Acid-alkali resistant inorganic composite ink and preparation method thereof

By preparing acid- and alkali-resistant inorganic composite inks and using ingredients such as modified acrylate emulsion and modified fluorescein, the problem of insufficient adhesion and flame retardancy of acrylic inks is solved, and high adhesion, durability and flame retardancy are achieved. The unique ink improves the fluorescence performance and light stability.

CN118027743BActive Publication Date: 2024-10-18佛山市西泰陶瓷科技有限公司
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410349057.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-26
Publication Date
2024-10-18
Estimated Expiration
2044-03-26

AI Technical Summary

Technical Problem

Acrylate water-based inks have low adhesion fastness, slow drying rate, poor friction resistance, and insufficient flame retardant properties on substrates such as films and aluminum foils, which limits their promotion in the field of green printing. The fluorescent properties of the amino derivatives of fluorescein Not good, modification methods are needed to improve its overall performance.

Method used

Develop an acid and alkali resistant inorganic composite ink, using modified acrylate emulsion, modified fluorescein, inorganic pigments, inorganic nanopowders, surfactants, preservatives, driers and auxiliary solvents, through specific formula ratios and Process steps are used to prepare the ink with excellent adhesion, durability, acid and alkali resistance and flame retardancy.

Benefits of technology

It improves the adhesion firmness, durability, acid and alkali resistance and flame retardant properties of the ink, enhances the fluorescence performance and light stability, and improves the comprehensive performance in the field of anti-counterfeiting detection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004759345260000031
    Figure BDA0004759345260000031
  • Figure BDA0004759345260000032
    Figure BDA0004759345260000032
  • Figure BDA0004759345260000051
    Figure BDA0004759345260000051
Patent Text Reader

Abstract

The invention discloses an acid- and alkali-resistant inorganic composite ink, relates to the field of ink, and includes the following raw materials by weight: 10-15 parts of modified acrylic emulsion, 8-10 parts of modified fluorescein, 10-20 parts of inorganic pigment, 10-20 parts of inorganic nanopowder, 0.3-0.5 parts of surfactant, 0.2-0.4 parts of preservative, 2-3 parts of drying agent, 8-10 parts of auxiliary solvent, 5-10 parts of ammonia water and 50-60 parts of deionized water. Chloroether resin has excellent adhesion, durability and acid and alkali resistance, nano silicon dioxide enhances mechanical properties, polyphosphate flame retardant and plasticizes acrylic emulsion, and improves the adhesion firmness, durability, acid and alkali resistance and flame retardant properties of composite ink. The active groups in the modified fluorescein produce hydrogen bonds or covalent crosslinking with hydroxyl and carboxyl groups in the modified acrylic emulsion, giving the composite ink stable fluorescence characteristics, good heat resistance and light stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of ink, and in particular to an acid- and alkali-resistant inorganic composite ink and a preparation method thereof. Background Art

[0002] Acrylic resin has good film-forming properties, and the surface printing ink prepared by it has high gloss and good color development. It is also widely used as an adhesive material in the ink industry. Acrylic ester inks are mostly used for paper printing and are also used in the field of anti-counterfeiting. When used on substrates such as films and aluminum foils, they have defects such as low adhesion, slow drying rate and poor friction resistance. In addition, the flame retardant properties of acrylates are insufficient, and the additive flame retardants have defects such as poor compatibility with polymers and easy migration, which limits their promotion in the field of green printing. Therefore, it is necessary to develop a suitable modification method to improve the comprehensive performance of acrylic ester water-based inks.

[0003] Fluorescein, commonly used in acrylic anti-counterfeiting fluorescent inks, is an aromatic compound with carboxyl and hydroxyl groups. It is the matrix of the luminescent substance and a highly fluorescent substance with a high extinction coefficient, excitation and emission wavelengths in the visible light region, high fluorescence quantum yield, non-toxicity, and low cost. Fluorescein and its derivatives have excellent fluorescence properties and other photochemical and physical properties. However, since aminofluorescein is connected to an aromatic group, its fluorescence quantum yield and derivatization ability are reduced. In order to improve the fluorescence properties of aminofluorescein and enhance its responsiveness and photostability, it is urgent to develop a new type of fluorescent molecule to improve the comprehensive performance of acrylic anti-counterfeiting fluorescent inks in the field of anti-counterfeiting detection. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides an acid- and alkali-resistant inorganic composite ink and a preparation method thereof.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] An acid-base resistant inorganic composite ink comprises the following raw materials in parts by weight: 10-15 parts of modified acrylic emulsion, 8-10 parts of modified fluorescent pigment, 10-20 parts of inorganic pigment, 10-20 parts of inorganic nano powder, 0.3-0.5 parts of surfactant, 0.2-0.4 parts of preservative, 2-3 parts of drying agent, 8-10 parts of auxiliary solvent, 5-10 parts of ammonia water and 50-60 parts of deionized water;

[0007] The inorganic pigment is titanium dioxide;

[0008] The inorganic nano powder is a mixture of nano zinc oxide and nano silicon nitride in a mass ratio of 1:2;

[0009] The surfactant is one or more of polyoxyethylene lauryl ether, Tween 20 and Tween 40 mixed in a certain proportion;

[0010] The preservative is phenol;

[0011] The drying agent is a mixture of ethanol and isopropanol in a mass ratio of 1:1;

[0012] The auxiliary solvent is one or more of ethylene glycol, propylene glycol, glycerol and 1,4-butanediol mixed in a certain proportion;

[0013] The modified acrylic ester emulsion is prepared by the following steps:

[0014] Step A1: Add hydroxyethyl acrylate and anhydrous ethanol into a flask, slowly drop 3-aminopropyltrimethoxysilane at 25°C under nitrogen protection, raise the temperature to 75-85°C after the dropwise addition, stir and react for 48 hours, and vacuum dry at 50°C to obtain intermediate 1, wherein the amount ratio of hydroxyethyl acrylate, anhydrous ethanol and 3-aminopropyltrimethoxysilane is 0.2-0.25 mol:100 mL:0.1 mol;

[0015] During the reaction, hydroxyethyl acrylate and 3-aminopropyltrimethoxysilane undergo Michael addition reaction to generate intermediate 1. The structure of intermediate 1 is shown below:

[0016]

[0017] Step A2: Add allyl phosphine dichloride (CAS No. 1498-47-1) and methanol to a beaker, add intermediate 1 and triethylamine under stirring at 0°C, and stir to react for 3-4 hours to obtain intermediate 2. The amount ratio of allyl phosphine dichloride, methanol, intermediate 1 and triethylamine is 0.1 mol: 80-100 mL: 0.1 mol: 0.6 mol;

[0018] During the reaction of step A2, allylphosphine dichloride reacts with intermediate 1 to generate intermediate 2. The structure of intermediate 2 is shown below:

[0019]

[0020] Step A3: Add nano-silicon dioxide to anhydrous ethanol, and ultrasonically disperse for 20-30 minutes to obtain a mixed solution a; add intermediate 2 to deionized water, stir at 50°C for 5-6 hours, and cool to room temperature to obtain a mixed solution b; add mixed solution b to mixed solution a under stirring, and then adjust the pH to 8.5-9.5 with ammonia water, heat to 50°C, stir to react for 10-12 hours, filter, and dry in a drying oven at 60°C for 6-8 hours to obtain intermediate 3; the dosage ratio of nano-silicon dioxide, anhydrous ethanol, intermediate 2, deionized water and ammonia water is 1g:20mL:1g:20mL:5-10mL;

[0021] During the reaction of step A3, the siloxane groups in intermediate 2 are hydrolyzed to obtain silanols, which bond with the hydroxyl groups on the surface of nano-silicon dioxide to obtain intermediate 3.

[0022] Step A4: After the chloroether resin, intermediate 3 and composite monomer are mixed and stirred for 1-1.5h, sodium bicarbonate, deionized water and sodium methyl propylene sulfonate are added, and the mixture is stirred for 30-40min to obtain an emulsion; deionized water is added to the emulsion, the temperature is raised to 70°C, ammonium persulfate is added, the temperature is raised to 80-85°C, and the mixture is stirred for 7-8h to obtain a reaction solution, the reaction solution is cooled to 40°C, the pH is adjusted to 8.0 with aqueous ammonia, the mixture is stirred for 20min, the mixture is cooled to room temperature, and the mixture is filtered to obtain a modified acrylic ester emulsion; chloroether resin, intermediate 3, composite monomer, sodium bicarbonate, deionized water, sodium methyl propylene sulfonate and persulfate are added to the emulsion, the mixture is heated to 70°C, ammonium persulfate is added, the temperature is raised to 80-85°C, and the mixture is stirred for 7-8h to obtain a reaction solution, the reaction solution is cooled to 40°C, the pH is adjusted to 8.0 with aqueous ammonia, the mixture is stirred for 20min, the mixture is cooled to room temperature, and the mixture is filtered to obtain a modified acrylic ester emulsion; The dosage ratio of ammonium acid is 3.0g:0.3g:41.2g:10-12g:55mL:20-25g:0.5g, the dosage of deionized water is the total amount of deionized water added in the reaction, and the volume ratio of the deionized water added twice is 10:1. The composite monomer includes methacrylic acid, methyl methacrylate, vinyl acetate, butyl acrylate, styrene and hydroxypropyl acrylate, and the mass ratio of methacrylic acid, methyl methacrylate, vinyl acetate, butyl acrylate, styrene and hydroxypropyl acrylate is 1.0g:2.3g:4.6g:17.0g:10.0g:6.3g.

[0023] During the reaction of step A4, the C-Cl bond in the structure of the chloroether resin is homolytically cleaved under the action of the ammonium persulfate initiator, and a polymerization reaction occurs with the acrylate monomer and the intermediate 3 containing a terminal unsaturated double bond. The chloroether resin has excellent adhesion and durability, and does not contain acid-base sensitive ester groups and the like, and has good acid and alkali resistance. The nano-silicon dioxide contained in the intermediate 3 enhances the mechanical properties of the polymer. The polyphosphate formed after the polymerization reaction can flame retard and plasticize the acrylate emulsion, and can be grafted into the polymer through reaction, which can enhance the dispersion compatibility of the phosphorus-containing flame retardant in the polymer and avoid migration, thereby making the modified acrylate emulsion have good adhesion, durability, acid and alkali resistance and flame retardancy.

[0024] The modified fluorescein is prepared by the following steps:

[0025] Step B1: Add 5-oxo-5-[(2,2,6,6-tetramethylpiperidin-4-yl)amino]pentanoic acid (CAS No. 300574-81-6) and ethanol into a flask, start stirring, then add 20% sulfuric acid solution and epichlorohydrin, stir at 110-130° C. for 5-6 hours, extract, and dry to obtain intermediate a, wherein the amount ratio of 5-oxo-5-[(2,2,6,6-tetramethylpiperidin-4-yl)amino]pentanoic acid, ethanol, 20% sulfuric acid solution and epichlorohydrin is 0.1 mol: 70-80 mL: 1-3 mL: 0.1 mol;

[0026] During the reaction of step B1, 5-oxo-5-[(2,2,6,6-tetramethylpiperidin-4-yl)amino]pentanoic acid reacts with epichlorohydrin under acidic conditions to generate intermediate a. The structure of intermediate a is shown below:

[0027]

[0028] Step B2: First, add 4-amino-2-(6-hydroxy-3-oxo-xanthene-9-yl)-benzoic acid ethyl ester (CAS No. 219122-41-5) and sodium hydroxide into deionized water, and stir for 10-20 minutes to obtain a mixed solution 1; then add the intermediate a and 1,4-dioxane into a flask, stir for 5-10 minutes, place the flask in a 0°C ice water bath, and slowly dropwise add the mixed solution 1 into the flask under stirring. After the dropwise addition is completed, add the mixed solution 1 at 100-1 The mixture was stirred at 20°C for 12-14 hours, cooled to room temperature, deionized water was added, and the mixture was washed with deionized water. The mixture was dried in a drying oven at 110°C for 12 hours to obtain intermediate b. The dosage ratio of 4-amino-2-(6-hydroxy-3-oxy-xanthene-9-yl)-benzoic acid ethyl ester, sodium hydroxide, deionized water, intermediate a and 1,4-dioxane was 0.1 mol: 0.1 mol: 150-180 mL: 0.1 mol: 100 mL.

[0029] During the reaction of step B2, 4-amino-2-(6-hydroxy-3-oxo-xanthene-9-yl)-ethyl benzoate reacts with intermediate a to remove hydrogen chloride, introduces a hindered amine structure with light stabilization, and generates intermediate b. The structure of intermediate b is shown below:

[0030]

[0031] Step B3: Add intermediate b and 4-vinylbenzenebutylamine to ethyl acetate, start stirring, react at 50-60°C for 18-24h, and cool to room temperature to obtain modified fluorescein; the amount ratio of intermediate b, 4-vinylbenzenebutylamine and ethyl acetate is 0.1 mol: 0.1 mol: 80-100 mL;

[0032] During the reaction of step B3, intermediate b reacts with 4-vinylbenzenebutylamine to generate a more structurally stable amide compound, namely modified fluorescein. The modified fluorescein is based on aminofluorescein as the basic skeleton and has good fluorescence. The active groups such as unsaturated double bonds, secondary amine groups and secondary hydroxyl groups enhance the reactivity of aminofluorescein. After grafting the hindered amine structure, the modified fluorescein is endowed with good light stability. After the molecular weight of the hindered amine light stabilizer itself is increased, its heat resistance and extraction resistance are improved. The structure of the modified fluorescein is shown below:

[0033]

[0034] Beneficial effects of the present invention: The present invention prepares an acid- and alkali-resistant inorganic composite ink, which is made of raw materials such as modified acrylic emulsion, modified fluorescein, inorganic pigment, inorganic nanopowder, surfactant, preservative, drying agent, auxiliary solvent, ammonia water and deionized water. The chloroether resin in the modified acrylic emulsion has excellent adhesion and durability. The chloroether resin does not contain ester groups and other groups that are sensitive to acid and alkali, and has good acid and alkali resistance, which improves the adhesion firmness, durability and acid and alkali resistance of the composite ink; nano-silicon dioxide enhances the mechanical properties of the polymer and improves the mechanical properties of the composite ink; the polyphosphate formed after the polymerization reaction can flame retard and plasticize the acrylic emulsion, and can be grafted into the polymer through reaction, which can enhance the dispersion compatibility of the phosphorus-containing flame retardant in the matrix and avoid migration, so that the composite ink has the excellent flame retardant properties of the phosphorus-based flame retardant.

[0035] The modified fluorescein is based on aminofluorescein and has good fluorescence. The active groups such as unsaturated double bonds, secondary amine groups and secondary hydroxyl groups enhance the reactivity of aminofluorescein, so that the modified fluorescein can produce hydrogen bonds or covalent cross-linking with the hydroxyl and carboxyl groups in the modified acrylic ester emulsion, thereby enhancing the dispersion of the modified fluorescein in the matrix, thereby making the composite ink have stable fluorescence properties. After the hindered amine structure is grafted, the molecular weight of the hindered amine light stabilizer itself increases, and its heat resistance and extraction resistance are improved, and the absorption of ultraviolet rays is better, giving the composite ink good heat resistance and light stability. DETAILED DESCRIPTION

[0036] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] Example 1

[0038] A modified acrylic emulsion is prepared by the following steps:

[0039] Step A1: Add hydroxyethyl acrylate and anhydrous ethanol into a flask, slowly drop 3-aminopropyltrimethoxysilane at 25°C under nitrogen protection, raise the temperature to 75°C after the dropwise addition, stir and react for 48h, and vacuum dry at 50°C to obtain intermediate 1, wherein the amount ratio of hydroxyethyl acrylate, anhydrous ethanol and 3-aminopropyltrimethoxysilane is 0.2mol:100mL:0.1mol;

[0040] Step A2: add allyl phosphine dichloride to methanol, add intermediate 1 and triethylamine with stirring at 0°C, and stir to react for 3 hours to obtain intermediate 2. The amount ratio of allyl phosphine dichloride, methanol, intermediate 1 and triethylamine is 0.1 mol: 80 mL: 0.1 mol: 0.6 mol;

[0041] Step A3: Add nano-silicon dioxide to anhydrous ethanol, and ultrasonically disperse for 20 minutes to obtain a mixed solution a; add intermediate 2 to deionized water, stir at 50°C for 5 hours, and cool to room temperature to obtain a mixed solution b; add mixed solution b to mixed solution a under stirring, and then adjust the pH to 8.5 with ammonia water, heat to 50°C, stir to react for 10 hours, filter, and dry in a drying oven at 60°C for 6 hours to obtain intermediate 3; the dosage ratio of nano-silicon dioxide, anhydrous ethanol, intermediate 2, deionized water and ammonia water is 1g:20mL:1g:20mL:5mL;

[0042] Step A4: After the chloroether resin, intermediate 3 and composite monomer are mixed and stirred for 1 hour, sodium bicarbonate, deionized water and sodium methacrylate are added, and the mixture is stirred for 30 minutes to obtain an emulsion; deionized water is added to the emulsion, the temperature is raised to 70°C, ammonium persulfate is added, the temperature is raised to 80°C, and the mixture is stirred for 7 hours to obtain a reaction solution, after the reaction solution is cooled to 40°C, the pH is adjusted to 8.0 with ammonia water, the mixture is stirred for 20 minutes, the mixture is cooled to room temperature, and the mixture is filtered to obtain a modified acrylic ester emulsion; chloroether resin, intermediate 3, composite monomer, sodium bicarbonate, deionized water, sodium methacrylate and ammonium persulfate The dosage ratio is 3.0g:0.3g:41.2g:10g:55mL:20g:0.5g, the dosage of deionized water is the total amount of deionized water added in the reaction, and the volume ratio of the deionized water added twice is 10:1. The composite monomer includes methacrylic acid, methyl methacrylate, vinyl acetate, butyl acrylate, styrene and hydroxypropyl acrylate, and the mass ratio of methacrylic acid, methyl methacrylate, vinyl acetate, butyl acrylate, styrene and hydroxypropyl acrylate is 1.0g:2.3g:4.6g:17.0g:10.0g:6.3g.

[0043] Example 2

[0044] A modified acrylic emulsion is prepared by the following steps:

[0045] Step A1: Add hydroxyethyl acrylate and anhydrous ethanol into a flask, slowly drop 3-aminopropyltrimethoxysilane at 25°C under nitrogen protection, raise the temperature to 80°C after the dropwise addition, stir and react for 48h, and vacuum dry at 50°C to obtain intermediate 1, wherein the amount ratio of hydroxyethyl acrylate, anhydrous ethanol and 3-aminopropyltrimethoxysilane is 0.22mol:100mL:0.1mol;

[0046] Step A2: add allyl phosphine dichloride to methanol, add intermediate 1 and triethylamine under stirring at 0°C, and react for 3.5 hours to obtain intermediate 2. The amount ratio of allyl phosphine dichloride, methanol, intermediate 1 and triethylamine is 0.1 mol: 90 mL: 0.1 mol: 0.6 mol;

[0047] Step A3: Add nano-silicon dioxide to anhydrous ethanol, and ultrasonically disperse for 25 minutes to obtain a mixed solution a; add intermediate 2 to deionized water, stir at 50°C for 5.5 hours, and cool to room temperature to obtain a mixed solution b; add mixed solution b to mixed solution a under stirring, and then adjust the pH to 9.0 with ammonia water, heat to 50°C, stir to react for 11 hours, filter, and dry in a drying oven at 60°C for 7 hours to obtain intermediate 3; the dosage ratio of nano-silicon dioxide, anhydrous ethanol, intermediate 2, deionized water and ammonia water is 1g:20mL:1g:20mL:7mL;

[0048] Step A4: After the chloroether resin, intermediate 3 and composite monomer are mixed and stirred for 1.2 hours, sodium bicarbonate, deionized water and sodium methyl propylene sulfonate are added, and the mixture is stirred for 35 minutes to obtain an emulsion; deionized water is added to the emulsion, the temperature is raised to 70°C, ammonium persulfate is added, the temperature is raised to 80°C, and the mixture is stirred for reaction for 7.5 hours to obtain a reaction solution, and the reaction solution is cooled to 40°C, the pH value is adjusted to 8.0 with aqueous ammonia, and the mixture is stirred for 20 minutes, cooled to room temperature, and filtered to obtain a modified acrylic ester emulsion; chloroether resin, intermediate 3, composite monomer, sodium bicarbonate, deionized water, sodium methyl propylene sulfonate and persulfate are added to the emulsion, the temperature is raised to 70°C, ammonium persulfate is added, the temperature is raised to 80°C, and the mixture is stirred for reaction for 7.5 hours to obtain a reaction solution, and the reaction solution is cooled to 40°C, the pH value is adjusted to 8.0 with aqueous ammonia, and the mixture is stirred for 20 minutes, cooled to room temperature, and filtered to obtain a modified acrylic ester emulsion. The dosage ratio of ammonium acid is 3.0g:0.3g:41.2g:11g:55mL:22g:0.5g, the dosage of deionized water is the total amount of deionized water added in the reaction, and the volume ratio of the deionized water added twice is 10:1. The composite monomer includes methacrylic acid, methyl methacrylate, vinyl acetate, butyl acrylate, styrene and hydroxypropyl acrylate, and the mass ratio of methacrylic acid, methyl methacrylate, vinyl acetate, butyl acrylate, styrene and hydroxypropyl acrylate is 1.0g:2.3g:4.6g:17.0g:10.0g:6.3g.

[0049] Example 3

[0050] A modified acrylic emulsion is prepared by the following steps:

[0051] Step A1: Add hydroxyethyl acrylate and anhydrous ethanol into a flask, slowly drop 3-aminopropyltrimethoxysilane at 25°C under nitrogen protection, raise the temperature to 85°C after the dropwise addition, stir and react for 48h, and vacuum dry at 50°C to obtain intermediate 1, wherein the amount ratio of hydroxyethyl acrylate, anhydrous ethanol and 3-aminopropyltrimethoxysilane is 0.25mol:100mL:0.1mol;

[0052] Step A2: add allyl phosphine dichloride to methanol, add intermediate 1 and triethylamine under stirring at 0°C, and stir to react for 4 hours to obtain intermediate 2. The amount ratio of allyl phosphine dichloride, methanol, intermediate 1 and triethylamine is 0.1 mol: 100 mL: 0.1 mol: 0.6 mol;

[0053] Step A3: Add nano-silicon dioxide to anhydrous ethanol, and ultrasonically disperse for 30 minutes to obtain a mixed solution a; add intermediate 2 to deionized water, stir at 50°C for 6 hours, and cool to room temperature to obtain a mixed solution b; add mixed solution b to mixed solution a under stirring, and then adjust the pH to 9.5 with ammonia water, heat to 50°C, stir to react for 12 hours, filter, and dry in a drying oven at 60°C for 8 hours to obtain intermediate 3; the dosage ratio of nano-silicon dioxide, anhydrous ethanol, intermediate 2, deionized water and ammonia water is 1g:20mL:1g:20mL:10mL;

[0054] Step A4: After the chloroether resin, intermediate 3 and composite monomer are mixed and stirred for 1.5 hours, sodium bicarbonate, deionized water and sodium methacrylate are added, and the mixture is stirred for 40 minutes to obtain an emulsion; deionized water is added to the emulsion, the temperature is raised to 70°C, ammonium persulfate is added, the temperature is raised to 85°C, and the mixture is stirred for 8 hours to obtain a reaction solution; after the reaction solution is cooled to 40°C, the pH value is adjusted to 8.0 with aqueous ammonia, the mixture is stirred for 20 minutes, the mixture is cooled to room temperature, and the mixture is filtered to obtain a modified acrylic ester emulsion; chloroether resin, intermediate 3, composite monomer, sodium bicarbonate, deionized water, sodium methacrylate and persulfate are added to the emulsion, the mixture is heated to 70°C, ammonium persulfate is added, the temperature is raised to 85°C, and the mixture is stirred for 8 hours to obtain a reaction solution; after the reaction solution is cooled to 40°C, the pH value is adjusted to 8.0 with aqueous ammonia, the mixture is stirred for 20 minutes, the mixture is cooled to room temperature, and the mixture is filtered to obtain a modified acrylic ester emulsion; The dosage ratio of ammonium is 3.0g:0.3g:41.2g:12g:55mL:25g:0.5g, the dosage of deionized water is the total amount of deionized water added in the reaction, and the volume ratio of the deionized water added twice is 10:1. The composite monomer includes methacrylic acid, methyl methacrylate, vinyl acetate, butyl acrylate, styrene and hydroxypropyl acrylate, and the mass ratio of methacrylic acid, methyl methacrylate, vinyl acetate, butyl acrylate, styrene and hydroxypropyl acrylate is 1.0g:2.3g:4.6g:17.0g:10.0g:6.3g.

[0055] Example 4

[0056] Step B1: Add 5-oxy-5-[(2,2,6,6-tetramethylpiperidin-4-yl)amino]pentanoic acid and ethanol into a flask, start stirring, then add 20% sulfuric acid solution and epichlorohydrin, stir at 110° C. for 5 h, extract, and dry to obtain intermediate a, wherein the amount ratio of 5-oxy-5-[(2,2,6,6-tetramethylpiperidin-4-yl)amino]pentanoic acid, ethanol, 20% sulfuric acid solution and epichlorohydrin is 0.1 mol: 70 mL: 1 mL: 0.1 mol;

[0057] Step B2: first, add 4-amino-2-(6-hydroxy-3-oxy-xanthene-9-yl)-benzoic acid ethyl ester and sodium hydroxide to deionized water, and stir for 10 minutes to obtain a mixed solution 1; then add the intermediate a and 1,4-dioxane to a flask, stir for 5 minutes, place the flask in a 0°C ice water bath, and slowly drop the mixed solution 1 into the flask under stirring. After the dropwise addition is completed, stir and react at 100°C for 12 hours, cool to room temperature, add deionized water, wash with deionized water, and dry in a drying oven at 110°C for 12 hours to obtain intermediate b, wherein the amount ratio of 4-amino-2-(6-hydroxy-3-oxy-xanthene-9-yl)-benzoic acid ethyl ester, sodium hydroxide, deionized water, intermediate a and 1,4-dioxane is 0.1 mol: 0.1 mol: 150 mL: 0.1 mol: 100 mL;

[0058] Step B3: Add intermediate b and 4-vinylbenzenebutylamine to ethyl acetate, start stirring, react at 50°C for 18 hours, and cool to room temperature to obtain modified fluorescein; the dosage ratio of intermediate b, 4-vinylbenzenebutylamine and ethyl acetate is 0.1 mol: 0.1 mol: 80 mL.

[0059] Example 5

[0060] Step B1: Add 5-oxy-5-[(2,2,6,6-tetramethylpiperidin-4-yl)amino]pentanoic acid and ethanol into a flask, start stirring, then add 20% sulfuric acid solution and epichlorohydrin, stir at 120°C for 5.5h, extract, and dry to obtain intermediate a, wherein the amount ratio of 5-oxy-5-[(2,2,6,6-tetramethylpiperidin-4-yl)amino]pentanoic acid, ethanol, 20% sulfuric acid solution and epichlorohydrin is 0.1mol:75mL:2mL:0.1mol;

[0061] Step B2: first, add 4-amino-2-(6-hydroxy-3-oxy-xanthene-9-yl)-benzoic acid ethyl ester and sodium hydroxide to deionized water, and stir for 15 minutes to obtain a mixed solution 1; then add the intermediate a and 1,4-dioxane to a flask, stir for 7 minutes, place the flask in a 0°C ice water bath, and slowly drop the mixed solution 1 into the flask under stirring. After the dropwise addition is completed, stir and react at 110°C for 13 hours, cool to room temperature, add deionized water, wash with deionized water, and dry in a drying oven at 110°C for 12 hours to obtain intermediate b, wherein the amount ratio of 4-amino-2-(6-hydroxy-3-oxy-xanthene-9-yl)-benzoic acid ethyl ester, sodium hydroxide, deionized water, intermediate a and 1,4-dioxane is 0.1 mol: 0.1 mol: 165 mL: 0.1 mol: 100 mL;

[0062] Step B3: Add intermediate b and 4-vinylbenzenebutylamine to ethyl acetate, start stirring, react at 55°C for 21 hours, and cool to room temperature to obtain modified fluorescein; the dosage ratio of intermediate b, 4-vinylbenzenebutylamine and ethyl acetate is 0.1 mol: 0.1 mol: 90 mL.

[0063] Example 6

[0064] Step B1: Add 5-oxy-5-[(2,2,6,6-tetramethylpiperidin-4-yl)amino]pentanoic acid and ethanol into a flask, start stirring, then add 20% by mass sulfuric acid solution and epichlorohydrin, stir at 130° C. for 6 hours, extract, and dry to obtain intermediate a, wherein the amount ratio of 5-oxy-5-[(2,2,6,6-tetramethylpiperidin-4-yl)amino]pentanoic acid, ethanol, 20% by mass sulfuric acid solution and epichlorohydrin is 0.1 mol: 80 mL: 3 mL: 0.1 mol;

[0065] Step B2: first, add 4-amino-2-(6-hydroxy-3-oxy-xanthene-9-yl)-benzoic acid ethyl ester and sodium hydroxide to deionized water, and stir for 20 minutes to obtain a mixed solution 1; then add the intermediate a and 1,4-dioxane to a flask, stir for 10 minutes, place the flask in a 0°C ice water bath, and slowly drop the mixed solution 1 into the flask under stirring. After the dropwise addition is completed, stir and react at 120°C for 14 hours, cool to room temperature, add deionized water, wash with deionized water, and dry in a drying oven at 110°C for 12 hours to obtain intermediate b, wherein the amount ratio of 4-amino-2-(6-hydroxy-3-oxy-xanthene-9-yl)-benzoic acid ethyl ester, sodium hydroxide, deionized water, intermediate a and 1,4-dioxane is 0.1 mol: 0.1 mol: 180 mL: 0.1 mol: 100 mL;

[0066] Step B3: Add intermediate b and 4-vinylbenzenebutylamine to ethyl acetate, start stirring, react at 60°C for 24 hours, and cool to room temperature to obtain modified fluorescein; the dosage ratio of intermediate b, 4-vinylbenzenebutylamine and ethyl acetate is 0.1 mol: 0.1 mol: 100 mL.

[0067] Example 7

[0068] An acid-base resistant inorganic composite ink comprises the following raw materials in parts by weight: 10 parts of modified acrylic emulsion, 8 parts of modified fluorescent pigment, 10 parts of inorganic pigment, 10 parts of inorganic nano powder, 0.3 parts of surfactant, 0.2 parts of preservative, 2 parts of drying agent, 8 parts of auxiliary solvent, 5 parts of ammonia water and 50 parts of deionized water; the inorganic pigment is titanium dioxide; the inorganic nano powder is a mixture of nano zinc oxide and nano silicon nitride in a mass ratio of 1:2; the surfactant is a mixture of polyoxyethylene lauryl ether and Tween 20 in a mass ratio of 1:1; the preservative is phenol; the drying agent is a mixture of ethanol and isopropanol in a volume ratio of 1:1; the auxiliary solvent is a mixture of ethylene glycol, propylene glycol and glycerol in a volume ratio of 1:1:1;

[0069] The acid- and alkali-resistant inorganic composite ink is prepared by the following steps:

[0070] The modified acrylic emulsion obtained in Example 1, the modified fluorescent substance obtained in Example 4, and a surfactant are added to a stirring kettle. After stirring at a speed of 500 r / min for 10 min, the speed is increased to 2000 r / min, and high-speed shearing and dispersion grinding are performed for 30 min. Then, inorganic pigments, inorganic nanopowders, preservatives, drying agents, auxiliary solvents and deionized water are added to the stirring kettle. After high-speed shearing and dispersion grinding at a speed of 3000 r / min for 60 min, the pH is adjusted to 8.0 with ammonia water, and the acid-base resistant inorganic composite ink is obtained by filtration.

[0071] Example 8

[0072] An acid-base resistant inorganic composite ink comprises the following raw materials in parts by weight: 12 parts of modified acrylic emulsion, 9 parts of modified fluorescent pigment, 15 parts of inorganic pigment, 15 parts of inorganic nano powder, 0.4 parts of surfactant, 0.3 parts of preservative, 2.5 parts of drying agent, 9 parts of auxiliary solvent, 7 parts of ammonia water and 55 parts of deionized water; the inorganic pigment is titanium dioxide; the inorganic nano powder is a mixture of nano zinc oxide and nano silicon nitride in a mass ratio of 1:2; the surfactant is a mixture of polyoxyethylene lauryl ether and Tween 40 in a mass ratio of 1:1; the preservative is phenol; the drying agent is a mixture of ethanol and isopropanol in a volume ratio of 1:1; the auxiliary solvent is a mixture of ethylene glycol, propylene glycol and 1,4-butanediol in a volume ratio of 1:1:1;

[0073] The acid- and alkali-resistant inorganic composite ink is prepared by the following steps:

[0074] The modified acrylic emulsion obtained in Example 2, the modified fluorescent substance obtained in Example 5, and a surfactant are added to a stirring kettle. After stirring at a speed of 500 r / min for 12 minutes, the speed is increased to 2000 r / min. After high-speed shearing and dispersion grinding for 30 minutes, inorganic pigments, inorganic nanopowders, preservatives, drying agents, auxiliary solvents and deionized water are added to the stirring kettle. After high-speed shearing and dispersion grinding at a speed of 3000 r / min for 60 minutes, the pH is adjusted to 8.5 with ammonia water, and the acid and alkali resistant inorganic composite ink is obtained by filtration.

[0075] Example 9

[0076] An acid-base resistant inorganic composite ink comprises the following raw materials in parts by weight: 15 parts of modified acrylic emulsion, 10 parts of modified fluorescent pigment, 20 parts of inorganic pigment, 20 parts of inorganic nano powder, 0.5 parts of surfactant, 0.4 parts of preservative, 3 parts of drying agent, 10 parts of auxiliary solvent, 10 parts of ammonia water and 60 parts of deionized water; the inorganic pigment is titanium dioxide; the inorganic nano powder is a mixture of nano zinc oxide and nano silicon nitride in a mass ratio of 1:2; the surfactant is a mixture of Tween 20 and Tween 40 in a mass ratio of 1:1; the preservative is phenol; the drying agent is a mixture of ethanol and isopropanol in a volume ratio of 1:1; the auxiliary solvent is a mixture of ethylene glycol, glycerol and 1,4-butanediol in a volume ratio of 1:1:1;

[0077] The acid- and alkali-resistant inorganic composite ink is prepared by the following steps:

[0078] The modified acrylic emulsion obtained in Example 3, the modified fluorescent substance obtained in Example 6, and a surfactant are added to a stirring kettle. After stirring at a speed of 600 r / min for 15 minutes, the speed is increased to 2000 r / min. After high-speed shearing and dispersion grinding for 30 minutes, inorganic pigments, inorganic nanopowders, preservatives, drying agents, auxiliary solvents and deionized water are added to the stirring kettle. After high-speed shearing and dispersion grinding at a speed of 3000 r / min for 60 minutes, the pH is adjusted to 9.0 with ammonia water, and the acid and alkali resistant inorganic composite ink is obtained by filtration.

[0079] Comparative Example 1

[0080] This comparative example is an ink prepared according to the ingredient ratio in Table 1 of the patent publication number CN117384513A.

[0081] Comparative Example 2

[0082] Compared with Example 9, the modified acrylic emulsion was replaced with acrylic emulsion, and the rest was exactly the same as Example 9 to prepare an acid and alkali resistant inorganic composite ink.

[0083] Comparative Example 3

[0084] Compared with Example 9, the modified fluorescent substance is replaced with fluorescent substance, and the other steps are exactly the same as Example 9 to obtain an acid- and alkali-resistant inorganic composite ink.

[0085] The acid- and alkali-resistant inorganic composite ink prepared by the present invention is further tested for its effect, and the test results are as follows.

[0086] The acid- and alkali-resistant inorganic composite ink prepared by the present invention was tested according to relevant standard methods, and the results are shown in Table 1.

[0087] Table 1:

[0088]

[0089] The adhesion test is carried out according to GB / T13217.7-2023.

[0090] Light fastness test method: The inks of Examples 7-9 and Comparative Examples 1-3 were coated on wool cloth used in the AATCC16-2004 standard, and were continuously illuminated under a xenon arc lamp for 20 hours. The light fastness was evaluated according to the AATCC16-2004 standard.

[0091] Acid and alkali resistance test method: The inks of Examples 7-9 and Comparative Examples 1-3 are coated on test plates, and then the test plates are immersed in a 7.5% by mass sulfuric acid solution and a 7.5% by mass sodium hydroxide solution, respectively, and observed after 48 hours and 168 hours; the test plates are asbestos-free fiber cement flat plates with a flat surface, a size of 150 mm × 70 mm, and a thickness of 3-6 mm.

[0092] Heat resistance test method: The inks of Examples 7-9 and Comparative Examples 1-3 were placed at 50°C and 600°C for observation.

[0093] According to the data in Table 1, compared with Example 1, Example 7, Example 8 and Example 9, it can be seen that the acid- and alkali-resistant inorganic composite ink prepared by the present invention has excellent adhesion, light fastness, acid- and alkali-resistant and heat resistance compared with commercially available inorganic composite inks, and does not burn at 600°C, indicating excellent flame retardancy; compared with Example 2, Example 9 shows that the modified acrylic emulsion is used, in which the chloroether resin introduced has good adhesion to the substrate and does not contain acid- and alkali-sensitive groups, which greatly improves the acid- and alkali-resistant and adhesion of the composite ink, and polyphosphate is grafted into the polymer, which greatly improves the flame retardancy; compared with Example 3, Example 9 shows that the modified fluorescein is used, and the active groups contained in it can be cross-linked with hydroxyl and carboxyl groups in the acrylic emulsion, so that its dispersibility in the modified acrylic emulsion is enhanced, and the hindered amine light stabilizer contained in the modified fluorescein, after its own molecular weight is increased, gives the composite ink good heat resistance and light stability.

[0094] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. An acid- and alkali-resistant inorganic composite ink, characterized in that: The invention comprises the following raw materials in parts by weight: 10-15 parts of modified acrylic emulsion, 8-10 parts of modified fluorescent pigment, 10-20 parts of inorganic pigment, 10-20 parts of inorganic nano powder, 0.3-0.5 parts of surfactant, 0.2-0.4 parts of preservative, 2-3 parts of drying agent, 8-10 parts of auxiliary solvent, 5-10 parts of ammonia water and 50-60 parts of deionized water; the inorganic pigment is titanium dioxide; the inorganic nano powder is a mixture of nano zinc oxide and nano silicon nitride in a mass ratio of 1:2; the surfactant is one or more of polyoxyethylene lauryl ether, Tween 20 and Tween 40; the preservative is phenol; the drying agent is a mixture of ethanol and isopropanol in a volume ratio of 1:1; the auxiliary solvent is one or more of ethylene glycol, propylene glycol, glycerol and 1,4-butanediol; The modified acrylic ester emulsion is prepared by the following steps: Step A1: Add hydroxyethyl acrylate and anhydrous ethanol into a flask, slowly drop 3-aminopropyltrimethoxysilane at 25°C under nitrogen protection, raise the temperature to 75-85°C after the addition is complete, stir and react for 48 hours, and vacuum dry at 50°C to obtain intermediate 1; Step A2: Add allylphosphine dichloride and methanol into a beaker, add intermediate 1 and triethylamine with stirring at 0°C, and stir to react for 3-4 hours to obtain intermediate 2; Step A3: Add nano-silicon dioxide to anhydrous ethanol, and ultrasonically disperse for 20-30 minutes to obtain a mixed solution a; add intermediate 2 to deionized water, stir at 50°C for 5-6 hours, and cool to room temperature to obtain a mixed solution b; add the mixed solution b to the mixed solution a under stirring, and then adjust the pH to 8.5-9.5 with ammonia water, heat to 50°C, stir to react for 10-12 hours, filter, and dry in a drying oven at 60°C for 6-8 hours to obtain intermediate 3; Step A4: After the chloroether resin, intermediate 3 and composite monomer are mixed and stirred for 1-1.5 hours, sodium bicarbonate, deionized water and sodium methyl propylene sulfonate are added, and the mixture is stirred for 30-40 minutes to obtain an emulsion; deionized water is added to the emulsion, the temperature is raised to 70° C., ammonium persulfate is added, the temperature is raised to 80-85° C., and the mixture is stirred for reaction for 7-8 hours to obtain a reaction solution, the reaction solution is cooled to 40° C., the pH is adjusted to 8.0 with aqueous ammonia, the mixture is stirred for 20 minutes, the mixture is cooled to room temperature, and the mixture is filtered to obtain a modified acrylic ester emulsion; The modified fluorescein is prepared by the following steps: Step B1: Add 5-oxo-5-[(2,2,6,6-tetramethylpiperidin-4-yl)amino]pentanoic acid and ethanol into a flask, start stirring, then add 20% by mass sulfuric acid solution and epichlorohydrin, stir at 110-130° C. for 5-6 hours, extract, and dry to obtain intermediate a; Step B2: first, add 4-amino-2-(6-hydroxy-3-oxo-xanthene-9-yl)-benzoic acid ethyl ester and sodium hydroxide into deionized water, and stir for 10-20 minutes to obtain a mixed solution 1; then add the intermediate a and 1,4-dioxane into a flask, stir for 5-10 minutes, place the flask in a 0°C ice water bath, and slowly drop the mixed solution 1 into the flask under stirring. After the dropwise addition is completed, stir and react at 100-120°C for 12-14 hours, cool to room temperature, add deionized water, wash with deionized water, and dry in a drying oven at 110°C for 12 hours to obtain the intermediate b; Step B3: Add intermediate b and 4-vinylbenzenebutylamine to ethyl acetate, start stirring, stir and react at 50-60° C. for 18-24 hours, and cool to room temperature to obtain modified fluorescein.

2. The acid- and alkali-resistant inorganic composite ink according to claim 1, characterized in that: In step A1, the usage ratio of hydroxyethyl acrylate, anhydrous ethanol and 3-aminopropyltrimethoxysilane is 0.2-0.25 mol:100 mL:0.1 mol.

3. The acid- and alkali-resistant inorganic composite ink according to claim 1, characterized in that: In step A2, the usage ratio of allylphosphine dichloride, methanol, intermediate 1 and triethylamine is 0.1 mol: 80-100 mL: 0.1 mol: 0.6 mol.

4. The acid- and alkali-resistant inorganic composite ink according to claim 1, characterized in that: In step A3, the usage ratio of nano-silica, anhydrous ethanol, intermediate 2, deionized water and ammonia water is 1 g: 20 mL: 1 g: 20 mL: 5-10 mL.

5. The acid- and alkali-resistant inorganic composite ink according to claim 1, characterized in that: In step A4, the amount ratio of chloroether resin, intermediate 3, composite monomer, sodium bicarbonate, deionized water, sodium methacrylate and ammonium persulfate is 3.0g:0.3g:41.2g:10-12g:55mL:20-25g:0.5g, the amount of deionized water is the total amount of deionized water added in the reaction, and the volume ratio of the deionized water added twice is 10:

1. The composite monomer includes methacrylic acid, methyl methacrylate, vinyl acetate, butyl acrylate, styrene and hydroxypropyl acrylate, and the mass ratio of methacrylic acid, methyl methacrylate, vinyl acetate, butyl acrylate, styrene and hydroxypropyl acrylate is 1.0g:2.3g:4.6g:17.0g:10.0g:6.3g.

6. The acid- and alkali-resistant inorganic composite ink according to claim 1, characterized in that: In step B1, the dosage ratio of 5-oxo-5-[(2,2,6,6-tetramethylpiperidin-4-yl)amino]pentanoic acid, ethanol, 20% sulfuric acid solution and epichlorohydrin is 0.1 mol: 70-80 mL: 1-3 mL: 0.1 mol.

7. The acid- and alkali-resistant inorganic composite ink according to claim 1, characterized in that: In step B2, the usage ratio of 4-amino-2-(6-hydroxy-3-oxo-xanthene-9-yl)-benzoic acid ethyl ester, sodium hydroxide, deionized water, intermediate a and 1,4-dioxane is 0.1 mol: 0.1 mol: 150-180 mL: 0.1 mol: 100 mL.

8. The acid- and alkali-resistant inorganic composite ink according to claim 1, characterized in that: In step B3, the usage ratio of intermediate b, 4-vinylbenzenebutylamine and ethyl acetate is 0.1 mol:0.1 mol:80-100 mL.

9. The method for preparing an acid- and alkali-resistant inorganic composite ink according to claim 1, characterized in that: The steps include: Add modified acrylic emulsion, modified fluorescent element and surfactant into a stirring kettle, stir at a speed of 500-600 r / min for 10-15 minutes, then increase the speed to 2000 r / min, high-speed shear and disperse grinding for 30 minutes, add inorganic pigment, inorganic nano powder, preservative, drying agent, auxiliary solvent and deionized water into the stirring kettle, high-speed shear and disperse grinding at a speed of 3000 r / min for 60 minutes, adjust the pH to 8.0-9.0 with ammonia water, and filter to obtain acid and alkali resistant inorganic composite ink.

Citation Information

Patent Citations

  • Fluorescent anti-counterfeiting safe ink with carbon quantum dots and preparation method of fluorescent anti-counterfeiting safe ink

    CN117384513A

  • Cure degree evaluation method, cure degree evaluation sheet and cure degree evaluation system for active energy ray-curable resin composition

    CN102334029A

  • Liquid tint materials and films made therefrom

    CN103649241A

  • Water-based nanometer anti-counterfeiting ink-jet ink and preparation method thereof

    CN113201254A

  • Active energy ray-curable ink composition, inkjet recording method, decorative sheet, decorative sheet molded product, method for producing in-mold molded product, and in-mold molded product