Steel plates for straight seam welding and their preparation methods

By microalloying Nb+Ti alloy and specific processing techniques, a tempered sorbite structure with nanoscale precipitates is formed, which solves the problem of matching high strength and toughness in straight seam welded pipes for crane booms, and reduces the amount of alloy used and production costs.

CN117947358BActive Publication Date: 2026-11-17HUNAN VALIN LIANYUAN IRON & STEEL CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410033337.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-09
Publication Date
2026-11-17
Estimated Expiration
2044-01-09

AI Technical Summary

Technical Problem

Existing technologies struggle to maintain good room temperature and low temperature toughness while ensuring high strength of straight seam welded pipes for crane booms. They also suffer from problems such as high alloy element usage and high cost.

Method used

By employing Nb+Ti alloy microalloying treatment, combined with specific processes such as rolling and quenching and tempering heat treatment, a tempered sorbite structure with nanoscale precipitates is formed. The chemical composition and process parameters are controlled to improve the strength and toughness matching of the steel plate.

Benefits of technology

This method achieves good room temperature and low temperature toughness in high-strength steel plates, reduces the amount of alloying elements used, and lowers production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117947358B_ABST
    Figure CN117947358B_ABST
Patent Text Reader

Abstract

This application discloses a steel plate for straight seam welding and its preparation method. The steel plate comprises the following chemical composition by mass percentage: C: 0.06%–0.08%, Si: 0.10%–0.20%, Mn: 1.50%–1.70%, Nb: 0.045%–0.055%, P≤0.010%, S≤0.030%, Mo: 0.30%–0.40%, Al: 0.02%–0.040%, Ti: 0.09%–0.11%, Ni: 0.04%–0.06%, Cr: 0.02%–0.04%, V: 0.025%–0.03%, with the remainder being Fe and unavoidable impurity elements. The steel plate for straight seam welding of this application possesses good strength, plasticity, and toughness, thereby improving the overall performance of the steel plate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of steel smelting technology, specifically relating to a steel plate for straight seam welding and its preparation method. Background Technology

[0002] As the weight, volume, and lifting height of items to be lifted in various construction projects increase, crawler cranes are demonstrating their superiority, and their demand is rising rapidly. Crane booms using straight seam welded pipes require high low-temperature impact toughness and withstand enormous pressure when operating in low-temperature environments.

[0003] To ensure the safety of straight seam welded pipes used in crane booms, these pipes must maintain good room temperature and low temperature toughness under high strength conditions, which makes production quite difficult.

[0004] To further reduce costs, the amount of alloying elements added to steel products needs to be reduced during composition design to meet the development requirements of lowering production costs and conserving alloy resources. Summary of the Invention

[0005] In view of this, this application provides a steel plate for straight seam welding and a method for preparing the same, aiming to improve the steel plate for straight seam welding by achieving a good match between strength, plasticity and toughness, thereby improving the overall performance of the steel plate.

[0006] In a first aspect, embodiments of this application provide a steel plate for straight seam welding, wherein the steel plate comprises the following chemical composition by mass percentage: C: 0.06%–0.08%, Si: 0.10%–0.20%, Mn: 1.50%–1.70%, Nb: 0.045%–0.055%, P≤0.010%, S≤0.030%, Mo: 0.30%–0.40%, Al: 0.02%–0.040%, Ti: 0.09%–0.11%, Ni: 0.04%–0.06%, Cr: 0.02%–0.04%, V: 0.025%–0.03%, with the remainder being Fe and unavoidable impurity elements.

[0007] According to one embodiment of this application, the metallographic structure of the steel plate is tempered sorbite.

[0008] According to one embodiment of this application, the tempered sorbite grain size in the steel used for straight seam welded steel plates is 5-8 μm.

[0009] According to one embodiment of this application, the thickness of the steel plate used for straight seam welding is 3 to 6 mm.

[0010] According to one embodiment of this application, the mechanical properties of the steel plate include: yield strength 890-1020 MPa; tensile strength 960-1100 MPa; elongation 14%-16%; and impact energy at -40℃ ≥45 J.

[0011] Secondly, embodiments of this application provide a method for preparing a steel plate for straight seam welding, comprising:

[0012] Molten steel is continuously cast to produce steel slabs, wherein the slabs contain the following chemical composition by mass percentage: C: 0.06%–0.08%, Si: 0.10%–0.20%, Mn: 1.50%–1.70%, Nb: 0.045%–0.055%, P≤0.010%, S≤0.030%, Mo: 0.30%–0.40%, Al: 0.020%–0.040%, Ti: 0.09%–0.11%, Ni: 0.04%–0.06%, Cr: 0.02%–0.04%, V: 0.025%–0.03%, with the remainder being Fe and unavoidable impurity elements;

[0013] Heated steel plates are produced by heating and holding steel slabs at the same temperature.

[0014] Heated steel plates are rolled to obtain hot-rolled steel plates;

[0015] Hot-rolled steel plates are subjected to quenching and tempering heat treatment to obtain steel plates for straight seam welding.

[0016] According to one embodiment of this application, the final heating temperature is 1200℃-1230℃; the holding time is 0.6-1.5h.

[0017] According to one embodiment of this application, rolling includes first to third passes of rolling at a temperature of 1120-1020°C; and final two passes of rolling at 800-920°C.

[0018] According to one embodiment of this application, the thickness of the hot-rolled steel sheet is 3-6 mm; the total reduction rate of the rolling process is 80%-90%.

[0019] According to one embodiment of this application, rolling a heated slab includes air cooling the heated slab to room temperature.

[0020] According to one embodiment of this application, quenching and tempering heat treatment includes:

[0021] The hot-rolled steel sheet is heated to 900℃-930℃ and held for 30-40 minutes to reaustify the hot-rolled steel sheet.

[0022] Next, quench the water to room temperature, then temper it at 630℃-670℃ for 20-30 minutes, and finally air cool it to room temperature.

[0023] This application has at least the following beneficial effects:

[0024] The steel plate for straight seam welding provided in this application is microalloyed with Nb+Ti alloy to refine the grain size. At the same time, through related processes such as controlled rolling, niobium and titanium in the steel plate are precipitated at the nanoscale with a precipitate size of 35-40nm to meet the performance requirements, resulting in a steel plate with a yield strength ≥890MPa, high strength, and good matching of plasticity and toughness. Attached Figure Description

[0025] To more clearly illustrate the technical solutions of the implementation regulations of this application, the drawings used in the embodiments of this application will be briefly introduced below. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0026] Figure 1 A graph showing the temperature change over time of a steel plate used for straight seam welding according to an embodiment of this application is shown.

[0027] Figure 2 The image shows an SEM microstructure of a steel plate used for straight seam welding according to Embodiment 1 of this application;

[0028] Figure 3 An SEM microstructure of a steel plate for straight seam welding according to Embodiment 2 of this application is shown;

[0029] Figure 4 An SEM microstructure of a steel plate for straight seam welding according to Embodiment 3 of this application is shown;

[0030] Figure 5 The SEM microstructure of the steel plate used for straight seam welding in Comparative Example 1 of this application is shown.

[0031] Figure 6 SEM microstructure of a steel plate used for straight seam welding, as shown in Comparative Example 2 of this application, is illustrated.

[0032] Figure 7 An SEM image of the steel plate used for straight seam welding, as shown in Comparative Example 3 of this application, is displayed. Detailed Implementation

[0033] To make the purpose, technical solution, and beneficial technical effects of this application clearer, the following detailed description is provided in conjunction with embodiments. It should be understood that the implementation details described in this specification are merely for illustrative purposes and are not intended to limit the scope of this application.

[0034] For simplicity, this application only explicitly discloses some numerical ranges. However, any lower limit can be combined with any upper limit to form a range not explicitly stated; and any lower limit can be combined with other lower limits to form a range not explicitly stated, just as any upper limit can be combined with any other upper limit to form a range not explicitly stated. Furthermore, although not explicitly stated, every point or individual value between the endpoints of the range is included within that range. Therefore, each point or individual value can be used as its own lower or upper limit and combined with any other point or individual value or with other lower or upper limits to form a range not explicitly stated.

[0035] In the description of this application, it should be noted that, unless otherwise stated, "above" and "below" include the stated number, and "multiple" in "one or more" means two or more.

[0036] The foregoing description of this application is not intended to describe every disclosed implementation or method. Instead, the following description provides more specific examples of exemplary embodiments. Throughout the application, guidance is provided through a series of embodiments, which can be used in various combinations. The examples listed are representative only and should not be construed as exhaustive.

[0037] Steel plates for straight seam welding

[0038] In a first aspect, embodiments of this application provide a steel plate for straight seam welding, wherein the steel plate comprises the following chemical composition by mass percentage: C: 0.06%–0.08%, Si: 0.10%–0.20%, Mn: 1.50%–1.70%, Nb: 0.045%–0.055%, P≤0.010%, S≤0.030%, Mo: 0.30%–0.40%, Al: 0.02%–0.040%, Ti: 0.09%–0.11%, Ni: 0.04%–0.06%, Cr: 0.02%–0.04%, V: 0.025%–0.03%, with the remainder being Fe and unavoidable impurity elements.

[0039] According to an embodiment of this application, the steel plate used for straight seam welding is manufactured using a low-cost method. The composition design considers adding alloying elements such as Cr, Ni, Mo, Nb, V, and Ti to C and Mn steel, while avoiding the addition of more expensive alloys such as W. With this composition, relevant process controls, such as quenching and tempering heat treatment, ensure that the strength and low-temperature toughness of the seamless steel plate meet the requirements.

[0040] According to the embodiments of this application, high-strength straight seam steel plates can be widely used in the main rotating tube of crawler crane booms and various high-strength structural components, and can also be applied to fields such as hydraulic cylinders and offshore platform structures to replace the use of seamless steel plates and reduce the overall manufacturing cost.

[0041] In the embodiments of this application, from the perspective of the prepared steel plate products, the use of microalloying combinations such as Nb, V, Ti, and Mo can better meet the performance requirements of the steel plate, while also significantly reducing the cost of materials.

[0042] Carbon (C): 0.06%–0.08%. The main function of C is solid solution strengthening, making it a crucial element for ensuring the strength of high-frequency straight seam steel plates. To improve hardenability and achieve a yield strength greater than 890 MPa, C must be above 0.05%. If the C content exceeds 0.10%, the plasticity and toughness of the steel will decrease, and a high C content will also lead to poor weldability. Therefore, the range of C is 0.06%–0.08%.

[0043] Mn content: 1.50%–1.70%. The effect of Mn on the mechanical properties of quenched and tempered steel is mainly achieved by improving the hardenability of the steel. If the Mn content is below 1.50%, the expected strengthening effect will not be achieved; if the Mn content is above 1.80%, the center segregation of the steel will worsen, and the plasticity and toughness will decrease. At the same time, a high Mn content will lead to poor weldability. Therefore, the Mn content is designed to be controlled within the range of 1.50%–1.70%.

[0044] Mo (Mo): 0.30%–0.40%. Mo can improve the hardenability and hot strength of steel, and prevent temper brittleness. The effect is more pronounced when the Mo content is above 0.30%, but higher Mo content will lead to poor weldability of the steel. Furthermore, Mo is a precious metal, so it should be added as little as possible while still meeting performance requirements. The Mo range is 0.30%–0.40%.

[0045] Al: 0.020-0.040%. Al is the main deoxidizing element in steel and also an inexpensive grain-refining element. The main purpose of adding Al in this invention is to refine the grains and fix the nitrogen in the steel, thereby significantly improving the impact toughness of the steel. The Al content should be greater than 0.020%. If the Al content exceeds 0.050%, it will lead to an increase in non-metallic inclusions in the steel or a decrease in toughness. Therefore, its upper limit is set below 0.050%, and its range can be 0.020% to 0.040%.

[0046] Ti: 0.09%~0.11%. Titanium has a strong affinity for N, O, and C. In this invention, ferrotitanium is added to the steel for micro-titanium treatment. Ti reacts with N in the steel to form TiN. The TiN precipitated in the partially solidified state can prevent grain growth during heating, thus improving the plasticity and toughness of the steel plate, and also improving its weldability. However, excessive addition of Ti can easily form TiN inclusions, which reduces the toughness of the steel plate. Therefore, its upper limit is set below 0.11%.

[0047] Nb: 0.045%–0.055%. Niobium mainly plays a role in grain refinement and strengthening in steel; adding too much weakens the strengthening effect and is uneconomical. The preferred range is 0.045%–0.055%.

[0048] P: ≤0.001%. Phosphorus tends to segregate at grain boundaries, which can increase the ductile-brittle transition temperature and reduce the toughness of steel. Too high a content will lead to a decrease in impact toughness at -40℃. It is limited to below 0.001%.

[0049] S: ≤0.003%. Sulfur readily forms non-hard inclusions with manganese and other materials. An increase in its content leads to an increase in the number of inclusions, which extend and deform along the rolling direction during processing, disrupting the continuity of the material matrix and reducing the low-temperature impact toughness of the seamless steel plate. It is best to limit it to below 0.005%, and more preferably below 0.003%.

[0050] Si: 0.10%~0.20%. Si is an effective deoxidizing element. Too low a content will weaken the deoxidation effect, while too high a content will reduce the toughness of the steel. The Si content range of 0.10%~0.20% is selected.

[0051] Ni: 0.04%~0.06%. Ni is a solid solution strengthening agent in steel, and it also has good hardenability. Most importantly, it can effectively improve the low-temperature performance of steel.

[0052] In some alternative embodiments, the metallographic structure of the steel plate is tempered sorbite.

[0053] According to embodiments of this application, tempered sorbite can be understood as sorbite formed through tempering. This type of sorbite is generally harder than the microstructure in its initial state.

[0054] According to embodiments of this application, during tempering, recrystallization and grain growth of metal grains may lead to a reduction in dislocation density and lattice defects, which is beneficial for grain refinement and enhances the machinability of the steel plate. By adjusting the tempering temperature and time through the tempering process, structures beneficial to toughness, such as sorbite, can be formed in the alloy.

[0055] According to embodiments of this application, the fine, uniform granular or lamellar structure in the sorbite structure gives the metal a high macroscopic hardness. Sorbite can improve the toughness of the metal and inhibit crack propagation, thereby improving the metal's toughness and tensile strength. The formation of sorbite can sometimes improve the fatigue resistance of the metal; furthermore, the fine structure of sorbite can slow the propagation of fatigue cracks and extend the lifespan of metal parts.

[0056] In some alternative embodiments, the tempered sorbite grain size in the steel used for straight seam welded steel plates is 5-8 μm.

[0057] According to the embodiments of this application, the steel plate has grains of the above-mentioned size through a specific process, thereby having a reduced dislocation density and lattice defects, which is beneficial to enhancing the processing performance of the steel plate.

[0058] In some alternative embodiments, the thickness of the steel plate used for straight seam welding is 3 to 6 mm. Steel pipes with an outer diameter of Φ40 mm to Φ100 mm and a wall thickness of 3 to 6 mm can be manufactured.

[0059] According to the embodiments of this application, the thickness of the steel plate is within the above-mentioned range, which is beneficial for preparing a straight seam welded steel plate while controlling its mechanical properties, and for giving the straight seam welded steel plate good performance.

[0060] In some alternative embodiments, the mechanical properties of the steel plate include: yield strength 890-1020 MPa; tensile strength 960-1100 MPa; elongation 14%-16%; and impact energy ≥45 J at -40℃.

[0061] Secondly, embodiments of this application provide a method for preparing a steel plate for straight seam welding, comprising:

[0062] Molten steel is continuously cast to produce steel slabs, wherein the slabs contain the following chemical composition by mass percentage: C: 0.06%–0.08%, Si: 0.10%–0.20%, Mn: 1.50%–1.70%, Nb: 0.045%–0.055%, P≤0.010%, S≤0.030%, Mo: 0.30%–0.40%, Al: 0.020%–0.040%, Ti: 0.09%–0.11%, Ni: 0.04%–0.06%, Cr: 0.02%–0.04%, V: 0.025%–0.03%, with the remainder being Fe and unavoidable impurity elements;

[0063] Heated steel plates are produced by heating and holding steel slabs at the same temperature.

[0064] Heated steel plates are rolled to obtain hot-rolled steel plates;

[0065] Hot-rolled steel plates are subjected to quenching and tempering heat treatment to obtain steel plates for straight seam welding.

[0066] According to the embodiments of this application, the preparation method of steel plates for straight seam welding generally includes: obtaining molten iron → KR desulfurization → converter smelting → ladle refining (LF+RH) → slab continuous casting → controlled rolling and controlled cooling → quenching and tempering heat treatment → performance testing → packaging and warehousing.

[0067] According to the embodiments of this application, by controlling the composition of the slab before rolling and smelting, it is beneficial to obtain steel plates with better strength, plasticity and toughness.

[0068] In some embodiments, the molten steel is used prior to continuous casting, including a smelting process. The smelting process is specifically as follows:

[0069] A layer of carbon powder is laid at the bottom of the medium-frequency induction furnace to ensure a low oxygen content in the steel. Scrap steel and pig iron are then added and heated for smelting. After the molten steel is cleared, a slag remover is added for the first slag removal treatment, followed by the addition of ferromanganese. Then, aluminum wire (0.1 kg) and ferrotitanium (0.1 kg) are added to each furnace of molten steel for deoxidation and nitrogen determination. The exposed molten surface is covered with a slag remover. After deoxidation and nitrogen determination are maintained for approximately 2–5 minutes, ferrovanadium, ferroniobium, and ferrotitanium are added for smelting at a temperature of 1500–1550℃ until the molten steel is cleared, followed by a second slag removal treatment.

[0070] Next, desulfurization and slag removal are carried out by adding a desulfurizing agent. After 3-5 minutes, a layer of slag removal agent is covered, and a third slag removal process is performed. After the composition is tested and found to be qualified, the steel is tapped. The furnace temperature is controlled at 1550℃ and the steel is poured into an iron round ingot mold with dimensions of 230mm×Φ120mm.

[0071] In some alternative implementations, the final heating temperature is 1200℃-1230℃; the holding time is 0.6-1.5h.

[0072] In some alternative embodiments, rolling includes first to third passes at a temperature of 1120-1020°C; and final two passes at 800-920°C.

[0073] In some embodiments, rolling includes: heating the steel slab to 1200°C-1230°C and holding it at that temperature for 1 hour, then starting two-stage controlled rolling; followed by a complete recrystallization temperature of 989°C; the first three passes of hot rolling are performed at temperatures ranging from 1120°C to 1020°C to ensure complete recrystallization; the last two passes are performed at temperatures below 920°C; and finally, the slab is air-cooled to room temperature. In some embodiments, the steel slab is a steel block cut to 55×40×31mm after casting.

[0074] In some alternative implementations, the thickness of the hot-rolled steel sheet is 3-6 mm; the total reduction rate of the rolling process is 80%-90%.

[0075] According to the embodiments of this application, the thickness of the hot-rolled steel plate can be understood as the thickness of the tube wall of the hot-rolled steel plate. By controlling the thickness of the hot-rolled steel plate within the above-mentioned range, and the total reduction rate of rolling within the above-mentioned range, it is beneficial to control the final thickness of the steel plate product, thereby facilitating the control of its mechanical properties and processing performance.

[0076] In some alternative implementations, rolling the heated slab includes air cooling the heated slab to room temperature.

[0077] According to the embodiments of this application, by air-cooling the heated slab to room temperature, it is beneficial to control its crystallization rate, refine the grains, facilitate the subsequent refinement of grains in the steel plate, and improve its toughness.

[0078] In some alternative implementations, the quenching and tempering heat treatment includes:

[0079] The hot-rolled steel sheet is heated to 900℃-930℃ and held for 30-40 minutes to reaustify the hot-rolled steel sheet.

[0080] Next, quench the water to room temperature, then temper it at 630℃-670℃ for 20-30 minutes, and finally air cool it to room temperature.

[0081] According to embodiments of this application, quenching and tempering (Q&T) is a common heat treatment process, particularly suitable for improving the properties of steel. This process typically involves two steps: quenching and tempering.

[0082] According to embodiments of this application, quenching can rapidly cool steel, thereby increasing its hardness and strength. Tempering is a key step in quenching and tempering heat treatment, which adjusts the hardness and strength of steel by heating it to a moderate temperature. This process helps reduce internal stress, improves toughness, and makes the steel more durable. It also promotes the formation of sorbite, and through quenching and tempering heat treatment, it helps to enhance the hardness, strength, toughness, wear resistance, and dimensional stability of the steel plate.

[0083] In some embodiments, the quenching and tempering heat treatment includes:

[0084] After final rolling, the welded pipe steel is air-cooled to room temperature, then heated to 900℃-930℃ and held for 30 minutes to reauthitize it. After holding, it is water-quenched to room temperature, then tempered at 630℃-670℃ for 30 minutes, and finally air-cooled to room temperature.

[0085] Example

[0086] The following embodiments describe the disclosure of this application in more detail. These embodiments are merely illustrative, as various modifications and variations will be apparent to those skilled in the art within the scope of the disclosure of this application. Unless otherwise stated, all parts, percentages, and ratios reported in the following embodiments are based on weight, and all reagents used in the embodiments are commercially available or synthesized by conventional methods and can be used directly without further processing, and the instruments used in the embodiments are commercially available.

[0087] Examples 1-3 and Comparative Examples 1-3

[0088] The straight seam welded steel plates of Examples 1-3 of this application comprise, by mass percentage, the following chemical elements: C: 0.06%–0.08%, Si: 0.10%–0.20%, Mn: 1.50%–1.70%, Nb: 0.045%–0.055%, P≤0.010%, S≤0.030%, Mo: 0.30%–0.40%, Al: 0.020%–0.040%, Ti: 0.09%–0.11%, Ni: 0.04%–0.06%, Cr: 0.02%–0.04%, V: 0.025%–0.03%, with the balance being Fe and unavoidable impurities. The specific compositions of the straight seam welded steel plates of Examples 1-3 are shown in Table 1. The specific compositions of the straight seam welded steel plates of Comparative Examples 1-3 are also shown in Table 1.

[0089] Table 1 shows the chemical composition of the experimental steel plates in each embodiment and comparative example.

[0090]

[0091]

[0092] The billet of the embodiment shown in Table 1 was placed in a heating furnace at 1200–1230°C and held for 60 min. It was then subjected to multi-pass hot rolling, with the first two passes involving a large reduction of 50%–60%. The initial rolling temperature was 1100–1120°C, and the final rolling temperature was 800–830°C, yielding a steel plate with a thickness of 3–6 mm. The final rolled steel plate underwent quenching and tempering heat treatment: quenching at 900°C–930°C for 30 min, tempering at 630°C–670°C for 30 min, followed by air cooling to room temperature. Specific process parameters for the straight seam welded steel plate of the embodiment are detailed in Table 2. Specific process parameters for the straight seam welded steel plate of the comparative example are detailed in Table 3.

[0093] Table 2. Process parameters for preparing straight seam welded steel plates in each embodiment.

[0094]

[0095] Table 3. Preparation process parameters of straight seam welded steel plates for each comparative example.

[0096]

[0097] Test section

[0098] The steel used for straight seam welded steel plates prepared in the examples and comparative examples was sampled according to GB / T 2975 "Sampling Location and Sample Preparation for Mechanical Property Testing of Steel and Steel Products".

[0099] The steel plates obtained in the examples and comparative examples were subjected to mechanical property testing in accordance with GB / T228.1-2010 "Metallic materials - Tensile testing - Part 1: Test at room temperature" with a gauge length of 50 mm. The properties corresponding to different process parameters are shown in Table 4.

[0100] Table 4 Mechanical properties of steel in the examples and comparative experiments

[0101]

[0102] As shown in Table 4 above, by controlling the composition of chemical elements in the steel plates of Examples 1 to 3, especially the content of Nb, V, Ti, Ni, Cr, and Mo, as well as the rolling and cooling processes, the steel plates have excellent mechanical properties and can meet the performance requirements of 890 MPa for straight seam welded steel plates. However, the steel plates in the comparative examples, due to their composition and processes not being within the scope of the application, do not meet the performance requirements of 890 MPa straight seam welded steel plates.

[0103] Furthermore, when calculating the mechanical properties of steel plates, the measured values ​​are all divided by the cross-sectional area of ​​the steel plate (thickness multiplied by width). Therefore, the mechanical properties of the steel plates mentioned above are not positively correlated with the thickness of the finished product, but are only related to the elements, metallographic structure and grain size.

[0104] (2) Metallographic structure observation:

[0105] Using a nitric acid-alcohol etching reagent, apply 1-2 drops of the reagent to the surface of the steel plate, leaving it on the sample surface for a short time until the sample surface darkens from its mirror image. After rinsing with alcohol, quickly process the sample on absorbent paper, and finally dry it with a hair dryer. The tissue type can then be determined under a metallographic microscope. The micrographs of Examples 1, 2, and 3 are shown in the figure below. Figure 2 , Figure 3 , Figure 4 As shown, the micrographs of Comparative Examples 1, 2, and 3 are as follows: Figure 5-7As shown, both the examples and the comparative examples have tempered sorbite microstructures. However, due to differences in composition and process, the size and distribution of recrystallized grains and precipitates in the microstructures are different, ultimately resulting in performance differences between the examples and the comparative examples.

[0106] The above are merely specific embodiments of this application, but the scope of protection of this application is not limited thereto. Any changes or substitutions made by those skilled in the art should be included within the scope of protection of this application. Therefore, the scope of protection of this application should be determined by the scope of the claims.

Claims

1. A steel plate for straight seam welding, characterized in that, The steel plate comprises the following chemical composition by mass percentage: C: 0.06%–0.08%, Si: 0.10%–0.20%, Mn: 1.50%–1.70%, Nb: 0.045%–0.055%, P≤0.010%, S≤0.030%, Mo: 0.30%–0.40%, Al: 0.02%–0.040%, Ti: 0.09%–0.11%, Ni: 0.04%–0.06%, Cr: 0.02%–0.04%, V: 0.025%–0.03%, with the remainder being Fe and unavoidable impurity elements; The metallographic structure of the steel plate is tempered sorbite, and the grain size of the tempered sorbite is 5-8 μm. The mechanical properties of the steel plate include: yield strength ≥ 989 MPa; tensile strength 1023~1100 MPa; elongation ≥ 14%; impact energy at -40℃ ≥ 125 J.

2. The steel plate for straight seam welding according to claim 1, characterized in that, The thickness of the steel plate used for straight seam welding is 3 to 6 mm.

3. A method for preparing the steel plate according to any one of claims 1 to 2, characterized in that, include: Molten steel is continuously cast to obtain steel slabs, wherein the slabs comprise the following chemical composition by mass percentage: C: 0.06%–0.08%, Si: 0.10%–0.20%, Mn: 1.50%–1.70%, Nb: 0.045%–0.055%, P≤0.010%, S≤0.030%, Mo: 0.30%–0.40%, Al: 0.020%–0.040%, Ti: 0.09%–0.11%, Ni: 0.04%–0.06%, Cr: 0.02%–0.04%, V: 0.025%–0.03%, with the remainder being Fe and unavoidable impurity elements; Heated steel plates are produced by heating and holding steel slabs at the same temperature. Heated steel plates are rolled to obtain hot-rolled steel plates; The hot-rolled steel plate is subjected to quenching and tempering heat treatment to obtain the steel plate used for straight seam welding.

4. The method according to claim 3, characterized in that, The final temperature of the heating is 1200℃-1230℃; the holding time is 0.6-1.5h.

5. The method according to claim 3, characterized in that, The rolling process includes the first to third passes at a temperature of 1120-1020°C, and the final two passes at a temperature of 800-920°C.

6. The method according to claim 3, characterized in that, The thickness of the hot-rolled steel plate is 3-6 mm; the total reduction rate of the rolling process is 80%-90%. The process of rolling the heated slab includes air cooling the heated slab to room temperature.

7. The method according to claim 3, characterized in that, The quenching and tempering heat treatment includes: The hot-rolled steel plate is heated to 900℃-930℃ and held for 30-40 minutes to reaustify the hot-rolled steel plate. Next, quench the water to room temperature, then temper it at 630℃-670℃ for 20-30 minutes, and finally air cool it to room temperature.

Citation Information

Patent Citations

  • Steel for 770MPa straight seam welded steel pipe and manufacturing method thereof

    CN115287531A

  • 800MPa-grade easily-welded hydroelectric steel plate with excellent low-temperature impact toughness

    CN115896622A

  • Laminated biaxially oriented polyester film for magnetic recording medium

    JP1994000930A