A full penetration welding process without root clearing for H-shaped structural parts

By processing V-shaped grooves and multi-layer multi-pass welding on H-shaped structural parts, combined with hydrogen elimination treatment, full penetration and unclear root welding is achieved, which solves the problems of long time consumption and pollution of traditional welding processes and improves welding efficiency. and quality.

CN118023651BActive Publication Date: 2024-10-18CHINA TIESIJU CIVIL ENGINEERING GROUP CO LTD +3
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410191698.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-21
Publication Date
2024-10-18
Estimated Expiration
2044-02-21

AI Technical Summary

Technical Problem

The welding process of traditional H-shaped structural parts requires root cleaning, which results in high requirements for workers, long time consumption, and the generation of dust and noise pollution, which affects the welding environment.

Method used

The full penetration and rootless welding process is used to process V-shaped grooves on the wings and webs of the H-shaped structural parts, combined with multi-layer and multi-pass welding and hydrogen elimination treatment to reduce the risk of welding deformation and cracks, and use solid welding wire. Welding with gantry-type twin-wire submerged arc welding eliminates the root cleaning step.

Benefits of technology

It significantly saves welding time, improves welding efficiency and quality, reduces dust and noise pollution, and is suitable for the production of H-shaped structural parts in bridges, ships and other industries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118023651B_ABST
    Figure CN118023651B_ABST
Patent Text Reader

Abstract

The invention belongs to the field of welding technology, and specifically relates to a full penetration and non-root cleaning welding process for an H-shaped structural member, comprising the following steps: step 1, preparation and web; both ends of the web steel plate are processed with single-sided V-shaped grooves, the groove angle is 40°±2°, no blunt edge is left at the root, and the assembly surface is closely fitted; step 2, positioning welding; step 3, formal welding: including root base welding on the slope side, filling welding on the slope side, cover surface on the ungrooved side and cover surface on the groove side; step 4, post-weld inspection; the welding process of the invention has fewer steps, no root cleaning is required, and about one-third of the time is saved, and the comprehensive welding process combines manual welding and automatic welding of equipment, can better balance welding quality and welding efficiency, and the process can obtain a higher production speed under the premise of ensuring excellent joint performance; it can be used for the production and manufacturing of H-shaped structural members in industries such as bridges, ships, and buildings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of structural component welding, and in particular relates to a full penetration welding process without root clearing of an H-shaped structural component. Background Art

[0002] A bridge project uses assembled I-shaped composite beams with a standard span of 50m. The main steel materials of the I-shaped composite beams are low-alloy high-strength steels of Q355D and Q420D, with a maximum plate thickness of 50mm. For the welding of thick steel plates that are highly sensitive to hydrogen-induced cracking, effective and feasible welding process measures must be taken in a targeted manner during manufacturing to ensure welding quality. Because there are a large number of H-shaped structural parts with full penetration welds on the bridge, the traditional welding process is to clean the roots (shovel the roots) after the initial layer of welding to keep the welds in good condition to ensure high-quality welds during subsequent full penetration welding. However, the root cleaning process has high requirements for workers' operation, which often leads to a long time for root cleaning, and the dust and noise generated by root cleaning will pollute the on-site welding environment.

[0003] Therefore, it is necessary to provide an improved technical solution to address the above-mentioned deficiencies in the prior art. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a full penetration welding process without root clearing for H-shaped structural parts.

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] A full penetration welding process without root clearing of H-shaped structural parts comprises the following steps:

[0007] Step 1, prepare two flange steel plates as flanges of the H-shaped structural member, and prepare a web steel plate as the web of the H-shaped structural member; both ends of the web steel plate are processed with a single-sided V-shaped groove, the groove angle is 40°±2°, no blunt edge is left at the root, and the assembly surface is closely fitted;

[0008] Step 2, positioning welding: assemble the two wing plate steel plates and the web plate steel plate horizontally into an H shape, and fix them by spot welding on the groove surface to initially form an H-shaped structural component as a whole;

[0009] Step 3: Formal welding: including the following steps:

[0010] Step 3.1, base welding: arrange two welders to weld in the same direction from the first end and the middle to the second end of the H-shaped structural member; use solid wire gas shielded welding at the root of the groove to perform base welding of the root weld on the slope side. The quality of the base weld should be guaranteed, with a certain penetration depth without welding through, and the back side should be bright red; weld in the flat position;

[0011] Step 3.2, filling: arrange two welders to weld in the same direction from the first end and the middle of the H-shaped structural member to the second end; use trolley-type single-wire submerged arc welding to fill the groove and weld in the flat welding position;

[0012] Step 3.3, side cover without groove: Use gantry double-wire submerged arc welding to weld the side cover without groove; welding in ship-shaped position, the inclination angle of H-shaped structural parts on the gantry double-wire submerged arc welding machine is 62°~65°;

[0013] Step 3.4, groove side cover: Use gantry type double wire submerged arc welding to cover the groove side, fill the groove, and weld a weld leg, and weld in the ship-shaped position; the inclination angle of the H-shaped structural part on the gantry type double wire submerged arc welding machine is 30°~45°;

[0014] Step 4: Post-weld inspection.

[0015] Furthermore, in step 2, after the reverse deformation is preset, the groove surface is spot welded and fixed. The welding of the positioning weld should avoid welding at the end, and the arc pit should be filled. Solid wire gas shielded welding is used, and the welding points are evenly arranged on the groove side. The thickness of the positioning weld is the same as the thickness of the formal base weld, the length is not less than 50mm, and the spacing is 500-600mm.

[0016] Furthermore, the positioning welding in step 2 and the base welding in step 3.1 both use CO2 solid wire gas shielded welding, the wire diameter is φ1.2mm, the welding current is 240~260A, the voltage is 28~32V, the gas flow rate is 20~25L / min, and the welding speed is 25~35cm / min.

[0017] Furthermore, the diameter of the welding wire of the trolley-type single-wire submerged arc welding in step 3.2 is φ5.0 mm, the welding current is 600-650 A, the voltage is 31-32 V, and the welding speed is 40 cm / min.

[0018] Furthermore, the welding wire diameter of the gantry double-wire submerged arc welding in step 3.3 and step 3.4 is φ5.0mm, the front welding wire is reversely connected to DC, the welding current is 950A, and the voltage is 32V; the rear welding wire is an AC power supply, the welding current is 800A, and the voltage is 35V; the front welding wire and the rear welding wire are in the same molten pool and move synchronously, the welding speed is 75cm / min, and the total welding heat input is 96KJ / cm.

[0019] Furthermore, in step 3.3 and step 3.4, the front welding wire is inclined forward by 12 degrees, and the rear welding wire is vertical; on a straight line longitudinally distributed between the lower ends of the front welding wire and the rear welding wire, the spacing between the front welding wire and the rear welding wire is 21 mm to 22 mm.

[0020] Furthermore, in step 3.3 and step 3.4, the gantry type double-wire submerged arc welding uses H10Mn2 welding wire and SJ101 flux, and the flux is baked at 350° C. for 2 hours before use.

[0021] Furthermore, the thickness of the wing plate steel plate is 30 mm to 60 mm, and the thickness of the web plate steel plate is 18 mm to 20 mm.

[0022] Furthermore, the full penetration welding process without root clearing of the H-shaped structural parts adopts multi-layer and multi-pass welding, one pass for each layer, preheating before welding, the preheating temperature is not less than 100°C, and the interlayer temperature is 150-200°C;

[0023] The weld should be dehydrogenated immediately after completion. The heating temperature of the dehydrogenation treatment is 200-250°C, the insulation time is 1.5min / 1mm-2.0min / 1mm, and not less than 1h, and then slowly cooled to room temperature.

[0024] Furthermore, the appearance inspection of the weld in step 4 should be carried out after cooling to ambient temperature, and the weld surface should not have defects such as surface pores, slag inclusions, cracks and arc scratches;

[0025] The weld leg size should not be less than 1 / 4 of the web steel plate thickness t, and should not be greater than 10mm. The height difference of the weld surface should be within the range of 0 to 1.5mm; and ultrasonic testing should be carried out 24 hours after welding.

[0026] The beneficial effects of the present invention are:

[0027] The welding process of the present invention has fewer steps and does not require root cleaning, which saves about one-third of the time. The comprehensive welding process combines manual welding and automatic welding with equipment, which can better balance welding quality and welding efficiency. The process can achieve a higher production speed while ensuring excellent joint performance. It can be used for the production and manufacturing of H-type structural parts in industries such as bridges, ships, and buildings. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. Among them:

[0029] Figure 1 Schematic diagram of the groove structure of an embodiment of the present invention.

[0030] Figure 2 Schematic diagram of weld bead arrangement according to an embodiment of the present invention.

[0031] Figure 3 Schematic diagram of welding direction according to an embodiment of the present invention.

[0032] Figure 4 Schematic diagram of a bottom weld according to an embodiment of the present invention.

[0033] Figure 5 Schematic diagram of a filling weld according to an embodiment of the present invention.

[0034] Figure 6 Schematic diagram of the cover weld on the ungrooved side of an embodiment of the present invention.

[0035] Figure 7 Schematic diagram of the groove side cover weld according to an embodiment of the present invention.

[0036] Figure 8 The figure is a schematic diagram of the arrangement of the front welding wire and the rear welding wire of the double-wire submerged arc welding according to an embodiment of the present invention.

[0037] Fig. 9 The weld leg size and the height difference requirements of the weld surface of the embodiment of the present invention.

[0038] Fig.10 Schematic diagram of a turning fixture for an H-shaped structural member according to an embodiment of the present invention.

[0039] In the figure: 1-base weld, 2-filling weld, 3-ungrooved side cover weld, 4-grooved side cover weld, 5-turnover fixture. DETAILED DESCRIPTION

[0040] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present invention.

[0041] In the description of the present invention, the terms "longitudinal", "lateral", "upper", "lower", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings. They are only for the convenience of describing the present invention and do not require that the present invention must be constructed and operated in a specific orientation. Therefore, they should not be understood as limitations on the present invention. The terms "connected" and "connected" used in the present invention should be understood in a broad sense. For example, they can be fixed connections or detachable connections; they can be directly connected or indirectly connected through intermediate components. For ordinary technicians in this field, the specific meanings of the above terms can be understood according to specific circumstances.

[0042] The present invention will be described in detail below with reference to the accompanying drawings and in combination with embodiments. It should be noted that the embodiments and features in the embodiments of the present invention can be combined with each other without conflict.

[0043] For the assembled I-shaped composite beam introduced in the background technology of the present invention, effective and feasible welding process measures must be taken in a targeted manner during manufacturing to ensure the welding quality.

[0044] Targeted measures include:

[0045] 1) Optimize process design, select small angle groove form, reduce welding welding filling amount, and control welding deformation;

[0046] 2) Set anti-deformation and pre-place welding shrinkage deformation allowance:

[0047] For H-shaped components, the upper and lower flange plates are pre-processed for anti-deformation to reduce welding angle deformation. At the same time, longitudinal deformation and transverse shrinkage allowances are pre-considered for different plate thicknesses, different cross-sections, and different groove forms;

[0048] 3) Prevent welding cracks:

[0049] (1) Control of interlayer temperature during preheating and welding: The welding process of the present invention adopts multi-layer and multi-pass welding, with one pass for each layer, a total of wire passes, preheating before welding, the preheating temperature is not less than 100°C, the interlayer temperature is 150-200°C, and post-welding heat measures;

[0050] (2) Measures to prevent welding cracks:

[0051] Select welding materials with low sulfur and phosphorus content and high manganese content; reduce sulfur and phosphorus segregation in weld metal, improve the shape of some crystals, and enhance thermal cracking resistance;

[0052] Control welding process parameters and conditions. The root welding of the weld is the starting point of thick plate welding. It is the foundation for ensuring the quality of the weld. It is also a sensitive area for cracks. Therefore, the welding measures at the root of the weld must be carried out with great care:

[0053] Control the cooling rate of weld metal between 800℃-500℃ (t8 / 5 value): During thick plate welding, the heat affected zone of the weld is cooled quickly, and coarse-grained martensite structure is most likely to form during the crystallization process, which makes the steel brittle during welding and increases the tendency of cold cracks. Therefore, during thick plate welding, t8 / 5 must be strictly controlled; that is, the cooling time from 800℃ to 500℃ in the heat affected zone of the weld, especially at the fusion line of the weld, is controlled, that is, the t8 / 5 value;

[0054] After welding, the weld is dehydrogenated (H) treated to reduce the H content in the weld, which will play a great role in reducing the occurrence of cold cracks. The dehydrogenation treatment should be carried out immediately after the weld is completed. The heating temperature of the dehydrogenation treatment should reach 200-250℃, the holding time is 1.5min / 1mm-2.0min / 1mm, and not less than 1h, and then slowly cooled to room temperature.

[0055] For a bridge project in the background technology of the present invention, since there are a large number of H-shaped structural members with full penetration of the main body welds, the total root cleaning time is relatively long. In order to achieve the purpose of full penetration without root cleaning, the present invention proposes a full penetration and no root cleaning welding process for H-shaped structural members, comprising the following steps:

[0056] Step 1: prepare two flange steel plates as flanges of the H-shaped structural member, and prepare a web steel plate as the web of the H-shaped structural member; Figure 1 As shown, both ends of the web plate are processed with a single-sided V-shaped groove, the groove angle is 40°±2°, no blunt edge is left at the root, and the assembly surface is closely fitted; closely fitting can be understood as the assembly gap with the wing plate steel plate is less than 1mm (excluding 1mm), the purpose is to ensure the penetration effect and the welding quality;

[0057] Step 2, positioning welding: assemble the two wing plate steel plates and the web plate steel plate horizontally into an H shape, and fix them by spot welding on the groove surface to initially form an H-shaped structural component as a whole;

[0058] Step 3: Formal welding: including the following steps:

[0059] Step 3.1, base welding: arrange two welders (welder A and welder B) to weld in the same direction from the first end and the middle of the H-shaped structural member to the second end respectively; use solid welding wire gas shielded welding to perform base welding of the root weld on the slope side at the root of the groove, and the quality of the base weld should be guaranteed. The present invention is somewhat different from the single-sided welding and double-sided forming of the butt weld. The base welding of the present invention has a certain penetration depth on the basis of no welding penetration, and the back side is bright red; welding in the flat welding position; Figure 4 is a schematic diagram of a base weld, in which a base weld 1 is marked;

[0060] Step 3.2, filling: arrange two welders (welder A and welder B) to weld in the same direction from the first end and the middle of the H-shaped structural member to the second end; use trolley-type single-wire submerged arc welding to fill the groove and weld in the flat welding position; Figure 3 The welding direction is schematically drawn in FIG. Figure 5 is a schematic diagram of a filling weld bead, in which a filling weld bead 2 is marked;

[0061] Step 3.3, ungrooved side cover (key weld): Use gantry double-wire submerged arc welding for ungrooved side cover; the welding sequence is from one end of the H-shaped structure to the other end; welding in the ship-shaped position, the inclination angle of the H-shaped structure on the gantry double-wire submerged arc welding machine is 62°~65°; Figure 6 Schematic diagram of the cover weld on the ungrooved side, in which the cover weld 3 on the ungrooved side is marked;

[0062] Step 3.4, groove side cover: Use gantry type double wire submerged arc welding to cover the groove side, fill the groove, and weld a weld leg; the welding order is from one end of the H-shaped structure to the other end; welding in the ship-shaped position; the inclination angle of the H-shaped structure on the gantry type double wire submerged arc welding machine is 30°~45°; Figure 2 and Figure 7 The schematic diagram of the weld bead arrangement after welding is completed, in which the groove side cover weld bead 4 is marked;

[0063] Step 4: Post-weld inspection: The weld leg size and the height difference of the weld surface should meet the Fig. 9 As shown:

[0064] Step 3.3, the cover surface on the ungrooved side is the key weld, and the quality must be guaranteed during operation; the first weld (base weld) on the front side is not welded through, and only partial penetration is guaranteed; the cover surface on the ungrooved side is the reverse side (ungrooved side) weld, and the reverse side weld is needed to melt to the front base weld to achieve full penetration.

[0065] The present invention does not require root cleaning, thus eliminating the root cleaning process and the base welding process after root cleaning in the traditional 6 processes, reducing the process to 4 processes, saving about one-third of the time, and improving the welding efficiency while ensuring the welding quality.

[0066] Furthermore, in step 2, before positioning welding, the welding area and the surrounding 30 mm range should be polished and cleaned to remove grease, rust and other impurities that may affect the welding quality;

[0067] After preset reverse deformation, spot weld and fix it on the groove surface. Avoid welding at the end of the tack weld and fill the arc pit. Use solid wire gas shielded welding and evenly arrange the welding points on the groove side.

[0068] The thickness of the positioning weld is the same as the thickness of the formal base weld, the length is not less than 50mm, and the spacing is 500-600mm.

[0069] Further, the positioning welding in step 2 and the backing welding in step 3.1 are both performed by CO2 solid wire gas shielded welding, the wire diameter is φ1.2mm, the welding current is 240-260A, the voltage is 28-32V, the gas flow rate is 20-25L / min, and the welding speed is 25-35cm / min;

[0070] The diameter of the welding wire for the trolley-type single-wire submerged arc welding in step 3.2 is φ5.0 mm, the welding current is 600-650 A, the voltage is 31-32 V, and the welding speed is 40 cm / min;

[0071] The diameter of the welding wire for the gantry double-wire submerged arc welding in step 3.3 and step 3.4 is φ5.0mm, the front welding wire is reversely connected with DC, the welding current is 950A, and the voltage is 32V; the rear welding wire is an AC power supply, the welding current is 800A, and the voltage is 35V; the front welding wire and the rear welding wire are in the same molten pool and move synchronously, the welding speed is 75cm / min, and the total welding heat input is 96KJ / cm;

[0072] The welding process parameters of each weld are shown in Table 1:

[0073] Table 1 Welding process parameters

[0074]

[0075]

[0076] Furthermore, Figure 8 As shown, in step 3.3 and step 3.4, the front welding wire is inclined forward by 12° and the rear welding wire is vertical; on a straight line longitudinally distributed between the lower ends of the front welding wire and the rear welding wire, the spacing between the front welding wire and the rear welding wire is 21 to 22 mm.

[0077] Furthermore, in step 3.3 and step 3.4, the gantry type double-wire submerged arc welding uses H10Mn2 welding wire and SJ101 flux, and the flux is baked at 350° C. for 2 hours before use.

[0078] Furthermore, the thickness of the wing plate steel plate is 30 mm to 60 mm, and the thickness of the web plate steel plate is 18 mm to 20 mm.

[0079] Furthermore, the appearance inspection of the weld in step 4 should be carried out after cooling to ambient temperature. There should be no defects such as surface pores, slag inclusions, cracks and arc scratches on the weld surface, otherwise they must be removed and re-welded;

[0080] The weld leg size should not be less than 1 / 4 of the web steel plate thickness t, and should not be greater than 10mm. The height difference of the weld surface should be within the range of 0 to 1.5mm; and ultrasonic testing should be carried out 24 hours after welding.

[0081] like Fig.10 As shown, it is a schematic diagram of the turning fixture of the H-shaped structural member of the present invention. The turning fixture 5 is composed of a plurality of detachable sub-components, and the sub-components are detachably fixed by bolts or pins. A plurality of D40mm diameter lifting holes are opened on the turning fixture 5.

[0082] Comparative Example

[0083] The present invention sets three comparative examples, and the thickness of the web steel plate in each comparative example is 18 mm. The length of the blunt edge of the groove, the groove angle or some processes in the three comparative examples are different from those of the present invention; Table 2 is a table of main process parameters of the embodiments of the present invention and the comparative examples; Table 3 is a table of tensile and impact test results of weld metals of the embodiments of the present invention and the comparative examples:

[0084] Table 2 Process parameters of the embodiments of the present invention and the comparative examples

[0085]

[0086]

[0087] Table 3 is a table of the tensile and impact test results of the weld metals of the embodiments of the present invention and the comparative examples.

[0088]

[0089] It should be noted that the qualified rate in Table 3 is the qualified rate of experimental parts. In actual production, the qualified rate of welding should be slightly lower than 100%.

[0090] It can be seen from the test results in the above table that the process of this embodiment can meet the requirements of the standard and can be used for welding assembled I-shaped composite beams.

[0091] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention are within the scope of protection of the pending claims of the present invention.

Claims

1. A full penetration welding process without root clearing for H-shaped structural parts. It is characterized in that The following steps are involved: Step 1, prepare two wing plate steel plates as the wing plates of the H-shaped structural member, and prepare a web plate steel plate as the web plate of the H-shaped structural member; the thickness of the wing plate steel plate is 30mm-60mm, and the thickness of the web plate steel plate is 18mm-20mm; both ends of the web plate steel plate are processed with a single-sided V-shaped groove, the groove angle is 40°±2°, no blunt edge is left at the root, and the assembly surface is closely attached; closely attached means that the assembly gap between the web plate steel plate and the wing plate steel plate is less than 1mm; Step 2, positioning welding: assemble the two wing plate steel plates and the web plate horizontally into an H shape, and fix them by spot welding on the groove surface to initially form an H-shaped structural component as a whole; Step 3: Formal welding: including the following steps: Step 3.1, base welding: arrange two welders to weld in the same direction from the first end and the middle to the second end of the H-shaped structural member; use solid wire gas shielded welding at the root of the groove to perform base welding of the root weld on the slope side. The quality of the base weld should be guaranteed, with a certain penetration depth without welding through, and the back side should be bright red; weld in the flat position; Step 3.2, filling: arrange two welders to weld in the same direction from the first end and the middle of the H-shaped structural member to the second end; use trolley-type single-wire submerged arc welding to fill the groove and weld in the flat welding position; the wire diameter of the trolley-type single-wire submerged arc welding is φ5.0mm, the welding current is 600-650A, the voltage is 31-32V, and the welding speed is 40cm / min; Step 3.3, side cover without groove: Use gantry double-wire submerged arc welding to weld the side cover without groove; welding in ship-shaped position, the inclination angle of H-shaped structural parts on the gantry double-wire submerged arc welding machine is 62°~65°; Step 3.4, groove side cover: Use gantry type double wire submerged arc welding to cover the groove side, fill the groove, and weld a weld leg, and weld in the ship-shaped position; the inclination angle of the H-shaped structural part on the gantry type double wire submerged arc welding machine is 30°~45°; Step 4: Post-welding inspection; Among them, the positioning welding in step 2 and the base welding in step 3.1 are both made of CO 2 Solid wire gas shielded welding, wire diameter is φ1.2mm, welding current is 240~260A, voltage is 28~32V, gas flow is 20~25L / min, welding speed is 25~35cm / min; The welding wire diameter of the gantry double-wire submerged arc welding in step 3.3 and step 3.4 is φ5.0mm, the front welding wire is reversely connected to DC, the welding current is 950A, and the voltage is 32V; the rear welding wire is an AC power supply, the welding current is 800A, and the voltage is 35V; the front welding wire and the rear welding wire are in the same molten pool and move synchronously, the welding speed is 75cm / min, and the total welding heat input is 96KJ / cm.

2. The full penetration welding process without root clearing of H-shaped structural parts according to claim 1, Features: In step 2, after preset reverse deformation, the groove surface is spot welded and fixed. The welding of the positioning weld should avoid welding at the end, and the arc pit should be filled. Use solid wire gas shielded welding, and the welding spots are evenly arranged on the groove side. The thickness of the positioning weld is the same as the thickness of the formal base weld, the length is not less than 50mm, and the spacing is 500-600mm.

3. The full penetration welding process without root clearing of H-shaped structural parts according to claim 1, Features: In step 3.3 and step 3.4, the front welding wire is inclined forward by 12° and the rear welding wire is vertical; on a straight line longitudinally distributed between the lower ends of the front welding wire and the rear welding wire, the spacing between the front welding wire and the rear welding wire is 21 mm to 22 mm.

4. The full penetration welding process without root clearing of H-shaped structural parts according to claim 1, Features: In step 3.3 and step 3.4, the gantry type double-wire submerged arc welding uses H10Mn2 welding wire and SJ101 flux, and the flux is baked at 350°C for 2 hours before use.

5. The full penetration welding process without root clearing of H-shaped structural parts according to claim 1, Features: The H-shaped structural parts are welded by a full penetration welding process without root clearing, with multi-layer and multi-pass welding, one pass for each layer, preheating before welding, the preheating temperature is not less than 100°C, and the interlayer temperature is 150-200°C; The weld should be dehydrogenated immediately after completion. The heating temperature of the dehydrogenation treatment is 200-250°C, the insulation time is 1.5min / 1mm-2.0min / 1mm, and not less than 1h, and then slowly cooled to room temperature.

6. The full penetration welding process without root clearing of H-shaped structural parts according to claim 1, Features: The visual inspection of the weld in step 4 should be carried out after cooling to ambient temperature. There should be no surface pores, slag inclusions, cracks and arc scratch defects on the weld surface; The weld leg size should not be less than 1 / 4 of the web steel plate thickness t, and should not be greater than 10mm. The height difference of the weld surface should be within the range of 0 to 1.5mm; and ultrasonic testing should be carried out 24 hours after welding.

Citation Information

Patent Citations

  • T, L type heavy-plate joint fusion-penetration welding method

    CN101491855A

  • Full penetration fillet weld back-gouging-free welding technology

    CN104259634A

  • H-steel or T-steel full-penetration back-gouging-free welding method

    CN104625357A

  • Full-penetration and root-removing-free welding method for T-section steel

    CN108788410A

  • Full penetration gouging-free I-shaped steel welding method introducing welding pre-deformation

    CN114192944A