carboxylated Ba... 0.90 La 0.10 Fe 12 O 19 The powder was dispersed in hydrochloric acid solution and then processed in a cell disruptor for 30 minutes to obtain suspension I; Add 0.2899 g of aniline monomer and 0.0725 g of 6-(2-aminophenoxy)hexane-1-ol to suspension I, and then treat with a cell disruptor for 30 min to obtain suspension II; 0.9410 g of ammonium persulfate was added to 8.2 mL of hydrochloric acid solution and ultrasonically dispersed and dissolved to obtain a 0.5 mol / L ammonium persulfate hydrochloric acid solution. Suspension II was transferred to a low-temperature water bath and pre-cooled at 0°C with stirring at 400 rpm for 30 min. A 0.5 mol / L ammonium persulfate hydrochloric acid solution was added to the suspension using a peristaltic pump at a flow rate of 0.2 mL / min. After the addition was completed, the reaction was allowed to proceed for 20 h. The solution was then washed multiple times by centrifugation with anhydrous ethanol:water = 1:1 until the supernatant was free of dark green color. After drying, the final product was obtained.
[0021] The (aniline-co-6-(2-aminophenoxy)hexane-1-ol) copolymer conductive polymer prepared by this method is coated with carboxylated Ba 0.90 La 0.10 Fe 12 O 19 Nanoparticles were successfully prepared.
[0022] Transmission electron microscopy images show that the morphology of the prepared powder surface copolymer exhibits a loose porous structure and a convex structure (such as...). Figure 4 As shown in the figure). From its reflection loss diagram and two-dimensional reflection loss diagram, it can be seen that the fabrication of electromagnetic wave absorbing materials with strong absorption, thin thickness, and wide bandwidth has been achieved (e.g., Figure 5 and Figure 6 (As shown).
[0023] In summary, these are merely preferred embodiments of the present invention and are not intended to limit the scope of the invention. All equivalent variations and modifications made in accordance with the shape, structure, features and spirit described in the claims of the present invention should be included within the scope of the claims of the present invention.
Claims
1. A method for preparing a barium ferrite / (aniline-co-6-(2-aminophenoxy)hexane-1-ol) copolymer conductive polymer nanocomposite microwave absorbing medium, characterized in that: 6-(2-aminophenoxy)hexane-1-ol was introduced as a second monomer, and it was co-carboxylated with the aniline monomer in Ba. 1-x La x Fe 12 O 19 In-situ polymerization is performed on the surface to enrich the morphology of the polyaniline, including the following steps: (1) Prepare hydrochloric acid solution; (2) Carboxylated Ba 1-x La x Fe 12 O 19 Dispersed in hydrochloric acid solution, the mixture was processed in a cell disruptor to obtain suspension I; (3) Add aniline monomer and 6-(2-aminophenoxy)hexane-1-ol to suspension I, and treat with a cell disruptor to obtain suspension II; (4) Prepare an ammonium persulfate hydrochloric acid solution as an initiator; (5) After transferring suspension II into a low-temperature water bath and stirring and pre-cooling for a period of time, slowly add the prepared initiator dropwise and react for a period of time to obtain suspension III; (6) The suspension III was centrifuged to obtain the precipitate, which was then washed by centrifugation with an alcohol-water solution. The resulting product was dried, ground, and sieved to finally obtain carboxylated Ba. 1-x La x Fe 12 O 19 / (aniline-co-6-(2-aminophenoxy)hexane-1-ol) copolymer conductive polymer nanocomposite microwave absorbing medium; Where x = 0.05~0.20, in step (3) carboxylation of Ba 1-x La x Fe 12 O 19 The mass ratio of the copolymer to the comonomer is 10:1 to 10:
3.
2. The preparation method of the barium ferrite / (aniline-co-6-(2-aminophenoxy)hexane-1-ol) copolymer conductive polymer nanocomposite microwave absorbing medium according to claim 1, characterized in that: The concentration of hydrochloric acid solution in step (1) is 1 mol / L.
3. The preparation method of the barium ferrite / (aniline-co-6-(2-aminophenoxy)hexane-1-ol) copolymer conductive polymer nanocomposite microwave absorbing medium according to claim 1, characterized in that: In step (2), Ba 1-x La x Fe 12 O 19 The preparation method is as follows: A mixed metal salt solution of ferric nitrate, barium nitrate, and lanthanum nitrate was prepared with a molar ratio of 12:(1-x):x, so that the iron ion concentration was 0.5 mol / L. The amount of sodium hydroxide used is 3n (Fe 3+ )*120%, sodium carbonate dosage is (n(Ba 2+ )+n(La 3+ Prepare a mixed precipitant solution by multiplying the concentration of sodium hydroxide by 150% to achieve a sodium hydroxide concentration of 5 mol / L. The prepared metal salt solution was added to the mixed precipitant solution, stirred for 2 hours, and then filtered to obtain the precursor precipitate. The precursor, sodium chloride, and potassium chloride were mixed in a 1:1:1 mass ratio, ball-milled at 400 rpm for 4 hours, calcined at 800℃ for 2 hours, and then washed to obtain Ba. 1-x La x Fe 12 O 19 Nanoparticles.
4. The method for preparing the barium ferrite / (aniline-co-6-(2-aminophenoxy)hexane-1-ol) copolymer conductive polymer nanocomposite microwave absorbing medium according to claim 1, characterized in that: In step (2), carboxylation of Ba 1-x La x Fe 12 O 19 The preparation method is as follows: Will Ba 1-x La x Fe 12 O 19 Nanoparticles and oleic acid were dispersed in deionized water at a mass ratio of 1:1 and reacted at 70°C for 1 hour. After washing away excess oleic acid by centrifugation with ethanol, the product was redispersed in an ethanol solution. Hydrogen peroxide was added at a molar ratio of n(OA):n(H2O2)=1:2 and the reaction was carried out for 8 hours to obtain the carboxylated product.
5. The method for preparing the barium ferrite / (aniline-co-6-(2-aminophenoxy)hexane-1-ol) copolymer conductive polymer nanocomposite microwave absorbing medium according to claim 1, characterized in that: The preparation method of 6-(2-aminophenoxy)hexane-1-ol in step (3) is as follows: 5g of 2-aminophenol was dissolved in 100mL of dichloromethane as solution 1, and di-tert-butyl ester solution was added to 50mL of dichloromethane as solution 2. Solution 2 was slowly added dropwise to solution 1. After the addition was completed, the mixture was stirred at 23℃ for 22h. Then, the solvent was removed under negative pressure and the mixture was ground with glacial pentane to obtain product 1. 9.58 g of product 1 was dissolved in 100 mL of DMF solution, and 9.5 g of potassium carbonate and 8.7 g of hexanol bromide were added. The mixture was stirred at 23 °C for 17 h. Subsequently, the reaction mixture was filtered and the filtrate was concentrated under negative pressure. The residue was dissolved in 100 mL of EtoAc solution, washed with water and brine, dried on MgSO4, and the solvent was removed under negative pressure. The primary product was purified by column chromatography to obtain product 2. 1.39 g of product 2 was dissolved in 6 mL of dichloromethane. A mixed solution of 2.8 mL of trifluoroacetic acid and 2.8 mL of dichloromethane was added dropwise. The mixture was stirred at 23 °C for 45 min. The solvent was removed under negative pressure. 50 mL of 1 mol / L NaOH solution was added. The aqueous phase was extracted with Et2O. The solution was then dried on MgSO4 and the solvent was removed under negative pressure. The final product, 6-(2-aminophenoxy)hexane-1-ol, was obtained by column chromatography.
6. The method for preparing the barium ferrite / (aniline-co-6-(2-aminophenoxy)hexane-1-ol) copolymer conductive polymer nanocomposite microwave absorbing medium according to claim 1, characterized in that: In step (3), the molar ratio of aniline monomer to 6-(2-aminophenoxy)hexane-1-ol is 9:
1.
7. The method for preparing the barium ferrite / (aniline-co-6-(2-aminophenoxy)hexane-1-ol) copolymer conductive polymer nanocomposite microwave absorbing medium according to claim 1, characterized in that: In step (4), the molar ratio of the copolymer monomer to ammonium persulfate is 1:1.2, and the concentration of the prepared ammonium persulfate hydrochloric acid solution is 0.5 mol / L.
8. The method for preparing the barium ferrite / (aniline-co-6-(2-aminophenoxy)hexane-1-ol) copolymer conductive polymer nanocomposite microwave absorbing medium according to claim 1, characterized in that: In step (5), the initiator is added at a rate of 0.2 to 0.4 mL / min, the reaction temperature is 0°C, and the reaction time is 20 h.