Composition for non-curing waterproof coating, non-curing waterproof coating and preparation method and application thereof
By using a combination of hydrogenated asphalt, synthetic rubber and wax-containing additives, the problem of poor compatibility between asphalt and high-temperature-resistant wax in non-cured waterproof coatings is solved, and the low-temperature flexibility, heat resistance and water channeling resistance of the coating are improved. , ensuring its stability and bonding performance over a wide temperature range.
Patent Information
- Application Number
- CN202311819832.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-27
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-12-27
AI Technical Summary
The existing non-curing waterproof coatings have delamination due to poor compatibility between asphalt and high-temperature-resistant wax, which affects their low-temperature flexibility, heat resistance and water channeling resistance.
A combination of hydrogenated asphalt, synthetic rubber, plasticizers and wax-containing additives is used to improve the compatibility of the composition through specific preparation methods and process conditions, including hydrogenating the asphalt in an organic solvent and using The nickel-palladium-cerium oxide composite catalyst controls the degree of hydrogenation and the proportion of the composition to ensure uniform mixing of each component.
It solves the delamination problem of non-cured waterproof coatings, significantly improves low-temperature flexibility, heat resistance, extensibility and water channeling resistance, and ensures the stability and bonding performance of the coating in a wide temperature range.
Smart Images

Figure BDA0004633671880000081 
Figure BDA0004633671880000101 
Figure BDA0004633671880000111
Abstract
Description
Technical Field
[0001] The invention relates to the field of building waterproofing, and in particular to a composition for a non-curing waterproof coating, a non-curing waterproof coating, and a preparation method and application thereof. Background Art
[0002] Non-curing waterproof coatings are widely used in various new construction or maintenance waterproofing projects. They can be used for waterproofing of conventional parts as well as special parts such as expansion joints. The main ingredients are plasticizers, asphalt, rubber, and high temperature resistant wax.
[0003] Among them, high temperature resistant wax is an anti-high temperature auxiliary agent, which ensures that the non-curing waterproof coating still has a certain cohesive force in a high temperature environment. After the composite roll material, it ensures that the roll material will not be dislocated, offset or fall off in a high temperature environment.
[0004] However, since asphalt is a high-polarity material and high-temperature resistant wax is a low-polarity material, the two have poor direct compatibility and are prone to stratification, resulting in uneven distribution of materials inside the non-curing waterproof coating. The upper layer of the material has poor low-temperature flexibility due to the floating of the high-temperature resistant wax, and the lower layer has poor high-temperature resistance due to the lack of high-temperature resistant wax, thus affecting the stability of the non-curing waterproof coating.
[0005] For example, CN115141547A discloses a non-curing waterproof coating, comprising the following components: softening oil, modified wax powder, thermoplastic elastomer, resin, silane coupling agent and filler. The main purpose is to utilize the grafted groups on the modified wax powder in the composition to react with other components containing unsaturated double bonds to improve the compatibility of the modified wax powder in the system.
[0006] Therefore, it is of great significance to develop a new non-curing waterproof coating. Summary of the invention
[0007] The purpose of the present invention is to overcome the problems of the non-curing waterproof coating in the prior art, such as the delamination phenomenon, the inability to balance the high and low temperature performance, and the poor elongation and water penetration resistance.
[0008] In order to achieve the above-mentioned object, the first aspect of the present invention provides a composition for a non-curing waterproof coating, the composition comprising hydrogenated asphalt, synthetic rubber, a plasticizer and a wax-containing additive;
[0009] Based on the total weight of the composition, the content of the hydrogenated asphalt is 40-60wt%, the content of the synthetic rubber is 5-15wt%, the content of the plasticizer is 20-40wt%, and the content of the wax-containing additive is 5-15wt%;
[0010] The hydrogenated asphalt is prepared by a method comprising the following steps: in the presence of an organic solvent, introducing the asphalt into a reactor equipped with a nickel-palladium-cerium oxide composite catalyst for hydrogenation treatment; the conditions of the hydrogenation treatment include: a temperature of 280-350° C., a pressure of 4-8 MPa, a volume ratio of hydrogen to asphalt of 1200-1800:1, and a mass space velocity of 0.05-0.3 h -1 .
[0011] The second aspect of the present invention provides a method for preparing a non-curing waterproof coating, which is carried out using the components in the composition for non-curing waterproof coating described in the first aspect, comprising: in a reactor,
[0012] (S1) preheating and mixing a plasticizer and hydrogenated asphalt to obtain material I;
[0013] (S2) performing a first stirring mixing of the material I and the synthetic rubber to obtain a material II;
[0014] (S3) The material II and the wax-containing additive are subjected to a second stirring and mixing process to obtain the non-curing waterproof coating.
[0015] The third aspect of the present invention provides a non-curing waterproof coating prepared by the method for preparing a non-curing waterproof coating according to the second aspect.
[0016] The fourth aspect of the present invention provides the use of the non-curing waterproof coating described in the third aspect in the field of building waterproofing.
[0017] Through the above technical solution, the present invention has at least the following advantages:
[0018] (1) The delamination phenomenon of non-curing waterproof coatings has been solved, the compatibility of various raw materials has been improved, the low-temperature flexibility, heat resistance, elongation, self-healing and anti-water penetration performance of non-curing waterproof coatings have been significantly improved, and the performance of non-curing waterproof coatings has been comprehensively improved.
[0019] (2) Ensure that the non-curing waterproof coating does not crack when the ambient temperature is between -25 and 75°C, and after being compounded with the roll material, it can firmly adhere to the roll material on both the vertical and inclined surfaces to prevent the roll material from falling off. DETAILED DESCRIPTION
[0020] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0021] In the present invention, unless otherwise specified, room temperature means 25±2°C.
[0022] As mentioned above, the first aspect of the present invention provides a composition for a non-curing waterproof coating, the composition comprising hydrogenated asphalt, synthetic rubber, a plasticizer and a wax-containing additive;
[0023] Based on the total weight of the composition, the content of the hydrogenated asphalt is 40-60wt%, the content of the synthetic rubber is 5-15wt%, the content of the plasticizer is 20-40wt%, and the content of the wax-containing additive is 5-15wt%;
[0024] The hydrogenated asphalt is prepared by a method comprising the following steps: in the presence of an organic solvent, introducing the asphalt into a reactor containing a nickel-palladium-cerium oxide composite catalyst (hereinafter referred to as the first reactor for distinction) for hydrogenation treatment; the conditions of the hydrogenation treatment include: a temperature of 280-350° C., a pressure of 4-8 MPa, a volume ratio of hydrogen to asphalt of 1200-1800:1, and a mass space velocity of 0.05-0.3 h -1 .
[0025] According to a preferred embodiment, the conditions of the hydrogenation treatment are controlled so that the degree of hydrogenation of the obtained hydrogenated asphalt is 70-85%.
[0026] The hydrogenation degree of the hydrogenated asphalt is calculated by the following formula:
[0027] Degree of hydrogenation % = [1 - (content of unsaturated bonds in hydrogenated asphalt after hydrogenation / content of unsaturated bonds in raw asphalt before hydrogenation)] × 100%.
[0028] It should be noted that the content of the unsaturated bonds can be detected by conventional methods in the art, for example, by UV / visible spectroscopy or nuclear magnetic resonance.
[0029] Preferably, the reactor (ie the first reactor) is a fixed bed catalytic reactor.
[0030] Preferably, the needle penetration of the asphalt is 60-100 and the softening point is 40°C-60°C.
[0031] More preferably, the asphalt is selected from at least one of coal tar asphalt, petroleum asphalt and natural asphalt.
[0032] Preferably, the organic solvent is selected from at least one of cyclohexane and carbon tetrachloride.
[0033] More preferably, the volume ratio of the asphalt to the organic solvent is 1:4-6.
[0034] The method for preparing hydrogenated asphalt of the present invention can also be pre-treated by various means known in the art, and the present invention has no special requirements for this. For example, direct dissolution can be used. Exemplarily, the present invention may include: directly adding the organic solvent to a stirred tank at room temperature to dissolve the asphalt. This article will not go into details here, and those skilled in the art should not be understood as limiting the present invention.
[0035] It should be noted that the method for preparing hydrogenated asphalt of the present invention can also be post-processed by various means known in the art, and the present invention has no special requirements for this, for example, condensation, distillation, etc. can be used. Exemplarily, the present invention may include condensing the mixture obtained after the hydrogenation step, and then performing solvent recovery treatment, and the remaining solid obtained is the hydrogenated asphalt of the present invention, which will not be described in detail herein, and those skilled in the art should not be understood as limiting the present invention.
[0036] The inventors of the present invention have found that when the hydrogenated asphalt obtained by the method of the present invention is used to prepare a non-curing waterproof coating, the raw materials will not delaminate, and the low-temperature flexibility, heat resistance, elongation, self-healing and water penetration resistance of the non-curing waterproof coating are significantly improved.
[0037] According to a preferred embodiment, the nickel-palladium-cerium oxide composite catalyst is prepared by a method comprising the following steps:
[0038] (1) mixing a cerium oxide carrier with a bipyridine derivative containing a hydroxyl group to obtain a carrier material I;
[0039] (2) The support material I is contacted and mixed with a metal source solution to obtain the nickel-palladium-cerium oxide composite catalyst.
[0040] Preferably, the weight ratio of the cerium oxide carrier to the bipyridine derivative containing hydroxyl groups is 500:2-5. The inventors of the present invention have found that, in this preferred case, the nickel-palladium-cerium oxide composite catalyst provided by the present invention can improve the hydrogenation degree of the hydrogenated asphalt.
[0041] Preferably, the metal source solution contains nickel and palladium in a molar ratio of 1:0.4-0.6. The inventors of the present invention have found that, in this preferred case, the nickel-palladium-cerium oxide composite catalyst provided by the present invention can improve the hydrogenation degree of the hydrogenated asphalt.
[0042] Preferably, the specific surface area of the cerium oxide carrier is 2-5m 2 / g, pore volume of 0.2-0.5mL / g, columnar. The inventors of the present invention have found that, in this preferred case, the nickel-palladium-cerium oxide composite catalyst provided by the present invention can improve the hydrogenation degree of the hydrogenated asphalt.
[0043] Preferably, the bipyridine derivative containing a hydroxyl group is selected from at least one of 4'-hydroxy-2,2':6',2"-terpyridine and 2,2'-bipyridine-4,4'-dicarboxylic acid. The inventors of the present invention have found that, in this preferred case, the nickel-palladium-cerium oxide composite catalyst provided by the present invention can improve the hydrogenation degree of the hydrogenated asphalt.
[0044] Preferably, the amount of the metal source solution is 10-80 mL relative to 10 g of the carrier material I.
[0045] Preferably, the nickel element concentration in the metal source solution is 0.01-0.1 mol / L, and the palladium element concentration is 0.004-0.06 mol / L.
[0046] Preferably, in step (1) and step (2), the conditions of the mixing reaction and the contact mixing are the same or different, and each independently includes: a temperature of 30-50° C. and a time of 20-28 h.
[0047] It should be noted that, in step (1), in order to obtain the support material I, the bipyridine derivative containing a hydroxyl group may be dissolved in the organic solvent. For example, the organic solvent may be ethanol or ether, and the amount of the organic solvent added is mainly to control the amount of the organic solvent added to completely dissolve the bipyridine derivative containing a hydroxyl group. This article will not go into details here, and those skilled in the art should not be construed as limiting the present invention.
[0048] Preferably, in step (1), a first drying is performed after the mixing reaction to obtain the carrier material I.
[0049] Preferably, in step (2), after the contact mixing, second drying, calcination and activation treatment are sequentially performed to obtain the nickel-palladium-cerium oxide composite catalyst.
[0050] Preferably, the conditions of the first drying and the second drying are the same or different, and independently include: a temperature of 40-100° C. and a time of 1-10 h.
[0051] Preferably, the calcination conditions include: 400-500° C., and time of 4-8 h.
[0052] It should be noted that the activation treatment can be carried out by methods known in the art. For example, the activation treatment can be carried out by heating in a hydrogen atmosphere to reduce the oxide to a metal. This article will not go into details and those skilled in the art should not understand it as a limitation of the present invention.
[0053] The method for preparing the nickel-palladium-cerium oxide composite catalyst in the present invention can also be carried out by a pretreatment method known in the art, and the present invention has no special requirements for this. For example, the cerium oxide carrier can be heat-treated to remove surface impurities and adsorbates. The present invention has no special requirements for process parameters such as the temperature of the heat treatment, which will not be repeated herein, and those skilled in the art should not be understood as limiting the present invention.
[0054] Preferably, the synthetic rubber is at least one of styrene-isoprene-styrene rubber and styrene-butadiene-styrene rubber.
[0055] Particularly preferably, the synthetic rubber is styrene-butadiene-styrene rubber; further preferably, the melt index of the styrene-butadiene-styrene rubber at 200° C. and 5 kg is 0.01-2 g / 10 min.
[0056] Preferably, the plasticizer is selected from at least one of cycloparaffinic oil, polyisobutylene with a number average molecular weight not higher than 5000, polybutadiene with a number average molecular weight not higher than 5000, aromatic oil, and waste engine oil.
[0057] Particularly preferably, the plasticizer is selected from a plasticizer having a kinematic viscosity of 100-300 m at 40°C. 2 / s of cyclohexane oil.
[0058] Preferably, the wax-containing additive is selected from at least one of polyethylene wax, Fischer-Tropsch wax, and polypropylene wax with a number average molecular weight not higher than 20,000.
[0059] As mentioned above, the second aspect of the present invention provides a method for preparing a non-curing waterproof coating, which is carried out using the components in the non-curing waterproof coating composition described in the first aspect, comprising: in a reactor (hereinafter referred to as the second reactor for distinction),
[0060] (S1) preheating and mixing a plasticizer and hydrogenated asphalt to obtain material I;
[0061] (S2) performing a first stirring mixing of the material I and the synthetic rubber to obtain a material II;
[0062] (S3) The material II and the wax-containing additive are subjected to a second stirring and mixing process to obtain the non-curing waterproof coating.
[0063] Preferably, the reactor (ie the second reactor) is a planetary stirred tank.
[0064] Preferably, in step (S1), the preheating mixing condition is to raise the temperature of the material I to 160-200°C.
[0065] Preferably, in step (S2), the first stirring and mixing conditions include a temperature of 160-200°C.
[0066] Preferably, in step (S3), the second stirring and mixing conditions include a temperature of 150-180°C.
[0067] Preferably, in step (S2), the first stirring and mixing time is 1.5-3 hours.
[0068] Preferably, in step (S3), the second stirring and mixing time is 0.5-1.5 h.
[0069] The present invention has no special requirements on the stirring speeds of the first stirring and mixing and the second stirring and mixing, and they can be selected according to stirring speeds known in the art.
[0070] As mentioned above, the third aspect of the present invention provides a non-curing waterproof coating prepared by the method for preparing a non-curing waterproof coating described in the second aspect.
[0071] As mentioned above, the fourth aspect of the present invention provides the use of the non-curing waterproof coating described in the third aspect in the field of building waterproofing.
[0072] The present invention will be described in detail below by way of examples. In the following examples, unless otherwise specified, all raw materials and instruments used are commercially available, and the specific sources of the raw materials are shown in Table 1.
[0073] Table 1
[0074]
[0075] The model information of some instruments used in the following examples is as follows:
[0076] Fixed bed catalytic reactor, model SW-Q2, purchased from Tianjin Zhongke Research Technology Co., Ltd.;
[0077] The planetary stirred tank, model TX-J-2, was purchased from Taiyi (Shanghai) Industrial Co., Ltd.
[0078] The A series preparation examples of the present invention are used to prepare nickel-palladium-cerium oxide composite catalysts.
[0079] The cerium oxide supports used in the following examples were all heat-treated before being mixed with the bipyridine derivatives containing hydroxyl groups. The heat-treatment conditions included a temperature of 100° C. and a time of 2 h.
[0080] Preparation Example A1
[0081] (1) mixing a cerium oxide carrier with a bipyridine derivative containing a hydroxyl group (dissolved in ethanol) for reaction, and drying the mixture obtained after the mixing reaction at 60° C. for 10 h to obtain a carrier material I;
[0082] (2) The carrier material I is contacted and mixed with the metal source solution, the mixture obtained after the contact and mixing is dried at 60° C. for 5 h and then calcined at 450° C. for 6 h, and the calcined sample is heated in a hydrogen atmosphere to obtain a nickel-palladium-cerium oxide composite catalyst.
[0083] Unless otherwise specified, the remaining preparation examples were carried out by referring to the method of Preparation Example A1, except that the raw materials and process parameters used in each preparation example were different, and the details are shown in Table 2.
[0084] Table 2
[0085] Preparation Example A1 Preparation Example A2 Step (1) Cerium oxide support type Ceria Support I Ceria Support II Dosage / g 100g Same as Preparation Example A1 Bipyridine derivatives containing hydroxyl groups / g 0.5 Same as Preparation Example A1 Mixed reaction Temperature / ℃ 40 Same as Preparation Example A1 Time / h 24 Same as Preparation Example A1 Step (2) Carrier material I / g 80 Same as Preparation Example A1 Metal source solution Nickel concentration (mol / L) 0.02 Same as Preparation Example A1 Palladium concentration (mol / L) 0.01 Same as Preparation Example A1 Anions in metal source solution <![CDATA[NO3 - ]]> Same as Preparation Example A1 Dosage / mL 80 Same as Preparation Example A1 Contact Mixing Temperature / ℃ 40 Same as Preparation Example A1 Time / h 24 Same as Preparation Example A1 Nomenclature of nickel-palladium-cerium oxide composite catalyst Catalyst A1 Catalyst A2
[0086] The B series preparation examples of the present invention are used to prepare hydrogenated asphalt.
[0087] Preparation Example B1
[0088] At room temperature, an organic solvent (cyclohexane) is added to a stirred tank to dissolve asphalt (petroleum asphalt), and the dissolved asphalt is introduced into a fixed bed catalytic reactor equipped with a nickel-palladium-cerium oxide composite catalyst for hydrogenation treatment. The mixture obtained after the hydrogenation treatment step is condensed, and the cyclohexane is recovered. The remaining solid is the hydrogenated asphalt.
[0089] The conditions of the hydrotreatment are shown in Table 3.
[0090] Unless otherwise specified, the remaining preparation examples were carried out according to the method of Preparation Example B1, except that the raw materials and process parameters used in each preparation example were different, and the details are shown in Table 3.
[0091] Table 3
[0092]
[0093] Unless otherwise specified, the amounts of raw materials used in the following examples are all parts by weight, and each part by weight represents 1 g.
[0094] Example 1
[0095] (S1) preheating and mixing a plasticizer and hydrogenated asphalt in a planetary stirred tank to obtain material I;
[0096] (S2) mixing the material I and the synthetic rubber to obtain a material II;
[0097] (S3) The material II and the wax-containing additive are subjected to a second stirring and mixing process to obtain a non-curing waterproof coating T1.
[0098] Unless otherwise specified, the remaining examples are carried out in accordance with the method of Example 1, except that the raw materials and process parameters used in each example are different, and the specific details are shown in Table 4.
[0099] Table 4
[0100]
[0101] Comparative Example 4
[0102] Comparative Example 4 was carried out in accordance with the method of Example 1, except that 50 parts by weight of hydrogenated asphalt B1 in Example 1 was replaced with 25 parts by weight of hydrogenated asphalt and 25 parts by weight of petroleum asphalt to prepare a non-curing waterproof coating D-T4.
[0103] Comparative Example 5
[0104] Comparative Example 5 was carried out in accordance with the method of Example 1, except that the hydrogenated asphalt B1 in Example 1 was replaced with an equal weight portion of petroleum asphalt to prepare a non-curing waterproof coating D-T5.
[0105] Test Case
[0106] After the waterproof coating in the above example is discharged and canned and cooled, the upper 1 / 4 sample and the lower 1 / 4 sample are taken respectively, and the lowest limit low temperature flexibility, the highest limit heat resistance, elongation, self-healing and water penetration resistance of the samples are tested respectively according to the reference standard JC / T 2428-2017 "Non-curing rubber asphalt waterproof coating". The test results are shown in Table 5.
[0107] Table 5
[0108]
[0109]
[0110] From the results in Table 5, it can be seen that there are differences in the low-temperature flexibility and heat resistance performance in the comparative example, and the delamination phenomenon is obvious. The low-temperature flexibility, heat resistance, elongation, self-healing property, and anti-water channeling performance of the non-curing waterproof coating prepared by the present invention are all improved, and the delamination phenomenon of the non-curing waterproof coating is solved, and the performance of the non-curing waterproof coating is comprehensively improved.
[0111] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A non-curing waterproof coating composition, characterized in that: The composition contains hydrogenated asphalt, synthetic rubber, plasticizer and wax-containing additive; Based on the total weight of the composition, the content of the hydrogenated asphalt is 40-60wt%, the content of the synthetic rubber is 5-15wt%, the content of the plasticizer is 20-40wt%, and the content of the wax-containing additive is 5-15wt%; The synthetic rubber is at least one of styrene-isoprene-styrene rubber and styrene-butadiene-styrene rubber; The hydrogenated asphalt is prepared by a method comprising the following steps: in the presence of an organic solvent, introducing asphalt into a reactor equipped with a nickel-palladium-cerium oxide composite catalyst for hydrogenation treatment; the needle penetration of the asphalt is 60-100, and the softening point is 40°C-60°C; the conditions of the hydrogenation treatment include: a temperature of 280-350°C, a pressure of 4-8MPa, a volume ratio of hydrogen to asphalt of 1200-1800:1, and a mass space velocity of 0.05-0.3h -1 ; The degree of hydrogenation of the hydrogenated asphalt is 70-85%.
2. The non-curing waterproof coating composition according to claim 1, wherein The plasticizer is selected from at least one of cycloparaffin oil, polyisobutylene with a number average molecular weight not higher than 5000, polybutadiene with a number average molecular weight not higher than 5000, aromatic oil, and waste engine oil.
3. The non-curing waterproof coating composition according to claim 1, wherein The wax-containing additive is selected from at least one of polyethylene wax, Fischer-Tropsch wax, and polypropylene wax with a number average molecular weight not higher than 20,000.
4. A method for preparing a non-curing waterproof coating, characterized in that: The method is carried out using the components of the non-curing waterproof coating composition according to any one of claims 1 to 3, comprising: in a reactor, (S1) preheating and mixing the plasticizer and hydrogenated asphalt to obtain material I; (S2) performing a first stirring mixing of the material I and the synthetic rubber to obtain a material II; (S3) The material II and the wax-containing additive are subjected to a second stirring and mixing process to obtain the non-curing waterproof coating.
5. The method according to claim 4, wherein: The reactor is a planetary stirred tank.
6. The method according to claim 4 or 5, wherein: In step (S1), the preheating and mixing conditions are to raise the temperature of the material I to 160-200°C; And / or, in step (S2), the first stirring and mixing conditions include a temperature of 160-200°C; And / or, in step (S3), the second stirring and mixing condition includes a temperature of 150-180°C.
7. A non-curing waterproof coating prepared by the method for preparing a non-curing waterproof coating according to any one of claims 4 to 6.
8. Use of the non-curing waterproof coating according to claim 7 in the field of building waterproofing.