A method for preparing ultraviolet light-cured epoxy acrylic resin coating
By using polyether modified acrylate-based diphenylsulfone active diluent and benzophenone in epoxy acrylic resin coatings, the heat resistance and flexibility of the coating are solved, and higher hardness is achieved. Toughness and impact resistance, suitable for applications where high performance is required.
Patent Information
- Application Number
- CN202410187226.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-20
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-02-20
AI Technical Summary
Epoxy acrylic resin coatings have poor heat resistance, flexibility and impact resistance, making them difficult to meet certain application needs.
采用聚醚改性丙烯酸酯基二苯砜作为活性稀释剂,通过与环氧丙烯酸树脂进行交联反应,结合二苯甲酮和复配光敏剂,形成紫外光固化涂料,提高涂层的硬度、韧性和耐热性。
It significantly improves the hardness, toughness and impact resistance of the coating, enhances the heat resistance of the cured coating, and has the advantages of rapid light curing and green environmental protection.
Smart Images

Figure BDA0004706400090000031 
Figure BDA0004706400090000041 
Figure BDA0004706400090000042
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ultraviolet light curing coatings, in particular to a method for preparing ultraviolet light curing epoxy acrylic resin coatings. Background Art
[0002] UV-curing coating is a green and environmentally friendly coating with the advantages of less volatile components, less pollution, excellent film-forming properties, and easy construction. Among them, epoxy acrylic resin UV-curing coating has good mechanical properties, high anti-corrosion properties, and excellent insulation properties. It has broad development prospects in the wood, food packaging, medical equipment, and automotive industries. However, epoxy acrylic resin has problems such as poor heat resistance, poor flexibility, and impact resistance.
[0003] Traditional UV-curable epoxy acrylic resin uses tripropylene glycol diacrylate, trimethylolpropane triacrylate and the like as active diluents; in recent years, developing new UV-curable active diluents and improving the comprehensive performance of epoxy acrylic resins have become research hotspots. The paper "Synthesis and Performance Characterization of a New UV-curable Active Diluent" reports the use of benzyl glycidyl ether and acrylic acid for ring-opening addition reaction to synthesize benzyl glycidyl ether acrylate with photocuring activity as a UV-curable active diluent, which greatly improves the mechanical properties of epoxy acrylic resins such as hardness and impact resistance. The present invention provides a polyether-modified acrylate-based diphenyl sulfone active diluent, which is intended to improve the heat resistance, flexibility, impact resistance and other properties of epoxy acrylic resin coatings. Summary of the invention
[0004] The invention provides an ultraviolet light-cured epoxy acrylic resin coating, which solves the problem that the epoxy acrylic resin coating has poor heat resistance, flexibility, impact resistance and the like.
[0005] The technical scheme provided by the invention is: an ultraviolet light-cured epoxy acrylic resin coating, comprising the following components in weight ratio: 52-70% epoxy acrylic resin, 1.2-3% benzophenone, 1.5-5% composite photosensitizer, and 28-40% polyether-modified acrylate-based diphenyl sulfone active diluent.
[0006] Furthermore, the composite photosensitizer is selected from any one of benzoin dimethyl ether, benzoin butyl ether or 2-hydroxy-2-methyl-1-phenylpropanone.
[0007] Furthermore, a method for preparing a UV-curable epoxy acrylic resin coating is provided: epoxy acrylic resin is added to a polyether-modified acrylate-based diphenyl sulfone active diluent, mixed evenly by high-speed shearing, and then benzophenone and a compounded photosensitizer are added to obtain a UV-curable epoxy acrylic resin coating; the coating is evenly coated on a tinplate sheet, and irradiated under a UV curing machine for 30-60 seconds to obtain a cured coating of the UV-curable epoxy acrylic resin coating.
[0008] Furthermore, the preparation method of the polyether-modified acrylate-based diphenyl sulfone active diluent is:
[0009] S1. Add 4,4-diaminodiphenyl sulfone, glycidyl methacrylate and inhibitor p-hydroxyanisole to 1,4-dioxane solvent, react at a temperature of 50-80°C for 12-24h, remove 1,4-dioxane by rotary evaporation after the reaction, separate by silica gel column chromatography, eluent is ethyl acetate and petroleum ether solution, volume ratio is 1:19, to obtain acrylate diphenyl sulfone intermediate.
[0010] S2. Add chlorinated polyethylene glycol monomethyl ether, acrylate-based diphenyl sulfone intermediate and N,N-diisopropylethylamine to toluene solvent, and react at a temperature of 40-65°C for 12-36 hours. After the reaction, remove toluene by rotary evaporation, dissolve the product in distilled water, then add petroleum ether and mix evenly, extract and separate, collect the aqueous phase, concentrate and dry, and obtain a polyether-modified acrylate-based diphenyl sulfone active diluent.
[0011] Furthermore, the molar ratio of 4,4-diaminodiphenyl sulfone, glycidyl methacrylate and p-hydroxyanisole in S1 is 100:420-500:0.04-0.07.
[0012] Furthermore, the molar ratio of chlorinated polyethylene glycol monomethyl ether, acrylate diphenyl sulfone intermediate and N,N-diisopropylethylamine in S2 is 450-600:100:420-480.
[0013] Furthermore, the preparation method of the chlorinated polyethylene glycol monomethyl ether in S2 is: adding polyethylene glycol monomethyl ether and succinic anhydride in a molar ratio of 1:3.2-4 to a toluene solvent, reflux at a temperature of 110-130°C for 4-10 hours, and after the reaction, removing toluene by rotary evaporation, washing with ether to obtain a carboxyl polyethylene glycol monomethyl ether intermediate; then adding it and thionyl chloride to toluene, reflux at a temperature of 70-85°C for 18-36 hours, and after the reaction, removing toluene and thionyl chloride by rotary evaporation, washing with ether to obtain the chlorinated polyethylene glycol monomethyl ether.
[0014] Furthermore, the molecular weight of polyethylene glycol monomethyl ether in S2 is between 200-400.
[0015] The technical effect of the present invention is as follows: 4,4-diaminodiphenyl sulfone and glycidyl methacrylate are subjected to addition reaction to obtain an acrylate diphenyl sulfone intermediate, which is then subjected to an esterification reaction with low molecular weight chlorinated polyethylene glycol monomethyl ether to prepare a novel polyether-modified acrylate diphenyl sulfone active diluent. Benzophenone and 2-hydroxy-2-methyl-1-phenylacetone are compounded to form a composite photoinitiator, which is mixed with epoxy acrylic resin to obtain an ultraviolet light-cured epoxy acrylic resin coating, which is then cured by ultraviolet light to obtain a cured coating, which has the advantages of fast light curing speed, no volatile organic solvents, and green environmental protection.
[0016] The multiple acrylate groups contained in the active diluent can undergo cross-linking and curing with the epoxy acrylic resin, which is beneficial to enhancing the cross-linking degree of the cured coating and making the coating have better hardness and strength; at the same time, the flexible polyether molecular chain with a branched structure contained in the active diluent can improve the toughness and impact resistance of the coating and play a good toughening effect; the diphenyl sulfone structure in the active diluent has excellent high temperature resistance, which increases the thermal decomposition temperature of the epoxy acrylic resin cured coating and enhances the heat resistance of the coating. DETAILED DESCRIPTION
[0017] In order to better understand the content of the present invention, the present invention will be further described below in conjunction with embodiments.
[0018] Example 1
[0019] (1) 0.5 mol of polyethylene glycol monomethyl ether MPEG200 and 1.6 mol of succinic anhydride are added to a toluene solvent, and the mixture is refluxed at 130°C for 6 h. After the reaction, the toluene is removed by rotary evaporation, and the mixture is washed with ether to obtain a carboxyl polyethylene glycol monomethyl ether intermediate. The intermediate and 5 mol of thionyl chloride are then added to toluene, and the mixture is refluxed at 80°C for 36 h. After the reaction, the toluene and thionyl chloride are removed by rotary evaporation, and the mixture is washed with ether to obtain an acyl chloride polyethylene glycol monomethyl ether. The reaction formula is as follows:
[0020]
[0021] (2) Add 0.2 mol of 4,4-diaminodiphenyl sulfone, 0.84 mol of glycidyl methacrylate and 0.08 mmol of inhibitor p-hydroxyanisole to 1,4-dioxane solvent, react at 80° C. for 18 h, remove 1,4-dioxane by rotary evaporation after the reaction, separate by silica gel column chromatography, eluent is ethyl acetate and petroleum ether solution, volume ratio is 1:19, to obtain acrylate diphenyl sulfone intermediate; the reaction formula is as follows:
[0022]
[0023] (3) Add 0.45 mol of chlorinated polyethylene glycol monomethyl ether, 0.1 mol of acrylated diphenyl sulfone intermediate and 0.42 mol of N,N-diisopropylethylamine to toluene solvent, react at 55° C. for 12 h, remove toluene by rotary evaporation after the reaction, dissolve the product in distilled water, then add petroleum ether and mix evenly, extract and separate, collect the aqueous phase, concentrate and dry, and obtain a viscous liquid, which is a polyether-modified acrylated diphenyl sulfone active diluent; the reaction formula is as follows:
[0024]
[0025] (4) Add two parts of type A epoxy acrylic resin with a weight ratio of 68.3% to 28% of a medium polyether-modified acrylate-based diphenyl sulfone active diluent, mix them evenly by high-speed shearing, and then add 2.2% of benzophenone and 1.5% of a composite photosensitizer 2-hydroxy-2-methyl-1-phenylpropanone to obtain a UV-curable epoxy acrylic resin coating; evenly apply the coating on a tinplate sheet, and irradiate it under a UV curing machine for 60 seconds to obtain a cured coating of the UV-curable epoxy acrylic resin coating.
[0026] Example 2
[0027] (1) 0.5 mol of polyethylene glycol monomethyl ether MPEG400 and 2 mol of succinic anhydride are added to a toluene solvent, and the mixture is refluxed at 130°C for 6 hours. After the reaction, the toluene is removed by rotary evaporation, and the mixture is washed with ether to obtain a carboxyl polyethylene glycol monomethyl ether intermediate; the intermediate and 10 mol of thionyl chloride are then added to toluene, and the mixture is refluxed at 70°C for 24 hours. After the reaction, the toluene and thionyl chloride are removed by rotary evaporation, and the mixture is washed with ether to obtain an acyl chloride polyethylene glycol monomethyl ether.
[0028] (2) 0.2 mol of 4,4-diaminodiphenyl sulfone, 1 mol of glycidyl methacrylate and 0.14 mmol of inhibitor p-hydroxyanisole were added to 1,4-dioxane solvent, and the mixture was reacted at 80° C. for 12 h. After the reaction, 1,4-dioxane was removed by rotary evaporation, and the mixture was separated by silica gel column chromatography using ethyl acetate and petroleum ether solution as eluents in a volume ratio of 1:19 to obtain an acrylate-based diphenyl sulfone intermediate.
[0029] (3) 0.6 mol of acyl chloride polyethylene glycol monomethyl ether, 0.1 mol of acrylated diphenyl sulfone intermediate and 0.48 mol of N,N-diisopropylethylamine were added to a toluene solvent, and the mixture was reacted at 65° C. for 12 h. After the reaction, toluene was removed by rotary evaporation, and the product was dissolved in distilled water. Petroleum ether was then added and mixed evenly, and the mixture was separated by extraction. The aqueous phase was collected, concentrated and dried to obtain a viscous liquid, which was a polyether-modified acrylated diphenyl sulfone active diluent.
[0030] (4) Add two parts of type A epoxy acrylic resin with a weight ratio of 62.5% to 30% of a medium polyether-modified acrylate-based diphenyl sulfone active diluent, mix them evenly by high-speed shearing, and then add 3% of benzophenone and 4.5% of a composite photosensitizer benzoin dimethyl ether to obtain a UV-curable epoxy acrylic resin coating; evenly apply the coating on a tinplate sheet, and irradiate it under a UV curing machine for 30 seconds to obtain a cured coating of the UV-curable epoxy acrylic resin coating.
[0031] Example 3
[0032] (1) 0.5 mol of polyethylene glycol monomethyl ether MPEG400 and 1.8 mol of succinic anhydride are added to a toluene solvent, and the mixture is refluxed at 120°C for 8 h. After the reaction, the toluene is removed by rotary evaporation, and the mixture is washed with ether to obtain a carboxyl polyethylene glycol monomethyl ether intermediate; the intermediate and 8 mol of thionyl chloride are then added to toluene, and the mixture is refluxed at 70°C for 36 h. After the reaction, the toluene and thionyl chloride are removed by rotary evaporation, and the mixture is washed with ether to obtain an acyl chloride polyethylene glycol monomethyl ether.
[0033] (2) 0.2 mol of 4,4-diaminodiphenyl sulfone, 0.9 mol of glycidyl methacrylate and 0.1 mmol of inhibitor p-hydroxyanisole were added to 1,4-dioxane solvent, and the mixture was reacted at 50° C. for 24 h. After the reaction, 1,4-dioxane was removed by rotary evaporation, and the mixture was separated by silica gel column chromatography using ethyl acetate and petroleum ether solution as eluents in a volume ratio of 1:19 to obtain an acrylate-based diphenyl sulfone intermediate.
[0034] (3) 0.48 mol of acyl chloride polyethylene glycol monomethyl ether, 0.1 mol of acrylated diphenyl sulfone intermediate and 0.45 mol of N,N-diisopropylethylamine were added to a toluene solvent, and the mixture was reacted at 65° C. for 18 h. After the reaction, toluene was removed by rotary evaporation, and the product was dissolved in distilled water. Petroleum ether was then added and mixed evenly, and the mixture was separated by extraction. The aqueous phase was collected, concentrated and dried to obtain a viscous liquid, which was a polyether-modified acrylated diphenyl sulfone active diluent.
[0035] (4) Add two parts of type A epoxy acrylic resin with a weight ratio of 60.8% to 33% of medium polyether modified acrylate-based diphenyl sulfone active diluent, mix them evenly by high-speed shearing, and then add 1.2% of benzophenone and 5% of compound photosensitizer benzoin butyl ether to obtain ultraviolet light-cured epoxy acrylic resin coating; evenly apply the coating on a tinplate sheet, and irradiate it under a ultraviolet light curing machine for 30 seconds to obtain a cured coating of the ultraviolet light-cured epoxy acrylic resin coating.
[0036] Example 4
[0037] (1) 0.5 mol of polyethylene glycol monomethyl ether MPEG200 and 2 mol of succinic anhydride are added to a toluene solvent, and the mixture is refluxed at 120°C for 10 hours. After the reaction, the toluene is removed by rotary evaporation, and the mixture is washed with ether to obtain a carboxyl polyethylene glycol monomethyl ether intermediate; the intermediate and 10 mol of thionyl chloride are then added to toluene, and the mixture is refluxed at 85°C for 24 hours. After the reaction, the toluene and thionyl chloride are removed by rotary evaporation, and the mixture is washed with ether to obtain an acyl chloride polyethylene glycol monomethyl ether.
[0038] (2) 0.2 mol of 4,4-diaminodiphenyl sulfone, 0.84 mol of glycidyl methacrylate and 0.08 mmol of inhibitor p-hydroxyanisole were added to 1,4-dioxane solvent, and the mixture was reacted at 60° C. for 12 h. After the reaction, 1,4-dioxane was removed by rotary evaporation, and the mixture was separated by silica gel column chromatography using ethyl acetate and petroleum ether solution as eluents in a volume ratio of 1:19 to obtain an acrylate-based diphenyl sulfone intermediate.
[0039] (3) 0.48 mol of acyl chloride polyethylene glycol monomethyl ether, 0.1 mol of acrylated diphenyl sulfone intermediate and 0.45 mol of N,N-diisopropylethylamine were added to a toluene solvent, and the mixture was reacted at 55° C. for 12 h. After the reaction, toluene was removed by rotary evaporation, and the product was dissolved in distilled water. Petroleum ether was then added and mixed evenly, and the mixture was separated by extraction. The aqueous phase was collected, concentrated and dried to obtain a viscous liquid, which was a polyether-modified acrylated diphenyl sulfone active diluent.
[0040] (4) Add two parts of type A epoxy acrylic resin with a weight ratio of 59.5% to 36% of a medium polyether-modified acrylate-based diphenyl sulfone active diluent, mix them evenly by high-speed shearing, and then add 3% of benzophenone and 1.5% of a composite photosensitizer benzoin dimethyl ether to obtain a UV-curable epoxy acrylic resin coating; evenly apply the coating on a tinplate sheet, and irradiate it under a UV curing machine for 60 seconds to obtain a cured coating of the UV-curable epoxy acrylic resin coating.
[0041] Example 5
[0042] (1) 0.5 mol of polyethylene glycol monomethyl ether MPEG200 and 2 mol of succinic anhydride are added to a toluene solvent, and the mixture is refluxed at 130°C for 4 h. After the reaction, the toluene is removed by rotary evaporation, and the mixture is washed with ether to obtain a carboxyl polyethylene glycol monomethyl ether intermediate; the intermediate and 5 mol of thionyl chloride are then added to toluene, and the mixture is refluxed at 80°C for 18 h. After the reaction, the toluene and thionyl chloride are removed by rotary evaporation, and the mixture is washed with ether to obtain an acyl chloride polyethylene glycol monomethyl ether.
[0043] (2) 0.2 mol of 4,4-diaminodiphenyl sulfone, 0.9 mol of glycidyl methacrylate and 0.14 mmol of inhibitor p-hydroxyanisole were added to 1,4-dioxane solvent, and the mixture was reacted at 80° C. for 12 h. After the reaction, 1,4-dioxane was removed by rotary evaporation, and the mixture was separated by silica gel column chromatography using ethyl acetate and petroleum ether solution as eluents in a volume ratio of 1:19 to obtain an acrylate-based diphenyl sulfone intermediate.
[0044] (3) 0.45 mol of acyl chloride polyethylene glycol monomethyl ether, 0.1 mol of acrylated diphenyl sulfone intermediate and 0.45 mol of N,N-diisopropylethylamine were added to a toluene solvent, and the mixture was reacted at 50° C. for 12 h. After the reaction, toluene was removed by rotary evaporation, and the product was dissolved in distilled water. Petroleum ether was then added and mixed evenly, and the mixture was separated by extraction. The aqueous phase was collected, concentrated and dried to obtain a viscous liquid, which was a polyether-modified acrylated diphenyl sulfone active diluent.
[0045] (4) Add two parts of type A epoxy acrylic resin with a weight ratio of 54% to 40% of a medium polyether-modified acrylate-based diphenyl sulfone active diluent, mix them evenly by high-speed shearing, and then add 2% of benzophenone and 4% of a composite photosensitizer 2-hydroxy-2-methyl-1-phenylpropanone to obtain a UV-curable epoxy acrylic resin coating; evenly apply the coating on a tinplate sheet, and irradiate it under a UV curing machine for 40 seconds to obtain a cured coating of the UV-curable epoxy acrylic resin coating.
[0046] Comparative Example 1
[0047] (1) 0.2 mol of 4,4-diaminodiphenyl sulfone, 1 mol of glycidyl methacrylate and 0.14 mmol of inhibitor p-hydroxyanisole were added to 1,4-dioxane solvent, and the mixture was reacted at 60° C. for 12 h. After the reaction, 1,4-dioxane was removed by rotary evaporation, and the mixture was separated by silica gel column chromatography with ethyl acetate and petroleum ether solution as the eluent in a volume ratio of 1:19 to obtain an acrylate-based diphenyl sulfone intermediate.
[0048] (2) Adding two parts of type A epoxy acrylic resin with a weight ratio of 66% to 28% of a medium acrylate diphenyl sulfone intermediate, high-speed shear mixing is performed, and then 2% of benzophenone and 4% of a composite photosensitizer 2-hydroxy-2-methyl-1-phenylpropanone are added to obtain a UV-curable epoxy acrylic resin coating; the coating is evenly coated on a tinplate sheet, and irradiated under a UV curing machine for 60 seconds to obtain a cured coating of the UV-curable epoxy acrylic resin coating.
[0049] The flexibility of the cured coating was tested according to GB / T 1731-2020.
[0050] The impact resistance of the cured coating was tested according to GB / T 1732-2020.
[0051] The adhesion of the cured coating was tested according to GB / T 9286-2021.
[0052] The hardness of the cured coating was tested according to GB / T 6739-2006.
[0053] Test the water resistance of the cured coating according to GB / T 1733-1993. Soak the cured coating in distilled water at room temperature for 6 hours, use filter paper to absorb the moisture on the coating surface, and observe the surface phenomenon of the coating.
[0054] The heat resistance of the cured coating was tested by a thermogravimetric analyzer, with a heating rate of 20°C / min, a test temperature of 20-700°C, and a nitrogen atmosphere. T5% is the temperature of 5% weight loss, and T50% is the temperature of 50% weight loss.
[0055]
[0056] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A UV-curable epoxy acrylic resin coating, characterized in that: The epoxy acrylic resin coating comprises the following components in weight ratio: 52-70% epoxy acrylic resin, 1.2-3% benzophenone, 1.5-5% composite photosensitizer, and 28-40% polyether modified acrylate diphenyl sulfone active diluent; The preparation method of the polyether-modified acrylate-based diphenyl sulfone active diluent is: S1. Add 4,4-diaminodiphenyl sulfone, glycidyl methacrylate and polymerization inhibitor p-hydroxyanisole to 1,4-dioxane solvent, and react at a temperature of 50-80° C. for 12-24 hours to obtain an acrylate diphenyl sulfone intermediate; S2. Add chlorinated polyethylene glycol monomethyl ether, acrylate-based diphenyl sulfone intermediate and N,N-diisopropylethylamine to toluene solvent, and react at a temperature of 40-65° C. for 12-36 hours to obtain a polyether-modified acrylate-based diphenyl sulfone active diluent.
2. The UV-curable epoxy acrylic resin coating according to claim 1, characterized in that: The composite photosensitizer is selected from any one of benzoin dimethyl ether, benzoin butyl ether or 2-hydroxy-2-methyl-1-phenylpropanone.
3. A method for preparing a UV-curable epoxy acrylic resin coating as claimed in claim 1 or 2, characterized in that: The preparation method comprises the following steps: adding epoxy acrylic resin to a polyether-modified acrylate-based diphenyl sulfone active diluent, uniformly mixing the mixture by high-speed shearing, and then adding benzophenone and a compounded photosensitizer to obtain an ultraviolet-cured epoxy acrylic resin coating; and irradiating the coating under an ultraviolet curing machine for 30-60 seconds to obtain a cured coating of the ultraviolet-cured epoxy acrylic resin coating.
4. The method for preparing the ultraviolet light-cured epoxy acrylic resin coating according to claim 3, characterized in that: The molar ratio of 4,4-diaminodiphenyl sulfone, glycidyl methacrylate and p-hydroxyanisole in S1 is 100:420-500:0.04-0.
07.
5. The method for preparing the UV-curable epoxy acrylic resin coating according to claim 3, characterized in that: The molar ratio of chlorinated polyethylene glycol monomethyl ether, acrylate diphenyl sulfone intermediate and N,N-diisopropylethylamine in S2 is 450-600:100:420-480.
6. The method for preparing the UV-curable epoxy acrylic resin coating according to claim 3, characterized in that: The preparation method of the chlorinated polyethylene glycol monomethyl ether in S2 is as follows: adding polyethylene glycol monomethyl ether and succinic anhydride in a molar ratio of 1:3.2-4 to a toluene solvent, and refluxing at a temperature of 110-130°C for 4-10 hours to obtain a carboxyl polyethylene glycol monomethyl ether intermediate; then adding it and thionyl chloride to toluene, and refluxing at a temperature of 70-85°C for 18-36 hours to obtain the chlorinated polyethylene glycol monomethyl ether.
7. The method for preparing the UV-curable epoxy acrylic resin coating according to claim 3, characterized in that: The molecular weight of polyethylene glycol monomethyl ether in S2 is between 200-400.
Citation Information
Patent Citations
Modified ultraviolet curing acrylic resin paint and preparation method thereof
CN115340810A
Yellowing-resistant ultraviolet curing coating and preparation method thereof
CN115572521A
Resin composite, composition, and their production methods
JP2001329027A
Ultraviolet light curable coating compositions
US4067791A