Method for forming germanium-silicon channel gate oxide layer
By forming a germanium-enriched interface layer on the germanium-silicon epitaxial layer and combining it with multiple annealing processes, the problem of uneven Ge enrichment in the gate oxide layer of the germanium-silicon channel was solved, thereby improving the interface quality and device performance of the germanium-silicon channel.
Patent Information
- Application Number
- CN202410115206.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-26
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-01-26
AI Technical Summary
The existing technology uses thermal oxidation to generate high-quality germanium-silicon channel gate oxide layers, but the reaction process consumes Si in the SiGe channel, resulting in uneven Ge enrichment and affecting device performance.
By forming a first gate oxide layer on the germanium-silicon epitaxial layer as a germanium-enriched interface layer, and combining atomic layer deposition and multiple annealing processes, the Ge distribution in the germanium-silicon channel is optimized. This includes thermal oxidation, deposition, and annealing steps to improve interface quality and Ge uniformity.
The resulting gate oxide layer is of high quality, reduces interface defects, and improves the Ge uniformity of the germanium-silicon channel, thereby improving the reliability and electrical performance of the device.
Smart Images

Figure CN117954311B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor technology, and in particular to a method for forming a germanium-silicon channel gate oxide layer. Background Technology
[0002] Compared to the traditional silicon-on-insulator (SOI) structure, the silicon-germanium-on-insulator (SGOI) structure can improve hole mobility and significantly enhance the performance of P-type metal oxide semiconductor field-effect transistors (PMOS).
[0003] Currently, thermal oxidation or atomic layer deposition (ALD) is the main methods used to generate the gate oxide layer in SiGe channels. Thermal oxidation produces a high-quality gate oxide layer with fewer defects, but the reaction process mainly consumes Si in the SiGe channel to form SiO2, resulting in Ge enrichment on the surface of the SiGe channel and uneven Ge distribution within the channel, which affects device performance.
[0004] To address the aforementioned issues, a novel method for forming germanium-silicon channel gate oxide layers is needed. Summary of the Invention
[0005] In view of the shortcomings of the prior art described above, the purpose of this invention is to provide a method for forming a germanium-silicon channel gate oxide layer, which solves the problem that the gate oxide layer generated by the thermal oxidation method in the prior art has high quality and few defects, but mainly consumes Si in the SiGe channel to form SiO2 during the reaction process, resulting in Ge enrichment on the surface of the SiGe channel and uneven Ge distribution in the channel, which affects the device performance.
[0006] To achieve the above and other related objectives, the present invention provides a method for forming a germanium-silicon channel gate oxide layer, comprising: Step 1: Provide a substrate, form a germanium-silicon epitaxial layer on the substrate, and remove the oxide layer on the germanium-silicon epitaxial layer; Step 2: A first gate oxide layer of the target thickness is formed on the germanium-silicon epitaxial layer using a thermal oxidation method. The first gate oxide layer serves as an interface layer for germanium enrichment. Step 3: Form a second gate oxide layer on the first gate oxide layer using a deposition method; Step 4: Use the first annealing to repair oxygen vacancies and densify the second gate oxide layer, so that a third gate oxide layer is formed at the interface between the first gate oxide layer and the germanium-silicon epitaxial layer. Step 5: Use a second annealing process to improve the uniformity of germanium in the germanium-silicon epitaxial layer.
[0007] Preferably, the substrate in step one is a silicon-on-insulator substrate.
[0008] Preferably, the method for removing the oxide layer on the germanium-silicon epitaxial layer in step one includes: the reaction gases are hydrogen and nitrogen, the hydrogen flow rate is 3-25 liters per minute, the nitrogen flow rate is 2-25 liters per minute, the temperature is 400-600℃, the processing time is 10 seconds-5 minutes, and the pressure is 5-25 Torr.
[0009] Preferably, the thermal oxidation method in step two includes: using oxygen or nitrous oxide as the reaction gas, a temperature of 650-1000℃, and a processing time of 8-90 seconds.
[0010] Preferably, the deposition method in step three is atomic layer deposition.
[0011] Preferably, the process conditions for the atomic layer deposition method in step three include: a temperature of 150-400℃, a cycle number of 10-60, and a gate oxide layer thickness of 15-50 angstroms.
[0012] Preferably, the first annealing method in step four includes at least one of uniform annealing, peak annealing, laser annealing, and flash annealing.
[0013] Preferably, the process conditions for the first annealing in step four include: a temperature of 700-1050℃, an atmosphere of oxygen and nitrogen, an oxygen flow rate of 0.05-5 ml / s, a nitrogen flow rate of 0.05-5 ml / s, and an annealing time of 1-60s.
[0014] Preferably, the second annealing method in step five is uniform temperature annealing.
[0015] Preferably, the process conditions for the second annealing in step five include: a hot annealing temperature of 800-1100℃, an atmosphere of oxygen and nitrogen, and an annealing time of 5-120s.
[0016] As described above, the method for forming the germanium-silicon channel gate oxide layer of the present invention has the following beneficial effects: The method of this invention produces high-quality gate oxide while reducing interface defects and improving interface quality. It also improves the uniformity of Ge in the SiGe channel, thereby enhancing the reliability and electrical performance of the device. Attached Figure Description
[0017] Figure 1 The diagram shown is a schematic representation of the process flow of the present invention. Figure 2 The diagram shown illustrates the formation of a germanium-silicon epitaxial layer according to the present invention. Figure 3 The diagram shown illustrates the removal of the oxide layer on the germanium-silicon epitaxial layer according to the present invention. Figure 4This is a schematic diagram illustrating the formation of the first gate oxide layer according to the present invention; Figure 5 This is a schematic diagram illustrating the formation of the second gate oxide layer according to the present invention; Figure 6 The diagram shown is a schematic diagram of the first annealing process of the present invention. Figure 7 The diagram shown is a schematic of the second annealing process of this invention. Detailed Implementation
[0018] The following specific examples illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and various details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention.
[0019] Please see Figure 1 The present invention provides a method for forming a germanium-silicon channel gate oxide layer, comprising: Step 1: Provide a substrate 101, on which a germanium-silicon epitaxial layer 102 is formed. The germanium-silicon epitaxial layer 102 will oxidize under natural conditions to form an oxide layer. Remove the oxide layer on the germanium-silicon epitaxial layer 102 to form... Figure 2 The structure shown; In some embodiments, the substrate 101 in step one is a silicon-on-insulator (SOI) substrate. The SOI substrate includes an insulating layer located beneath a thin semiconductor layer serving as the active layer of the SOI substrate. The semiconductor and bulk semiconductor of the active layer typically include the crystalline semiconductor material silicon, but may also include one or more other semiconductor materials, such as germanium, silicon-germanium alloys, compound semiconductors (e.g., GaAs, AlAs, InAs, GaN, AlN, etc.) or alloys thereof (e.g., GaxAl1-xAs, GaxAl1-xN, InxGa1-xAs, etc.), oxide semiconductors (e.g., ZnO, SnO2, TiO2, Ga2O3, etc.) or combinations thereof. The semiconductor material may be doped or undoped. Other substrates that may be used include multilayer substrates, gradient substrates, or mixed-orientation substrates.
[0020] In some embodiments, please refer to Figure 3 The method for removing the oxide layer on the germanium-silicon epitaxial layer 102 in step one includes: using hydrogen and nitrogen as the reaction gases, with a hydrogen flow rate of 3-25 liters per minute and a nitrogen flow rate of 2-25 liters per minute, a temperature of 400-600℃, a processing time of 10 seconds to 5 minutes, and a pressure of 5-25 Torr. For example, a hydrogen flow rate of 6 liters per minute, a removal temperature of 550℃, and a time of 60 seconds.
[0021] Step 2: Form a first gate oxide layer 103 of the target thickness on the germanium-silicon epitaxial layer 102 using a thermal oxidation method, forming a structure as shown in the figure. Figure 4 In the structure shown, the first gate oxide layer 103 serves as the interface layer for germanium enrichment. The ultrathin gate oxide layer is generated by thermal oxidation, resulting in high quality and few defects. The thickness of this step needs to be adjusted according to the actual process to avoid consuming too much silicon, which would lead to germanium enrichment in the germanium-silicon epitaxial layer 102.
[0022] Step 3: Form a second gate oxide layer 104 on the first gate oxide layer 103 using a deposition method, forming a structure as shown in the figure. Figure 5 The structure shown has a second gate oxide layer 104 with a thickness greater than that of the first gate oxide layer 103. For example, the second gate oxide layer 104 has a thickness of 18 angstroms, an atomic layer deposition temperature of 280°C, and a cycle number of 18.
[0023] In some embodiments, the deposition method in step three is atomic layer deposition.
[0024] In some embodiments, the process conditions for atomic layer deposition in step three include: a temperature of 150-400°C, a cycle number of 10-60, and a gate oxide layer thickness of 15-50 angstroms. For example, the thickness of the first gate oxide layer 103 is 9 angstroms, the temperature is 900°C, and the deposition time is 15 s.
[0025] Step 4: The second gate oxide layer 104 is subjected to oxygen vacancy repair and densification treatment using a first annealing process, resulting in the formation of a third gate oxide layer 105 at the interface between the first gate oxide layer 103 and the germanium-silicon epitaxial layer 102, forming a structure as shown in the image. Figure 6 The structure shown; In some embodiments, the first annealing method in step four includes at least one of uniform annealing, peak annealing, laser annealing, and flash annealing.
[0026] In some embodiments, the process conditions for the first annealing in step four include: a temperature of 700-1050°C, an atmosphere of oxygen and nitrogen, an oxygen flow rate of 0.05-5 mL / s, a nitrogen flow rate of 0.05-5 mL / s, and an annealing time of 1-60 s. For example, an annealing temperature of 1000°C, a high-temperature annealing time of 10 s, an oxygen flow rate of 0.5 slm / s, and a N2 flow rate of 20 slm / s.
[0027] Step 5: A second annealing process is used to improve the uniformity of germanium in the germanium-silicon epitaxial layer 102, forming a layer as shown in the image. Figure 7 The structure shown.
[0028] In some embodiments, the second annealing method in step five is uniform temperature annealing.
[0029] In some embodiments, the process conditions for the second annealing in step five include: a hot annealing temperature of 800-1100°C, an atmosphere of oxygen and nitrogen, and an annealing time of 5-120 seconds. For example, an annealing temperature of 1050°C and a high-temperature annealing time of 20 seconds.
[0030] The method of this invention produces high-quality gate oxide while reducing interface defects and improving interface quality. It also improves the uniformity of Ge in the SiGe channel, thereby enhancing the reliability and electrical performance of the device.
[0031] It should be noted that the illustrations provided in this embodiment are only schematic representations of the basic concept of the present invention. Therefore, the drawings only show the components related to the present invention and are not drawn according to the actual number, shape and size of the components in the actual implementation. In the actual implementation, the form, quantity and proportion of each component can be arbitrarily changed, and the layout of the components may also be more complex.
[0032] In summary, the method of the present invention produces high-quality gate oxide while reducing interface defects and improving interface quality. It also improves the uniformity of Ge in the SiGe channel, thereby enhancing the reliability and electrical performance of the device.
[0033] Therefore, this invention effectively overcomes the various shortcomings of the prior art and has high industrial application value.
[0034] The above embodiments are merely illustrative of the principles and effects of the present invention and are not intended to limit the invention. Any person skilled in the art can modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by those skilled in the art without departing from the spirit and technical concept disclosed in the present invention should still be covered by the claims of the present invention.
Claims
1. A method for forming a germanium-silicon channel gate oxide layer, characterized in that, At least including: Step 1: Provide a substrate, form a germanium-silicon epitaxial layer on the substrate, and remove the oxide layer on the germanium-silicon epitaxial layer; Step 2: A first gate oxide layer of the target thickness is formed on the germanium-silicon epitaxial layer using a thermal oxidation method. The first gate oxide layer serves as an interface layer for germanium enrichment. Step 3: Form a second gate oxide layer on the first gate oxide layer using a deposition method; Step 4: Use the first annealing to repair oxygen vacancies and densify the second gate oxide layer, so that a third gate oxide layer is formed at the interface between the first gate oxide layer and the germanium-silicon epitaxial layer. Step 5: Use a second annealing process to improve the uniformity of germanium in the germanium-silicon epitaxial layer.
2. The method for forming a germanium-silicon channel gate oxide layer according to claim 1, characterized in that: The substrate mentioned in step one is a silicon-on-insulator substrate.
3. The method for forming a germanium-silicon channel gate oxide layer according to claim 1, characterized in that: The method for removing the oxide layer on the germanium-silicon epitaxial layer in step one includes: using hydrogen and nitrogen as the reaction gases, with a hydrogen flow rate of 3-25 liters per minute, a nitrogen flow rate of 2-25 liters per minute, a temperature of 400-600℃, a processing time of 10 seconds to 5 minutes, and a pressure of 5-25 Torr.
4. The method for forming a germanium-silicon channel gate oxide layer according to claim 1, characterized in that: The thermal oxidation method in step two includes: using oxygen or nitrous oxide as the reaction gas, a temperature of 650-1000℃, and a processing time of 8-90 seconds.
5. The method for forming a germanium-silicon channel gate oxide layer according to claim 1, characterized in that: The deposition method described in step three is atomic layer deposition.
6. The method for forming a germanium-silicon channel gate oxide layer according to claim 5, characterized in that: The process conditions for the atomic layer deposition method in step three include: a temperature of 150-400℃, a cycle number of 10-60, and a gate oxide layer thickness of 15-50 angstroms.
7. The method for forming a germanium-silicon channel gate oxide layer according to claim 1, characterized in that: The first annealing method in step four includes at least one of uniform annealing, peak annealing, laser annealing, and flash annealing.
8. The method for forming a germanium-silicon channel gate oxide layer according to claim 7, characterized in that: The process conditions for the first annealing in step four include: a temperature of 700-1050℃, an atmosphere of oxygen and nitrogen, an oxygen flow rate of 0.05-5 ml / s, a nitrogen flow rate of 0.05-5 ml / s, and an annealing time of 1-60s.
9. The method for forming a germanium-silicon channel gate oxide layer according to claim 1, characterized in that: The second annealing method in step five is uniform temperature annealing.
10. The method for forming a germanium-silicon channel gate oxide layer according to claim 9, characterized in that: The process conditions for the second annealing in step five include: a hot annealing temperature of 800-1100℃, an atmosphere of oxygen and nitrogen, and an annealing time of 5-120s.
Citation Information
Patent Citations
Method for forming silicon-germanium epitaxial layer
CN102479717A
Manufacturing method of germanium-silicon layer of FDSOI
CN113937055A