A method for producing high-silicon pure iron

By controlling the impurity content in the production process of high-silicon pure iron, and by adopting processes such as molten iron pretreatment, converter high-oxygen decarburization, LF power supply heating and large argon gas stirring, the problem of impurity influence has been solved, high-quality high-silicon pure iron production has been achieved, and production costs have been reduced.

CN118048577BActive Publication Date: 2026-11-17HUNAN VALIN XIANGTAN IRON & STEEL CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410207324.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-26
Publication Date
2026-11-17
Estimated Expiration
2044-02-26

AI Technical Summary

Technical Problem

In existing technologies, high-silicon pure iron products contain high levels of impurities such as carbon, manganese, oxygen, and nitrogen, which affect magnetic properties and production costs, making it difficult to meet the high-quality requirements of amorphous alloys.

Method used

By employing processes such as molten iron pretreatment, converter high-oxygen decarburization, LF power supply heating and large argon gas stirring, LF addition of high-purity ferrosilicon for deoxidation, and RH oxygen blowing alloying, the impurity content is controlled, and a high-silicon pure iron product with C≤0.003% and Si=1.7%~2.0% is developed.

Benefits of technology

It effectively reduces impurity content, improves product quality, meets the demand for high-silicon pure iron for amorphous alloys, and reduces production costs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention relates to a method for producing high-silicon pure iron. The chemical composition of the steel, by weight percentage, is: C≤0.003%, Si: 1.7-2.0%, Mn≤0.03%, Cr≤0.02%, P≤0.012%, S≤0.005%, Al≤0.004%, Ti≤0.003%, TO≤0.0040%, N≤0.0050%, with the balance being Fe and unavoidable impurities. The method employs a KR+BOF+LF+RH+continuous casting process, where KR removes sulfur, resulting in molten iron with S≤0.003% entering the furnace. The furnace endpoint [C] is ≤0.05%, the endpoint oxygen concentration is ≥500ppm, no deoxidizer is added during the tapping process, and 2~4kg / ton steel lime and refining synthetic slag are added; LF power supply heating and large argon gas stirring are used. After the top slag of the ladle is slagified, it is then removed to ensure that the slag is removed cleanly; after the slag is removed, high-purity ferrosilicon is added for deoxidation, lime and refining synthetic slag are added to make white slag for desulfurization and heating; RH vacuum is applied, oxygen is blown to remove C, and high-purity ferrosilicon is added. After the sample composition is qualified, the vacuum is broken, and high-purity ferrosilicon is sprinkled on the top slag for deoxidation. The soft blowing time is ≥10 minutes to obtain high-silicon pure iron for amorphous applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of metallurgical technology and relates to a method for producing high-silicon pure iron. Background Technology

[0002] Amorphous materials are hailed as "dual-green" new materials. Amorphous alloy transformers made from amorphous materials are known as "green power plants without generators." Compared with traditional silicon steel transformers, amorphous alloy transformers achieve approximately 60% to 80% energy savings under no-load conditions, and their operating energy consumption and costs are also significantly lower than those of silicon steel transformers. Currently, some products on the market use pure iron with high silicon content as the smelting raw material.

[0003] Amorphous alloys are high-performance soft magnetic materials with strong magnetic properties, superior soft magnetic properties compared to silicon steel sheets, and low price. They are ideal materials for high-frequency transformers, instrument transformers, and inductors, and are widely used in electronics, power, medical, aerospace, and rail transportation fields.

[0004] Due to its excellent soft magnetic properties, it can be used in various high-frequency power components, pressure / magnetic / temperature sensors, current transformers, dedicated integrated circuit chips, and electromagnetic shielding devices. Furthermore, its extremely low coercivity, high saturation magnetic induction, and low loss properties make it a valuable material for replacing silicon steel in transformer cores, significantly reducing core losses and saving energy. Simultaneously, iron-based amorphous materials also possess corrosion resistance and wear resistance, are inexpensive to manufacture, and offer advantages in surface treatment.

[0005] Chinese patent CN201810192622.7 discloses a raw material for high-silicon amorphous materials, pure iron, and its production method. The composition and mass percentage of this raw material are: C≤0.0050%, Si 0.6~1.0%, Mn≤0.06%, S≤0.006%, Al≤0.004%, Ti≤0.003%, O≤0.006%, N≤0.0060%, with the balance being Fe and unavoidable impurities. In this patent, the content of impurities such as carbon, manganese, oxygen, and nitrogen is extremely detrimental to magnetism, significantly affecting iron loss and magnetic properties. Summary of the Invention

[0006] The present invention aims to provide a method for producing high-silicon pure iron and to develop a high-silicon pure iron product that meets the needs of customers using high-silicon pure iron for amorphous alloys.

[0007] A method for producing high-silicon pure iron, wherein the chemical composition of the steel by weight percentage is C≤0.003%, Si=1.7%~2.0%, Mn≤0.03%, Cr≤0.02%, P≤0.012%, S≤0.005%, Al≤0.004%, Ti≤0.003%, TO≤0.0040%, N≤0.0050%, with the balance being Fe and unavoidable impurities; the key process steps include: (1) Hot metal pretreatment: Hot metal is pretreated with KR to remove sulfur, and slag is removed. The sulfur content of the hot metal entering the furnace is ≤0.003%. (2) Converter smelting: The final C of the converter is ≤0.05%, the final oxygen is ≥500ppm, and 2~4kg / ton of steel lime and refining slag are added during the tapping process; (3) LF demanganese removal: LF is powered and heated, and stirred with large argon gas. After the top slag of the steel ladle is slag-forming, it is then removed and cleaned. (4) LF smelting: After slag removal, add high-purity ferrosilicon for deoxidation, add lime and refined synthetic slag to make white slag for desulfurization and heating; (5) RH smelting: After RH is evacuated and oxygen is blown to remove carbon, high-purity ferrosilicon is added. After the sample composition is qualified, the evacuation is broken and high-purity ferrosilicon is sprinkled on the top slag for deoxidation. The soft blowing time is ≥10 minutes, and then it is poured on the platform.

[0008] The key features and significant effects of this invention are as follows: It employs slag removal during molten iron pretreatment to reduce the sulfur content from the slag; deoxidation is performed in the converter at a high oxygen level, without deoxidation during tapping, and slag is added; LF power supply heating and large-volume argon stirring result in slag formation from the ladle top slag, improving manganese removal efficiency; high-purity ferrosilicon is added to the LF for deoxidation, creating white slag and reducing sulfur through heating; after oxygen blowing in the RH furnace for deoxidation, alloying is performed, and high-purity ferrosilicon powder is sprinkled on the slag surface for further deoxidation. This results in a high-silicon pure iron product with a finished product C≤0.003% and Si=1.70%~2.00%, meeting the needs of customers using high-silicon pure iron for amorphous alloys. This invention fully utilizes the advantages of existing equipment, reducing production costs while ensuring product quality. Detailed Implementation

[0009] The present invention will be further described below with reference to the embodiments. Example 1

[0010] A method for producing high-silicon pure iron, wherein the steel's chemical composition by weight percentage is: C≤0.003%, Si: 1.7-2.0%, Mn≤0.03%, Cr≤0.02%, P≤0.012%, S≤0.005%, Al≤0.004%, Ti≤0.003%, TO≤0.0040%, N≤0.0050%, with the balance being Fe and unavoidable impurities; the process steps include: (1) Pretreatment of molten iron: molten iron is pretreated with KR to remove sulfur, ensuring that the slag is removed cleanly, and the sulfur content of the molten iron entering the furnace is 0.0015%; (2) Converter smelting: Converter endpoint C: 0.0434%, endpoint oxygen 576ppm, 210kg steel lime and 98kg refining slag are added during the tapping process; (3) LF demanganese removal: LF is powered on and heated, and stirred with large argon gas. After the top slag of the steel ladle is slag-forming, it is then removed to ensure that the slag is removed cleanly. (4) LF smelting: After slag removal, add 218 kg of high-purity ferrosilicon for deoxidation, add 205 kg of lime and 203 kg of refining and synthetic slag to make white slag for desulfurization and heating. (5) RH smelting: RH vacuuming, oxygen blowing 118Nm 3 After carbon removal, 1298 kg of high-purity ferrosilicon was added. Samples were taken for testing, and the composition was found to be: C: 0.0017%, Si: 1.8921%, Mn: 0.0242%, Cr: 0.0112%, P: 0.0065%, S: 0.0032%, Al: 0.0014%, Ti: 0.0018%, TO: 0.0036%, N: 0.0034%. The composition was found to be qualified. The cavity was broken, and 40 kg of high-purity ferrosilicon was sprinkled on the top slag for deoxidation. The soft blowing time was 12 minutes, and the slag was poured on the platform. Example 2

[0011] A method for producing high-silicon pure iron, wherein the steel's chemical composition by weight percentage is: C ≤ 0.003%, Si = 1.7%~2.0%, Mn ≤ 0.03%, Cr ≤ 0.02%, P ≤ 0.012%, S ≤ 0.005%, Al ≤ 0.004%, Ti ≤ 0.003%, TO ≤ 0.0040%, N ≤ 0.0050%, with the balance being Fe and unavoidable impurities. The process steps include: (1) Pretreatment of molten iron: molten iron is pretreated with KR to remove sulfur, ensuring that the slag is removed cleanly, and the sulfur content of the molten iron entering the furnace is 0.0021%; (2) Converter smelting: Converter endpoint C: 0.0348%, endpoint oxygen 617ppm, 202kg steel lime and 104kg refining slag are added during the tapping process; (3) LF demanganese removal: LF is powered on and heated, and stirred with large argon gas. After the top slag of the steel ladle is slag-forming, it is then removed to ensure that the slag is removed cleanly. (4) LF smelting: After slag removal, add 186 kg of high-purity ferrosilicon for deoxidation, add 199 kg of lime and 202 kg of refining and synthetic slag to make white slag for desulfurization and heating. (5) RH smelting: RH vacuum is applied, and oxygen is blown at 106 Nm. 3After carbon removal, 1322 kg of high-purity ferrosilicon was added. Samples were taken for testing and the composition was found to be C=0.0022%, Si=1.8745%, Mn=0.0212%, Cr=0.0129%, P=0.0042%, S=0.0035%, Al=0.0014%, Ti=0.002%, TO=0.0038%, and N=0.0032%. The composition was found to be qualified. The cavity was broken, and 40 kg of high-purity ferrosilicon was sprinkled on the top slag for deoxidation. The soft blowing time was 14 minutes, and the slag was poured on the platform.

[0012] Example 3

[0013] A method for producing high-silicon pure iron, wherein the steel's chemical composition by weight percentage is: C ≤ 0.003%, Si: 1.7-2.0%, Mn ≤ 0.03%, Cr ≤ 0.02%, P ≤ 0.012%, S ≤ 0.005%, Al ≤ 0.004%, Ti ≤ 0.003%, TO ≤ 0.0040%, N ≤ 0.0050%, with the balance being Fe and unavoidable impurities. The process steps include: (1) Pretreatment of molten iron: molten iron is pretreated with KR to remove sulfur, ensuring that the slag is removed cleanly, and the sulfur content of the molten iron entering the furnace is 0.0018%; (2) Converter smelting: The converter endpoint C=0.0376%, the endpoint oxygen is 684ppm, and 198kg steel lime and 106kg refining slag are added during the tapping process; (3) LF demanganese removal: LF is powered on and heated, and stirred with large argon gas. After the top slag of the steel ladle is slag-forming, it is then removed to ensure that the slag is removed cleanly. (4) LF smelting: After slag removal, add 228 kg of high-purity ferrosilicon for deoxidation, add 204 kg of lime and 198 kg of refining and synthetic slag to make white slag for desulfurization and heating. (5) RH smelting: RH vacuuming, oxygen blowing 97Nm 3 After carbon removal, 1308 kg of high-purity ferrosilicon was added. Samples were taken for testing and the composition was found to be C=0.0020%, Si=1.7894%, Mn=0.0281%, Cr=0.0173%, P=0.058%, S=0.0045%, Al=0.0015%, Ti=0.0014%, TO=0.0039%, and N=0.0032%. The composition was found to be qualified. The cavity was broken, and 40 kg of high-purity ferrosilicon was sprinkled on the top slag for deoxidation. The soft blowing time was 15 minutes, and the slag was poured on the platform.

Claims

1. A method for producing high-silicon pure iron, characterized in that: The chemical composition of the steel by weight percentage is C≤0.003%, Si=1.7%~2.0%, Mn≤0.03%, Cr≤0.02%, P≤0.012%, S≤0.005%, Al≤0.004%, Ti≤0.003%, TO≤0.0040%, N≤0.0050%, with the balance being Fe and unavoidable impurities; Key process steps include: (1) Hot metal pretreatment: Hot metal is pretreated with KR to remove sulfur, and slag is removed. The sulfur content of the hot metal entering the furnace is ≤0.003%. (2) Converter smelting: The final C of the converter is ≤0.05%, the final oxygen is ≥500ppm, and 2~4kg / ton of steel lime and refining slag are added during the tapping process; (3) LF demanganese removal: LF is powered and heated, and stirred with large argon gas. After the top slag of the steel ladle is slag-forming, it is then removed and cleaned. (4) LF smelting: After slag removal, add high-purity ferrosilicon for deoxidation, add lime and refined synthetic slag to make white slag for desulfurization and heating; (5) RH smelting: After RH is vacuumed and oxygen is blown to remove carbon, high-purity ferrosilicon is added. After the sample composition is qualified, the vacuum is broken and high-purity ferrosilicon is sprinkled on the top slag for deoxidation. The soft blowing time is ≥10 minutes, and then it is poured on the platform.

Citation Information

Patent Citations

  • High-silicon amorphous raw material pure iron and production method thereof

    CN108559905A

  • High-Si pure iron for energy-saving type transformer iron core and production method of high-Si pure iron

    CN107058867A

  • Non-aluminum deoxidation raw material pure iron for amorphous soft magnetic ribbon and preparation method of non-aluminum deoxidation raw material pure iron

    CN115261564A