Aluminum alloys and their manufacturing methods

By controlling the cooling process of the alloy melt during casting, Al-Si-Mg-Fe-Mn compounds are preferentially precipitated, solving the deformation and energy consumption problems caused by heat treatment in aluminum alloy manufacturing. This enables the heat treatment-free manufacturing of high-hardness aluminum alloys, reducing costs and CO2 emissions.

CN117987695BActive Publication Date: 2026-11-17TOYOTA JIDOSHA KK
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202311460611.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-11-07
Filing Date
2023-11-06
Publication Date
2026-11-17
Estimated Expiration
2043-11-06

AI Technical Summary

Technical Problem

In the existing aluminum alloy manufacturing process, heat treatment causes deformation and high energy consumption, leading to increased costs and CO2 emissions. At the same time, it is difficult to obtain aluminum alloys with sufficient hardness without heat treatment.

Method used

By controlling the cooling process of the alloy melt during casting, Al-Si-Mg-Fe-Mn compounds are preferentially precipitated, while the precipitation of Mg-Si compounds is suppressed. Aluminum alloy materials composed of Si, Mg, Mn, and Fe are used, and the cooling temperature and time are controlled to suppress natural aging.

Benefits of technology

This technology enables aluminum alloys to maintain sufficient hardness without heat treatment, avoiding heat treatment deformation and increased energy consumption, and reducing costs and CO2 emissions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117987695B_ABST
    Figure CN117987695B_ABST
Patent Text Reader

Abstract

This invention relates to aluminum alloys and methods for manufacturing the same. It provides aluminum alloys with inhibited natural aging and methods for manufacturing the same. The invention relates to an Al-Si aluminum alloy comprising Si, Mg, Mn, Fe, and unavoidable impurities, containing Al-Si-Mg-Fe-Mn compounds. Furthermore, the invention relates to a method for manufacturing this Al-Si aluminum alloy by controlling the cooling process of the alloy melt during casting.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to aluminum alloys and their manufacturing methods. Background Technology

[0002] Lightening automotive components can improve fuel economy and reduce energy consumption. Therefore, research is underway to replace the ferrous materials used in the past with aluminum or aluminum alloys.

[0003] For example, Patent Document 1 describes a high-strength aluminum alloy with excellent castability and machinability, characterized in that, when the total is set to 100% by mass, it contains 3.5% to 7.5% by mass of silicon (Si), 0.45% to 0.8% by mass of magnesium (Mg) and 0.05% to 0.35% by mass of chromium (Cr), with the balance consisting of aluminum (Al) and unavoidable impurities.

[0004] Patent document 2 describes an aluminum alloy plate characterized by being composed of an Al-Mg-Si aluminum alloy, having an endothermic peak of height a of 1.0 to 5.0 mW / g in a differential scanning calorimetry curve with a heating rate of 20°C / min in the temperature range of 150 to 230°C, and having more than two exothermic peaks in the temperature range of 230 to 270°C, wherein the ratio of the peak height b1 on the low-temperature side to the peak height b2 on the high-temperature side of the exothermic peak is b1 / b2 less than 0.80.

[0005] Prior art literature

[0006] Patent documents

[0007] Patent Document 1: Japanese Patent Application Publication No. 2010-18875

[0008] Patent Document 2: Japanese Patent Application Publication No. 2017-14541 Summary of the Invention

[0009] In existing technologies, additional heat treatments, such as solution heat treatment and / or aging heat treatment, are applied to cast aluminum alloys. These heat treatments induce the precipitation of Mg-Si precipitates in the aluminum alloy, which provide the required hardness for the component and inhibit natural aging. Therefore, in existing technologies, high strength is achieved by utilizing precipitates to increase the hardness of the aluminum alloy.

[0010] On the other hand, there are the following issues: the heat treatment process described above can cause deformation of the parts due to heat treatment deformation, and the cost increases due to the consumption of heat energy, and it can also lead to high CO2 emissions.

[0011] Therefore, the objective of this invention is to provide an aluminum alloy that suppresses natural aging. Furthermore, the objective of this invention is to provide a method for manufacturing an aluminum alloy that can produce an aluminum alloy with sufficient hardness even without a heat treatment process after casting.

[0012] The inventors have conducted various studies on methods for solving the aforementioned problems. As a result, the inventors discovered that by controlling the cooling process of the alloy melt during casting in the manufacture of aluminum alloy materials containing Si, Mg, Manganese (Mn), and Iron (Fe), it is possible to manufacture aluminum alloys that suppress natural aging and possess sufficient hardness, thus completing the present invention. It is believed that in the aluminum alloy of the present invention, by controlling the cooling process of the alloy melt during casting, Al-Si-Fe-Mn compounds preferentially precipitate, and the precipitation of Mg-Si compounds, which would previously precipitate, is suppressed.

[0013] That is, the main idea of ​​this invention is as follows.

[0014] (1) An Al-Si aluminum alloy comprising Si, Mg, Mn, Fe and unavoidable impurities, wherein the Al-Si aluminum alloy comprises Al-Si-Mg-Fe-Mn compounds.

[0015] (2) According to the Al-Si aluminum alloy described in (1), when the Al-Si aluminum alloy is observed with an 80μm×80μm field of view by EPMA mapping, in the Al-Si-Mg-Fe-Mn compound, the regions with K-α strength of Mg of Mg, Mn and Fe are consistent with the regions with K-α strength of 10% to 20% of Mn and K-α strength of 5% to 14% of Fe. The regions with K-α strength of Mn of Mn and Fe are consistent with the regions with K-α strength of 44% or more of Fe.

[0016] (3) A method for manufacturing an Al-Si aluminum alloy, comprising:

[0017] (i) Raw material preparation process, preparing raw materials of Al-Si aluminum alloy containing Si, Mg, Mn, Fe and unavoidable impurities;

[0018] (ii) Melt preparation process, which involves heating the raw materials prepared in (i) raw material preparation process to prepare alloy melt;

[0019] (iii) The pouring process involves pouring the alloy melt prepared in (ii) the melt preparation process into a mold; and

[0020] (iv) Cooling process, in which the molten alloy poured in (iii) is cooled to solidify.

[0021] (iv) The cooling process includes a solidification holding process in which the alloy melt is held at a temperature of 510°C to 470°C for 20 to 40 minutes.

[0022] According to the present invention, an aluminum alloy that suppresses natural aging can be provided. Furthermore, according to the present invention, a method for manufacturing an aluminum alloy that can produce an aluminum alloy with sufficient hardness even without a heat treatment process after casting can be provided. Attached Figure Description

[0023] Figure 1 The graph shows the Vickers hardness of the Al-Si aluminum alloys of Comparative Examples 1 and 2 and Examples 1 and 2 after casting and forced aging.

[0024] Figure 2 This is a diagram showing the EPMA mapping (80μm × 80μm) of the Al-Si aluminum alloy of Example 1.

[0025] Figure 3 This is a diagram showing the EPMA mapping (80 μm × 80 μm) of the Al-Si aluminum alloy of Comparative Example 1. Detailed Implementation

[0026] The preferred embodiments of the present invention will now be described in detail.

[0027] In this specification, the features of the invention are described with appropriate reference to the accompanying drawings. Furthermore, the aluminum alloy and its manufacturing method of the present invention are not limited to the following embodiments, and can be implemented in various ways that can be obtained by modifications and improvements made by those skilled in the art without departing from the spirit of the invention. Additionally, in the present invention, the expression "numerical value (lower limit) to numerical value (upper limit)" indicates a range including both the lower and upper limits.

[0028] This invention relates to an Al-Si aluminum alloy, which is an Al-Si aluminum alloy containing Si, Mg, Mn, Fe and unavoidable impurities, and contains Al-Si-Mg-Fe-Mn compounds.

[0029] The Si content is not limited. The Si content, based on the total mass of the Al-Si aluminum alloy, is typically 0.1% to 15% by mass, and in one embodiment, it is 4% to 12% by mass. Here, the Si content can be determined using ICP optical emission spectrometry.

[0030] The Mg content is not limited. The Mg content, based on the total mass of the Al-Si aluminum alloy, is typically 0.01% to 1% by mass, and in one embodiment, it is 0.1% to 1% by mass. Here, the Mg content can be determined by ICP emission spectroscopy.

[0031] The Mn content is not limited. The Mn content, based on the total mass of the Al-Si aluminum alloy, is typically 0.01% to 1% by mass, and in one embodiment, it is 0.1% to 1% by mass. Here, the Mn content can be determined using ICP emission spectroscopy.

[0032] The Fe content is not limited. The Fe content, based on the total mass of the Al-Si aluminum alloy, is typically 0.01% to 1% by mass, and in one embodiment, it is 0.1% to 1% by mass. Here, the Fe content can be determined by ICP emission spectroscopy.

[0033] The Al-Si aluminum alloy of the present invention may also appropriately contain other modifying alloying elements, such as those selected from copper (Cu), titanium (Ti), nickel (Ni), zirconium (Zr), cobalt (Co), molybdenum (Mo), tungsten (W), zinc (Zn), lithium (Li), silver (Ag), gallium (Ga), germanium (Ge), scandium (Sc), strontium (Sr), indium (In), vanadium (V), praseodymium (Pr), samarium (Sm), tantalum (Ta), gold (Au), beryllium (Be), chromium (Cr), and arsenic (As). One or more of the following metals (other metals): selenium (Se), yttrium (Y), niobium (Nb), ruthenium (Ru), rhodium (Rh), palladium (Pd), cadmium (Cd), tin (Sn), antimony (Sb), tellurium (Te), cerium (Ce), neodymium (Nd), promethium (Pm), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), lutetium (Lu), hafnium (Hf), rhenium (Re), iridium (Ir), platinum (Pt), mercury (Hg), bismuth (Bi), and thorium (Th).

[0034] The individual contents of other metals are not limited. The individual contents of other metals, based on the total mass of the Al-Si aluminum alloy, are typically 0.0001% to 0.1% by mass, and in one embodiment, 0.001% to 0.05% by mass. The total content of other metals, based on the total mass of the Al-Si aluminum alloy, is typically 0.01% to 1% by mass, and in one embodiment, 0.03% to 0.1% by mass, and in another embodiment, 0.04% to 0.06% by mass. Furthermore, the contents of other metals can be determined using methods known in the art, and may vary depending on the alloying element, but can be determined, for example, by ICP emission spectroscopy.

[0035] The remaining portion (balance) of the Al-Si aluminum alloy of the present invention, other than the aforementioned metals, consists of aluminum (Al) and unavoidable impurities.

[0036] Phosphorus (P) and sulfur (S) are unavoidable impurities. The content of phosphorus (P) and sulfur (S) is not limited. The individual content of phosphorus (P) and sulfur (S), based on the total mass of the aluminum alloy, is typically less than 0.01% by mass. Furthermore, the content of phosphorus (P) and sulfur (S) can be determined using methods known in this art, which may vary depending on the element being measured, but for example, it can be determined using ICP emission spectroscopy.

[0037] In the Al-Si aluminum alloys of the present invention, Al-Si-Mg-Fe-Mn compounds can be identified by EPMA mapping of Al-Si aluminum alloys. In the EPMA mapping of Al-Si aluminum alloys, Al-Si-Mg-Fe-Mn compounds have the following characteristics (i) and (ii).

[0038] (i) When observing Al-Si aluminum alloys with an 80 μm × 80 μm field of view by EPMA mapping, the regions with K-α strength of Mg of 50% or more, the regions with K-α strength of Mn of 10% or more (10% to 20% in one embodiment) and the regions with K-α strength of Fe of 5% or more (5% to 14% in one embodiment) are consistent.

[0039] (ii) When observing Al-Si aluminum alloys with an 80 μm × 80 μm field of view via EPMA mapping, the regions with a K-α strength of Mn of 50% or more (80% or more in one embodiment) and a K-α strength of Fe of 25% or more (44% or more in one embodiment) are consistent with each other.

[0040] Here, the intensity (%) of K-α of various metals at a specific location in an 80μm×80μm field of view, for example in the case of Mg, represents the proportion (%) of K-α rays of Mg from a specific location in that field of view when the K-α rays from the entire 80μm×80μm field of view are set to 100%.

[0041] Furthermore, the presence of Si in Al-Si-Mg-Fe-Mn compounds in Al-Si aluminum alloys can also be confirmed by EPMA, just like Mg, Mn, and Fe.

[0042] The shape of Al-Si-Mg-Fe-Mn compounds is not limited. The shapes of Al-Si-Mg-Fe-Mn compounds include, for example, spherical, polygonal, and blocky shapes.

[0043] The average particle size of Al-Si-Mg-Fe-Mn compounds is not limited. The average particle size of Al-Si-Mg-Fe-Mn compounds, calculated as the average of the equivalent circular diameters of 100 particles in a TEM image, is typically 30 nm to 300 nm, and in one embodiment, it is 50 nm to 100 nm.

[0044] The Vickers hardness of the Al-Si aluminum alloy of the present invention is not limited. The Vickers hardness of the Al-Si aluminum alloy of the present invention is typically 40 HV to 100 HV, and in one embodiment, it is 50 HV to 60 HV.

[0045] The Vickers hardness of the Al-Si aluminum alloy of the present invention after forced aging is not limited. The Vickers hardness of the Al-Si aluminum alloy of the present invention after forced aging (210°C × 90 minutes) is typically 50 HV to 120 HV, and in one embodiment, it is 50 HV to 60 HV.

[0046] In other words, the change in Vickers hardness of the Al-Si aluminum alloy of the present invention before and after forced aging, calculated as {|Vickers hardness after forced aging - Vickers hardness before forced aging| / Vickers hardness before forced aging}×100, is usually less than 4%, and in one embodiment, it is less than 2%.

[0047] Here, the Vickers hardness of the Al-Si aluminum alloy of the present invention can be determined by the Vickers hardness test.

[0048] Therefore, the natural aging of the Al-Si aluminum alloy of the present invention is suppressed. Moreover, for the Al-Si aluminum alloy of the present invention, various post-casting heat treatments are not required.

[0049] The Al-Si aluminum alloy of this invention is an Al-Si aluminum alloy casting. A casting refers to a shaped object manufactured by casting. Therefore, castings include shaped objects manufactured by low-pressure casting, gravity casting, die casting, etc.

[0050] The aluminum alloy in this invention is formed by casting, thereby enabling its use as a lightweight material to replace ferrous materials, such as automotive body parts.

[0051] The Al-Si aluminum alloy of the present invention can be manufactured using the processes (i) to (iv) described in detail below.

[0052] (i) Raw material preparation process

[0053] In process (i), the raw materials for Al-Si aluminum alloys are not limited. Various pure metals, compounds, alloys, etc., can be used as raw materials for Al-Si aluminum alloys. Aluminum ingots and aluminum scrap can be used as raw materials for aluminum. Furthermore, raw materials for Al-Si aluminum alloys can be in the form of powders, molten metals, or castings (e.g., aluminum alloy ingots). Moreover, metals with high melting points can generally be added in the form of a master alloy with other additive elements, while metals with low melting points can be added in the form of pure metals.

[0054] The composition of the raw materials for Al-Si aluminum alloys is adjusted so that the content of various metals in the Al-Si aluminum alloy obtained after manufacturing is within the range described above. Therefore, the composition of the raw materials for Al-Si aluminum alloys is the same as that of Al-Si aluminum alloys, as long as substances that are lost due to volatilization or other factors during manufacturing are not used as raw materials.

[0055] (ii) Melt preparation process

[0056] In step (ii), the alloy melt can be prepared, for example, by heating the raw material of Al-Si aluminum alloy in a melting furnace, such as an electric arc melting furnace, to a temperature at which a liquid phase is generated (typically 680°C to 1200°C, or 1000°C to 1200°C in one embodiment).

[0057] In step (ii), the order, method, temperature, time, and mixing method of adding aluminum and various metals, which are raw materials for Al-Si aluminum alloys, are not limited. In step (ii), the alloy melt is prepared in a manner that makes the various metals homogeneous.

[0058] For example, in step (ii) of the present invention, various metals are added to an aluminum melt prepared by heating aluminum to 680°C, and then the temperature of the melt is raised to the melting temperature of the alloy system, for example, 1000°C, to prepare an alloy melt.

[0059] (iii) Casting process

[0060] In step (iii), the mold is not limited. Molds known in this art can be used as molds.

[0061] (iv) Cooling process

[0062] In step (iv), the alloy melt is solidified by cooling. Step (iv) includes a solidification holding step. In the solidification holding step, when the temperature of the alloy melt during solidification reaches 510°C to 470°C (in one embodiment, 500°C to 480°C) at the start of solidification, it is held at this temperature range for 20 to 40 minutes (in one embodiment, for 30 minutes).

[0063] Furthermore, in step (iv), the cooling rate of the alloy melt is not limited. The cooling rate of the alloy melt is typically 50°C / second to 200°C / second, and in one embodiment, it is 80°C / second to 120°C / second.

[0064] In step (iv), by holding the alloy melt within the aforementioned specific temperature range for the aforementioned specific time, Al-Si-Mg-Fe-Mn compounds preferentially precipitate in the alloy melt, while the precipitation of Mg2Si is suppressed. Since Mg2Si can induce natural aging, the suppression of Mg2Si precipitation results in suppressed natural aging in the Al-Si aluminum alloy obtained after step (iv). Therefore, the Al-Si aluminum alloy obtained using the manufacturing method of the present invention can suppress hardness changes caused by aging.

[0065] In the method for manufacturing Al-Si aluminum alloys of the present invention, except for the solidification holding step in the cooling process (iv), casting, which is known in the art, can be used.

[0066] Here, casting refers to pouring molten metal (including alloys) that has been melted at high temperatures into the hollow part (mold cavity) of a mold made of sand, metal, etc., and then cooling and solidifying it.

[0067] As for casting, for example, the conventional melting casting or die casting methods include continuous casting, continuous casting rolling, semi-continuous casting (DC casting), hot-top casting, etc.

[0068] [Example]

[0069] The following describes several embodiments of the present invention, but it is not intended to limit the present invention to the solutions shown in such embodiments.

[0070] I. Sample preparation and hardness measurement

[0071] (i) Prepare raw materials for aluminum alloys containing the chemical composition described in Table 1.

[0072] (ii) The raw materials prepared in (i) are heated to 700°C to prepare an alloy melt.

[0073] (iii) The alloy melt prepared in the melt preparation process of (ii) is poured into the mold.

[0074] (iv) The alloy melt poured in the casting process in (iii) is cooled to a temperature of 520°C (Comparative Example 1), 500°C (Example 1), 480°C (Example 2), or 460°C (Comparative Example 2), and the temperature is maintained for 30 minutes once the alloy melt reaches the temperature.

[0075] (v) After the solidification and holding process in (iv), the mold is cooled to 250°C, the Al-Si aluminum alloy is removed from the mold, and further air-cooled to 25°C.

[0076] Furthermore, as a conventional Al-Si aluminum alloy, the cooling process in steps (iv) and (v) of the above-mentioned (i) to (v) was changed to "cooling the alloy melt poured in step (iii) to 400°C, removing the Al-Si aluminum alloy from the mold, and further air-cooling it to 25°C", thus manufacturing a conventional Al-Si aluminum alloy (Comparative Example 3).

[0077] Table 1. Content (mass%) of various components in the examples and comparative examples

[0078] No. Si Mg Fe Mn Cu Sr Zn Sn Ni Ti Al Example 1 9.03 0.27 0.11 0.42 0.01 0.001 0.005 0.01 0.01 0.01 margin Example 2 9.03 0.27 0.11 0.42 0.01 0.001 0.005 0.01 0.01 0.01 margin Comparative Example 1 9.03 0.27 0.11 0.42 0.01 0.001 0.005 0.01 0.01 0.01 margin Comparative Example 2 9.03 0.27 0.11 0.42 0.01 0.001 0.005 0.01 0.01 0.01 margin Comparative Example 3 9.18 0.28 0.15 0.35 0.01 0.001 0.004 0.01 0.01 0.01 margin

[0079] The Vickers hardness of each Al-Si aluminum alloy was measured.

[0080] The presence or absence of natural aging in Al-Si aluminum alloys can be confirmed by forced aging. Therefore, each Al-Si aluminum alloy with a Vickers hardness measured was then subjected to heat treatment (forced aging) at 210°C for 90 minutes.

[0081] The Vickers hardness of each Al-Si aluminum alloy after forced aging was measured again. The results are shown in Table 2 and... Figure 1 .

[0082] Table 2. Vickers hardness of the examples and comparative examples

[0083]

[0084] From Table 2 and Figure 1It can be seen that during the cooling process, Al-Si aluminum alloys held at 510℃~470℃, especially 500℃~480℃ for 20 minutes~40 minutes, and particularly 30 minutes, exhibit suppressed changes in Vickers hardness before and after forced aging. Therefore, it can be concluded that natural aging is suppressed in Al-Si aluminum alloys manufactured in this manner.

[0085] II. EPMA analysis of the samples

[0086] The Al-Si aluminum alloys of Example 1 and Comparative Example 1 were analyzed by EPMA.

[0087] Figure 2 The EPMA mapping (80 μm × 80 μm) of the Al-Si aluminum alloy of Example 1 is shown.

[0088] Figure 3 The EPMA mapping (80 μm × 80 μm) of the Al-Si aluminum alloy of Comparative Example 1 is shown.

[0089] from Figure 2 It can be seen that in the Al-Si aluminum alloy of Example 1, the peak positions of K-α rays of Si, Mg, Mn, and Fe are approximately consistent, indicating the precipitation of Al-Si-Mg-Fe-Mn compounds. Specifically, in the EPMA mapping of Mg, Mn, and Fe, within an 80 μm × 80 μm field of view, the regions where the K-α intensity of Mg is 50% or more, the regions where the K-α intensity of Mn is 10% or more, particularly 10% to 20%, and the regions where the K-α intensity of Fe is 5% or more, particularly 5% to 14%. Furthermore, in the EPMA mapping of Mn and Fe, within an 80 μm × 80 μm field of view, the regions where the K-α intensity of Mn is 50% or more, particularly 80% or more, and the regions where the K-α intensity of Fe is 25% or more, particularly 44% or more, are consistent.

[0090] On the other hand, from Figure 3 It can be seen that in the Al-Si aluminum alloy of Comparative Example 1, the peak positions of K-α rays of Si, Mg, Mn and Fe are inconsistent, and both Fe-Mn-Si compounds and Mg2Si compounds are precipitated.

[0091] Mg₂Si compounds, through heat treatment (aging treatment), cause a stable increase in hardness, endowing Al-Si aluminum alloys with the ability to suppress natural aging, thereby imparting the hardness required as a characteristic of aluminum alloys. In other words, when Mg₂Si compounds are present in an aluminum alloy, natural aging occurs without heat treatment, resulting in an increase in hardness. In the Al-Si aluminum alloy of the present invention, the precipitates are Al-Si-Mg-Fe-Mn compounds. That is, in the Al-Si aluminum alloy of the present invention, since the precipitation of Mg₂Si compounds is suppressed at temperatures below 200°C, natural aging caused by Mg₂Si compounds, i.e., an increase in hardness, does not occur. Therefore, the Al-Si aluminum alloy of the present invention does not require additional heat treatment, such as solution heat treatment and / or aging heat treatment, and as a result, the effects caused by heat treatment deformation can be suppressed, as well as the increase in cost and CO₂ emissions due to heat energy consumption can be suppressed.

Claims

1. An Al-Si aluminum alloy comprising Si: 4%~12% by mass, Mg: 0.1%~1% by mass, Mn: 0.1%~1% by mass, and Fe: 0.1%~1% by mass, with the remainder consisting of Al and unavoidable impurities, and the Al-Si aluminum alloy comprising Al-Si-Mg-Fe-Mn compounds. This Al-Si aluminum alloy is produced by the following manufacturing method, which includes: (i) Raw material preparation process, preparing raw materials of Al-Si aluminum alloy containing Si, Mg, Mn, Fe and unavoidable impurities; (ii) The melt preparation process involves heating the raw materials prepared in (i) the raw material preparation process to prepare the alloy melt; (iii) The casting process involves pouring the alloy melt prepared in (ii) the melt preparation process into a mold; and (iv) Cooling process, in which the molten alloy poured in (iii) is cooled to solidify. (iv) The cooling process includes a solidification holding process in which the alloy melt is held at a temperature of 510°C to 470°C for 20 to 40 minutes.

2. The Al-Si aluminum alloy according to claim 1, When observing Al-Si aluminum alloys in an 80μm×80μm field of view using EPMA mapping, in the Al-Si-Mg-Fe-Mn compound, the regions with K-α strength of Mg exceeding 50%, the regions with K-α strength of Mn exceeding 10%~20%, and the regions with K-α strength of Fe exceeding 5% are consistent. Similarly, the regions with K-α strength of Mn exceeding 80% and the regions with K-α strength of Fe exceeding 44% are consistent.

3. A method for manufacturing an Al-Si based aluminum alloy, The Al-Si aluminum alloy comprises Si: 4%~12% by mass, Mg: 0.1%~1% by mass, Mn: 0.1%~1% by mass, and Fe: 0.1%~1% by mass, with the remainder consisting of Al and unavoidable impurities. Furthermore, the Al-Si aluminum alloy comprises Al-Si-Mg-Fe-Mn compounds. The manufacturing method includes: (i) Raw material preparation process, preparing raw materials of Al-Si aluminum alloy containing Si, Mg, Mn, Fe and unavoidable impurities; (ii) The melt preparation process involves heating the raw materials prepared in (i) the raw material preparation process to prepare the alloy melt; (iii) The casting process involves pouring the alloy melt prepared in (ii) the melt preparation process into a mold; and (iv) Cooling process, in which the molten alloy poured in (iii) is cooled to solidify. (iv) The cooling process includes a solidification holding process in which the alloy melt is held at a temperature of 510°C to 470°C for 20 to 40 minutes.

Citation Information

Patent Citations

  • High strength aluminum alloy, method for producing high strength aluminum alloy casting, and method for producing high strength aluminum alloy member

    JP2010018875A

  • Aluminum alloy sheet inhibiting room temperature aging and excellent in galling curability

    JP2017014541A

  • Production method for aluminium alloys

    CN110564991A

  • Process for producing Al-Mg-Si alloy plate, Al-Mg-Si alloy plate and Al-Mg-Si alloy material

    CN1639373A