Antistatic flocculent sheet and preparation method thereof

Through the combination of hollow fiber, nylon fiber and low melting point fiber and the polyurethane adhesive connecting layer, combined with the heating and extrusion process, the problems of fiber damage and high adhesive cost are solved, and high performance, water resistance and comfort are achieved. Preparation of antistatic flakes.

CN118003726BActive Publication Date: 2024-10-18ZHEJIANG ZHONGCHAO NEW MATERIAL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410330115.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-22
Publication Date
2024-10-18
Estimated Expiration
2044-03-22

AI Technical Summary

Technical Problem

When preparing flakes with the existing technology, fiber materials are easily damaged during the mixing and carding process, and the acupuncture process consumes high energy and requires frequent maintenance. The cost of the binder is high and affects the softness and comfort of the flakes, and it is easy to be damaged after washing. Stratification occurs.

Method used

Hollow fiber and nylon fiber are used as the base layer and outer layer, and are connected through a coating layer of low melting point fiber and polyurethane binder. The connecting layer is formed through a spraying process, and antistatic flakes are prepared by combining heating and extrusion processes to reduce needle punching. process to improve fiber connection stability.

Benefits of technology

It achieves high bonding strength, good physical properties, comfort and water resistance of the flakes, reduces production costs, avoids the defects of the needle punching process, and improves the overall performance of the flakes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118003726B_ABST
    Figure CN118003726B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of flake generation, and relates to an antistatic flake and a preparation method thereof. The specific steps are as follows: after laying a base layer as the bottom layer, laying a connecting layer and an outer layer on the end surface of the base layer in turn, thereby forming a substrate to be processed, winding the base layer around a conveying roller group for heating and extruding a synthetic flake, sending the flake to air cooling and curing, and sending the cooled flake to storage, wherein the base layer comprises a base layer, an outer layer and a connecting layer, the base layer is formed by mixing and spinning a first hollow fiber and a first nylon fiber, the connecting layer comprises a low-melting-point fiber and a coating layer on the upper and lower end surfaces thereof, the coating layer is made of an adhesive, and the melting point of the coating layer is lower than the melting point of the low-melting-point fiber. The flake of the product of the invention reduces the needling process in production, and its performance is higher than that of the flake produced by the needling process, and the flake has good physical properties, comfort and strong water resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of flake generation, and more specifically, to an antistatic flake and a preparation method thereof. Background Art

[0002] At present, the spray-bonded cotton floss is made of short fibers as the main raw material. Fibers of various lengths, finenesses and functions are fully mixed, then combed into a net, and then stacked layer by layer to a certain thickness or weight, sprayed with adhesive, and heat treated.

[0003] Announcement No. CN112391738B, a thermal insulation flake with air lock function and its preparation method, by using modified three-dimensional curled hollow polyester fiber in combination with viscose fiber and ES fiber to prepare the thermal insulation flake, so that the three-dimensional curled hollow polyester fiber is used as the frame support structure, which ensures the three-dimensional structure of the thermal insulation flake and maintains the thermal insulation effect after laying the net. During the production process: the first step is to mix the viscose fiber, ES fiber and modified three-dimensional curled hollow polyester fiber evenly to obtain the fiber raw material; then the fiber raw material is opened twice and then sent to a carding machine for carding to form a fiber web; the second step is to rearrange the fiber web fibers using a random roller so that the fiber web fibers form a criss-cross cross structure; the third step is to send the treated fiber web fibers to a web laying machine for web laying to obtain fiber flakes; the fourth step is to pre-needle and under-needle the fiber flakes, and spray hydrogen peroxide on the surface of the fiber flakes during the needling process, and then slice them to obtain primary flakes; the fifth step is to send the primary flakes to a normal pressure plasma surface treatment cleaning machine for surface treatment, and then obtain warm flakes.

[0004] The above-mentioned prior art adopts a method of mixing and combing three kinds of fiber materials. In the actual process, the dynamic force of the combing machine is difficult to adjust the appropriate power due to the mixing of the three materials, so the fibers will be damaged during the combing process; secondly, a needle punching machine is used to needle the fiber flakes to improve their physical properties. This process has high energy consumption, especially the needle punching machine must be frequently inspected, maintained, and checked for any dropped needles falling into the flakes.

[0005] For example, announcement number CN109267231A discloses a method for preparing a multi-layered, high-density thermal insulation flakes, which comprises fully mixing ultrafine denier fibers and / or ultrafine denier shaped fibers, low-melting-point fibers with a melting point of 100 to 160°C, and ordinary fibers, and then performing opening and cleaning; combing the opened and cleaned fibers into sheets, and then heating them to 100 to 150°C, keeping them warm for 1 to 30 seconds, and performing single-layer heat setting to obtain sheet fibers; laying out multiple layers of sheet fibers into a web, and then heating them to 140 to 200°C, keeping them warm for 1 to 20 minutes, and performing overall heat setting, and cutting to obtain a multi-layered, high-density thermal insulation flakes.

[0006] The common point of the above two prior arts is that the mutual connection and fixation between different fibers are achieved through the thermal change characteristics of low-melting-point fibers. In the first prior art, the structural stability of the flakes is further improved by needle punching, and the stability of the second flakes is determined by the performance of its low-melting-point fibers.

[0007] Announcement No. CN115354443B discloses a production process of an antistatic cashmere flake, which adopts the steps of preparing conductive fibers, superimposing and compounding the conductive fibers and cashmere in order, wherein the conductive fibers form a conductive fiber layer, and the cashmere forms a cashmere layer; the cashmere layer is located between two conductive fiber layers, the conductive fiber layer and the cashmere layer are bonded by an adhesive, and the edges are trimmed to obtain an antistatic cashmere flake;

[0008] The prior art requires bonding with an adhesive, which is complex in structure and extremely expensive. Moreover, after the flakes are formed and solidified, their softness is reduced, affecting comfort. After being washed several times, gaps will appear at the bonding points between the conductive fiber layer and the cashmere layer in the flakes, forming a stratified phenomenon.

[0009] Therefore, our research unit needs a new method for preparing flakes, which does not require a needle punching process and can improve the stability of the connection between the fibers of the flakes. Summary of the invention

[0010] In view of the shortcomings of the prior art, the object of the present invention is to provide an antistatic flocculent sheet with stable structure and good warmth retention and a preparation method thereof.

[0011] To achieve the above object, the present invention provides the following technical solutions:

[0012] An antistatic flocculent sheet comprises a base layer, an outer layer covering the end surface of the base layer, and a connecting layer between the base layer and the outer layer to fix the two layers into shape.

[0013] The base layer is formed by mixing and spinning the first hollow fiber and the first nylon fiber, wherein the first hollow fiber accounts for 60wt% of the mixed fiber.

[0014] The outer layer is formed by mixing the second hollow fiber and the second nylon fiber, wherein the second nylon fiber accounts for 80wt% of the mixed fiber.

[0015] The connecting layer includes low melting point fiber and a coating layer on the upper and lower end surfaces thereof, wherein the coating layer is made of an adhesive.

[0016] The melting point of the coating layer is lower than the melting point of the low-melting-point fiber.

[0017] The present invention is further configured as follows: the coating layer and the low-melting-point fiber are connected by a spraying process, which comprises the following steps:

[0018] The low melting point fiber is stretched and unfolded by a traction machine, and a binder composed of a polyurethane solution is sprayed on its two end surfaces by a sprayer. During the spraying process, the ambient temperature is 15℃-20℃ and the humidity is 50%rh-65%rh.

[0019] The distance between the spray port of the sprayer and the low-melting-point fiber is 20cm-30cm, the pressure of the sprayer during spraying is 2-5bar, and finally it is cooled and solidified to form a connecting layer.

[0020] The present invention is further configured such that the coating layer is sprayed with a thickness of 50-80 microns.

[0021] A method for preparing an antistatic flake comprises the following steps:

[0022] S1. After paving the base layer as the bottom layer, a connecting layer and an outer layer are laid on the end surface thereof in sequence, thereby forming a base material to be processed;

[0023] S2, winding the substrate around a conveying roller set to heat and extrude the synthetic flakes,

[0024] S3, send the flakes to air-cooling and curing,

[0025] S4. The cooled flakes are sent to storage.

[0026] The present invention is further configured as follows: step S2 includes the following steps:

[0027] S21, the substrate first passes through a preheating roller set for preheating the substrate, wherein the temperature on the preheating roller set is 60° C.-80° C., and the preheating time is 5 min-10 min;

[0028] S22, the substrate is preheated and then enters the heating roller group. After the substrate enters the heating group, the heating group starts to heat the substrate from 110°C to 150°C. The heating process is staged, with each 10°C as a stage, and the heating time of each stage is maintained for 15-20 minutes.

[0029] The present invention is further configured as follows: in the step S22, four groups of heating roller groups are provided corresponding to each stage of 10°C, and the four groups of heating roller groups are arranged in a front-to-back order with four heating temperatures, namely 110°C-120°C, 120°C-130°C, 130°C-140°C, and 140°C-150°C.

[0030] The present invention is further configured as follows: in step S22, there is an infrared camera for real-time monitoring of the heating temperature state of the substrate;

[0031] Each heating roller group adjusts the heating temperature of its output through the temperature control system.

[0032] The present invention is further configured as follows: the temperature control system includes a PID controller and a temperature sensor, the temperature sensor transmits the temperature in the heating roller group to the PC end, and the PID controller adjusts the temperature of the heating roller group.

[0033] Compared with the shortcomings of the prior art, the beneficial effects of the present invention are:

[0034] The flakes of this product reduce the needling process in production, and its performance is higher than that of flakes produced by the needling process. In addition, the flakes have good physical properties, comfort and strong water resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 Schematic diagram of the bonding strength test of Example 1-Example 2;

[0036] Figure 2 Schematic diagram of the bonding strength test of sample 1 and sample 2;

[0037] Figure 3 It is a schematic diagram of water repellency test of the present invention;

[0038] Figure 4 It is a test schematic diagram of the elastic retraction of the present invention. DETAILED DESCRIPTION

[0039] Antistatic floccules: including a base layer, an outer layer covering the end surface of the base layer, and a connecting layer between the base layer and the outer layer to fix the two layers into shape. The base layer is made of a first hollow fiber and a first nylon fiber mixed and spun, wherein the first hollow fiber accounts for 60wt% of the mixed fiber; the outer layer is made of a second hollow fiber and a second nylon fiber mixed and spun, wherein the second nylon fiber accounts for 80wt% of the mixed fiber; the connecting layer includes low-melting-point fiber and a coating layer on the upper and lower end surfaces thereof, and the coating layer is made of a binder, which is polyurethane.

[0040] The melting point of the polyurethane constituting the coating layer is lower than that of the low-melting-point fiber. The polyurethane melting point is CRISVON 1836P series produced by DIC, with a viscosity of 350-500dPa.S and a melting point of 105-120℃; the low-melting-point fiber is 2D*51mm low-melting-point fiber produced by Hangzhou Huvis, with a melting point of 110℃-150℃.

[0041] The coating layer and the low melting point fiber are connected by a spraying process, which has the following steps:

[0042] Example 1: The low-melting point fiber is stretched and unfolded by a traction machine, and an adhesive composed of a polyurethane solution is sprayed on its two end surfaces by a sprayer. During the spraying process, the ambient temperature is 15°C, the humidity is 50% RH, the distance between the spray port of the sprayer and the low-melting point fiber is 20 cm, the pressure of the sprayer during spraying is 2 bar, the thickness of the coating layer sprayed is 50 microns, and finally it is cooled and solidified to form a No. 1 connecting layer.

[0043] Example 2: The low-melting point fiber is stretched and unfolded by a traction machine, and an adhesive composed of a polyurethane solution is sprayed on its two end surfaces by a sprayer. During the spraying process, the ambient temperature is 20°C, the humidity is 65% RH, the distance between the spray port of the sprayer and the low-melting point fiber is 30 cm, the pressure of the sprayer during spraying is 5 bar, the thickness of the coating layer sprayed is 80 microns, and finally it is cooled and solidified to form the second connecting layer.

[0044] Example 3: The low-melting point fiber is stretched and unfolded by a traction machine, and an adhesive composed of a polyurethane solution is sprayed on its two end surfaces by a sprayer. During the spraying process, the ambient temperature is 18°C, the humidity is 60% RH, the distance between the spray port of the sprayer and the low-melting point fiber is 25 cm, the pressure of the sprayer during spraying is 4 bar, the thickness of the coating layer sprayed is 70 microns, and finally it is cooled and solidified to form a No. 3 connecting layer.

[0045] Comparative Example 1: The low-melting point fiber is stretched and unfolded by a traction machine, and an adhesive composed of a polyurethane solution is sprayed on its two end surfaces by a sprayer. During the spraying process, the ambient temperature is 13°C, the humidity is 45% RH, the distance between the spray port of the sprayer and the low-melting point fiber is 18 cm, the pressure of the sprayer during spraying is 1.5 bar, the thickness of the coating layer sprayed is 40 microns, and finally it is cooled and solidified to form a No. 4 connecting layer.

[0046] Comparative Example 2: The low-melting point fiber is stretched and unfolded by a traction machine, and an adhesive composed of a polyurethane solution is sprayed on its two end surfaces by a sprayer. During the spraying process, the ambient temperature is 25°C, the humidity is 70% RH, the distance between the spray port of the sprayer and the low-melting point fiber is 32 cm, the pressure of the sprayer during spraying is 6 bar, the thickness of the coating layer sprayed is 90 microns, and finally it is cooled and solidified to form a No. 5 connecting layer.

[0047] A method for preparing an antistatic flake comprises the following steps:

[0048] S1. After the base layer is laid as the bottom layer, the connecting layer and the outer layer are laid on the end surface in turn to form the base material to be processed.

[0049] S2, winding the substrate around a conveying roller group to heat and extrude the synthetic flakes, specifically, the substrate first passes through a preheating roller group for preheating the substrate, wherein the temperature on the preheating roller group is 80° C., and the preheating time is 10 minutes;

[0050] After preheating, the substrate enters the heating roller group. After the substrate enters the heating group, the heating group starts to heat the substrate from 110°C to 150°C. The heating process adopts a staged heating method. Four groups of heating roller groups are set with each 10°C as a stage. The heating time of each stage is maintained for 15-20min. The four groups of heating roller groups are arranged in a front-to-back sequence with four heating stages, namely 110°C-120°C, 120°C-130°C, 130°C-140°C, and 140°C-150°C.

[0051] An infrared camera is installed outside the heating roller group to monitor the heating temperature of the substrate in real time, and each heating roller group adjusts the heating temperature output by the temperature control system. The temperature control system includes a temperature sensor and a PID controller, which makes real-time adjustments based on the temperature signal measured by the temperature sensor to ensure temperature stability. The infrared camera then takes the state of the substrate during the heating process to adjust the length of time the substrate is heated, that is, to adjust the heating time of the four stages to ensure that the temperature gradient is suitable for heating the substrate, thereby ensuring that the substrate is heated evenly.

[0052] During processing, since the melting point of polyurethane is lower than that of low-melting-point fiber, preheating is used to increase its activity. Then, when heated, the polyurethane melts first. After melting, when the heated roller rolls and extrude it, the molten solution will penetrate into the low-melting-point fiber, the base layer and the outer fiber layer. During this period, since the temperature rises in stages, the outer skin of the low-melting-point fiber will slowly melt and combine with the polyurethane. Moreover, as it is extruded, the polyurethane solution will adhere to the inner core of the low-melting-point fiber, promoting its connection with the outer layer and the base layer, thereby improving its structural strength.

[0053] S3. Send the flakes to air-cooled curing for 48 hours.

[0054] S4. The cooled flakes are sent to be cut and stored.

[0055] The No. 1 connecting layer was used as the raw material of the base material to form the experimental body one through the above-mentioned preparation method; the No. 2 connecting layer was used as the raw material of the base material to form the experimental body two through the above-mentioned preparation method; the No. 3 connecting layer was used as the raw material of the base material to form the experimental body three through the above-mentioned preparation method; the No. 4 connecting layer was used as the raw material of the base material to form the experimental body four through the above-mentioned preparation method; the No. 5 connecting layer was used as the raw material of the base material to form the experimental body five through the above-mentioned preparation method.

[0056] In combination with the prior art, the hollow fibers, nylon fibers and low-melting-point fibers of the present application are prepared using the technical means of the known announcement number CN112391738B, which specifically comprises the following steps: in the first step, the hollow fibers, nylon fibers and low-melting-point fibers are evenly mixed to obtain a fiber raw material; the fiber raw material is then opened twice and then fed into a carding machine for carding to form a fiber web; in the second step, the fiber web is rearranged using a random roller to form a criss-cross structure of the fiber web; in the third step, the treated fiber web is fed into a web laying machine for web laying to obtain fiber flakes; in the fourth step, the fiber flakes are pre-needled and under-needled, and then sliced ​​to obtain a comparison sample 1.

[0057] The hollow fiber, nylon fiber and low-melting point fiber of the present application are bonded using the technical means of known publication number CN115354443B, specifically, the hollow fiber and nylon fiber are bonded by the adhesive disclosed therein, thereby generating comparative sample 2.

[0058] Main performance index test

[0059] The samples generated by the above-mentioned Experimental Body 1 to Experimental Body 5 were tested, mainly including bonding strength, water repellency, and compression resilience. The results are as follows:

[0060] The test of bonding strength uses data obtained by tensile testing the flakes using a universal material testing machine.

[0061] like Figure 1 In the bonding strength test diagram shown:

[0062] The elongation of the first test piece reached 29.8%, and the breaking strength was 192.5Kpa;

[0063] The elongation of the second test piece reached 33.8%, and the breaking strength was 196.5Kpa;

[0064] The elongation of the experimental body 3 reached 32.4%, and the breaking strength was 205.3Kpa;

[0065] The elongation of the experimental body 4 reached 27.65%, and the fracture strength was 150.2Kpa;

[0066] The elongation of the experimental body 5 reached 36.8%, and the breaking strength was 150.2Kpa;

[0067] The fracture strength of the experimental body 3 is the highest. Figure 2 The data of Comparative Sample 1 and Comparative Sample 2 show that the use of a binder in the fiber can increase the elongation of the fiber, thereby improving its ductility. The fiber combination of the present application can achieve the effect of a high breaking strength of a needle punching process without a needle punching process.

[0068] According to GB / T24218.16, the hydrostatic pressure resistance of the flake material is measured. Figure 3 As shown:

[0069] The data of Experimental Body 1 to Experimental Body 5 of the present application are obviously higher than the data of Sample 1 and Comparative Sample 2.

[0070] According to FZ / T64006 test sample compression resilience, such as Figure 4 As shown:

[0071] The data of Experimental Body 1 to Experimental Body 5 of the present application are obviously higher than the data of Sample 1 and Comparative Sample 2.

[0072] Based on the experimental data of bonding strength, water repellency and compression resilience, Example 3 is the best choice for this application.

[0073] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Common changes and substitutions made by those skilled in the art within the scope of the technical solution of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing an antistatic flake, characterized in that: It includes a base layer, an outer layer covering the end surface of the base layer, and a connecting layer between the base layer and the outer layer to fix the two layers into shape. The base layer is formed by mixing and spinning the first hollow fiber and the first nylon fiber, wherein the first hollow fiber accounts for 60wt% of the mixed fiber. The outer layer is formed by mixing the second hollow fiber and the second nylon fiber, wherein the second nylon fiber accounts for 80wt% of the mixed fiber. The connecting layer includes low melting point fiber and a coating layer on the upper and lower end surfaces thereof, wherein the coating layer is made of an adhesive. The melting point of the coating layer is lower than the melting point of the low-melting-point fiber. The coating layer and the low-melting-point fiber are connected by a spraying process, which has the following steps: the low-melting-point fiber is stretched and unfolded by a tractor, and a binder composed of a polyurethane solution is sprayed on its two end surfaces by a sprayer, and the ambient temperature during the spraying process is 15°C-20°C and the humidity is 50%rh-65%rh. The distance between the spray port of the sprayer and the low melting point fiber is 20cm-30cm, the pressure of the sprayer during spraying is 2-5bar, and finally it is cooled and solidified to form a connecting layer. The thickness of the coating layer sprayed is 50-80 microns. S1. After paving the base layer as the bottom layer, a connecting layer and an outer layer are laid on the end surface thereof in sequence, thereby forming a base material to be processed; S2, the substrate is wound around a conveying roller group to be heated and extruded into a flake, S3, send the flakes to air-cooling and curing, S4, the cooled flakes are sent to storage; S21, the substrate first passes through a preheating roller set for preheating the substrate, wherein the temperature on the preheating roller set is 80° C. and the preheating time is 10 minutes. S22, the substrate is preheated and then enters the heating roller group. After the substrate enters the heating group, the heating group starts to heat the substrate from 110°C to 150°C. The heating process is staged, with four groups of heating rollers set at 10°C per stage. The heating time of each stage is maintained at 15-20 minutes.

2. A method for preparing an antistatic flake according to claim 1, characterized in that: In the step S22, four groups of heating rollers are provided at each stage of 10°C. The four groups of heating rollers are arranged in a front-to-back order with four heating temperatures, namely 110°C-120°C, 120°C-130°C, 130°C-140°C, and 140°C-150°C.

3. A method for preparing an antistatic flake according to claim 2, characterized in that: In step S22, an infrared camera is used to monitor the heating temperature of the substrate in real time; Each heating roller group adjusts its output heating temperature through a temperature control system.

4. A method for preparing an antistatic flake according to claim 3, characterized in that: The temperature control system includes a PID controller and a temperature sensor. The temperature sensor transmits the temperature in the heating roller group to the PC end, and the PID controller adjusts the temperature of the heating roller group.

Citation Information

Patent Citations

  • Multilayer and high-density heat insulation wadding sheet and preparation method thereof

    CN109267231A

  • A heat-insulating wadding with air-locking function and its preparation method

    CN112391738B

  • A production process for antistatic cashmere wadding

    CN115354443B

  • Heat-insulating material special for clothes, bedding and sleeping-bag, etc.

    CN1130697A

  • Quilt core filler capable of conducting moisture directionally

    CN216733282U