High-rate stable non-aqueous electrolyte and lithium battery comprising same

By using a high-rate stable non-aqueous electrolyte composed of lithium salt, room-temperature ionic liquid electrolyte and composite additives in lithium batteries, the problem that traditional electrolyte solutions cannot meet the high ion migration number and electrochemical stability is solved, and the lithium battery is realized High power density and long life, broaden the operating temperature range and improve safety.

CN119029313APending Publication Date: 2024-11-26JIANGSU OLITER ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411437307.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-15
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Traditional lithium battery electrolyte solutions cannot meet the requirements of high ion migration number, high conductivity, wide electrochemical window, high thermal stability and low interface transfer resistance, affecting the service life and storage performance of lithium batteries.

Method used

Using a high-rate stable non-aqueous electrolyte composed of lithium salt, room temperature ionic liquid electrolyte and composite additives, including quaternary ammonium cationic liquid, co-solvent, vinyl vinyl sulfite, fluoroalkyl boronide, triisopropylene phosphate The ylphenyl ester, cyclohexylbenzene and nano-lithium carbonate can broaden the battery operating temperature range and improve safety by improving the migration rate of lithium ions at the interface between the electrolyte and the electrode.

Benefits of technology

It significantly improves the power density and service life of lithium batteries, broadens the working temperature range, enhances the safety of the battery at high power, reduces safety risks, and improves the compatibility of the electrolyte with the negative electrode.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses a high-rate stable non-aqueous electrolyte and a lithium battery containing the same. The high-rate stable non-aqueous electrolyte is prepared from a lithium salt, room-temperature ionic liquid electrolyte and a composite additive, wherein the room-temperature ionic liquid electrolyte is prepared from quaternary ammonium salt cationic liquid and a cosolvent in a mass ratio of 1: (0.1-0.5). Compared with the prior art, the ionic liquid is adopted to replace a traditional organic solvent, the working temperature range of the battery is widened, the stability to metal lithium is good, and the safety of the battery under high power density can be improved; various functional additives are compounded, so that the structure of a lithium ion battery negative electrode SEI membrane is improved, the overall stability of the battery is improved, the compatibility degree of an electrolyte and a negative electrode is improved, the cycle of the battery is improved, and the service life is prolonged; the nano lithium carbonate effectively improves various performances of the battery and improves the capacity of the battery. According to the invention, the contribution rate of lithium ions to the conductivity and the migration rate of the lithium ions in the electrolyte and the SEI film are improved, the conductivity of the electrolyte reaches 9.8-11.5 mS / cm, and the power of the lithium battery is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium batteries, and in particular to a high-rate stable non-aqueous electrolyte and a lithium battery containing the same. Background Art

[0002] Since the concept of rechargeable lithium batteries was proposed in the early 1970s, and lithium-ion batteries have been born and commercialized, they have quickly become a research hotspot in multiple disciplines such as advanced energy, materials, and electrochemistry due to their superior performance, and are widely used in small electronic devices such as laptops, mobile phones, digital cameras, mp3 players, and medical devices as driving power sources. Non-aqueous electrolytes are one of the key materials for lithium batteries, and their comprehensive properties (such as chemical and electrochemical stability, high and low temperature performance, etc.) directly affect the use of secondary lithium batteries. The non-aqueous electrolyte solutions used in rechargeable lithium (ion) batteries should generally meet the following requirements: (1) high ionic conductivity, generally reaching 10-3S / cm; (2) high lithium ion migration number to obtain high lithium ion conductivity; (3) wide electrochemical window, that is, the reversible insertion and extraction of lithium ions in the positive and negative electrodes without chemical or electrochemical decomposition of the electrolyte; (4) high thermal stability, no chemical or electrochemical decomposition within a wide operating temperature range; (5) high chemical stability, that is, no chemical reaction with the electrode materials of the battery system such as the positive electrode, negative electrode, current collector, binder, conductive agent and separator; (6) low interface transfer resistance; (7) good compatibility with the currently used positive and negative electrode materials; (8) non-toxic, non-polluting, safe to use, and preferably biodegradable; (9) easy to prepare and low cost.

[0003] However, conventional lithium battery electrolyte solutions may not meet the above requirements. Therefore, a non-aqueous electrolyte for lithium batteries is needed that can improve the service life and storage performance of lithium batteries while maintaining their good performance. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a high-rate stable non-aqueous electrolyte and a lithium battery containing the same, so as to effectively improve the migration rate of lithium ions at the interface between the electrolyte and the electrode, thereby improving the battery rate charge and discharge performance, widening the operating temperature range of the battery, and improving the safety of the battery at high power density.

[0005] The technical solution adopted by the present invention is as follows: a high-rate stable non-aqueous electrolyte, which is mainly composed of the following raw materials in parts by weight: 11-19 parts of lithium salt, 55-75 parts of room temperature ionic liquid electrolyte, and 6-21 parts of composite additives; The room temperature ionic liquid electrolyte is composed of a quaternary ammonium salt cation liquid and a co-solvent in a mass ratio of 1:(0.1-0.5); The composite additive is composed of the following raw materials in mass fraction: Vinyl vinyl sulfite 7-35%, fluoroalkyl boride 5-28%, triisopropylphenyl phosphate 11-20%, cyclohexylbenzene 8-26%, nano lithium carbonate 1-14%.

[0006] Preferably, the mass parts of the raw materials are: 13 parts of lithium salt, 63 parts of room temperature ionic liquid electrolyte, and 15 parts of composite additives; the room temperature ionic liquid electrolyte is composed of a quaternary ammonium salt cation liquid and a solvent in a mass ratio of 1:0.2.

[0007] Preferably, the composite additive comprises: 32% vinyl sulfite, 24% fluoroalkyl boride, 15% triisopropylphenyl phosphate, 18% cyclohexylbenzene, and 11% nano lithium carbonate.

[0008] Preferably, the cation of the quaternary ammonium salt cationic liquid is [(CH 3 ) 3 NC 6 H 13 ] + , the anion is [N(CF 3 SO 2 ) 2 ] - , [BF 4 ] - , [CF 3 SO 2 ] - ,[C(CF 3 SO 2 ) 3 ] - One or more of the following.

[0009] Preferably, the components of the co-solvent and their corresponding percentages are: ethylene carbonate 10-30%, ethyl methyl carbonate 20-45%, 4-trifluoromethylethylene carbonate 8-25%, and ethyl difluoroacetate 12-20%.

[0010] Preferably, the nano lithium carbonate is prepared by the following method: adding a dispersant to a lithium hydroxide aqueous solution with a molar concentration of 0.5-4 mol / L, the mass ratio of the dispersant to lithium ions is (0.9-1.7):100, stirring evenly at room temperature to obtain a lithium ion precursor, and then introducing carbon dioxide gas into the lithium ion precursor for contact reaction, the molar ratio of carbonate ions to lithium ions in the reaction system is (0.8-1.5):1, the contact temperature is 55-85°C, the contact time is 18-30h, and the pH is controlled to be 8.9-9.1. After the contact reaction is completed, the reaction product is allowed to stand at room temperature for 5-12h, and then the precipitate is separated by filtration, and the precipitate is washed with pure water, dried and ground to obtain nano lithium carbonate.

[0011] Preferably, the dispersant is one or a mixture of two or more of ethyl acetoacetate, p-toluenesulfonate, triethylamine, and tribromoaniline.

[0012] Preferably, the lithium salt is LiPF 6 、LiAsF 6 、LiSO 3 CF 3 , LiBF 4 Any one or a mixture of two or more.

[0013] Preferably, the fluoroalkyl boride is (C 6 H 3 F)O 2 B(C 6 H 3 F 2 )、(C 6 F 4 ) 2 B(C 6 F 5 ) or a mixture of two or more thereof.

[0014] A lithium battery comprises an anode, a cathode and a current collector, the key point being that the lithium battery also comprises the high-rate stable non-aqueous electrolyte described in any one of the above items.

[0015] Beneficial effects: Compared with the prior art, the present invention provides a high-rate stable non-aqueous electrolyte and a lithium battery containing the same. It uses ionic liquids to replace traditional organic solvents, and has the advantages of non-volatility, non-flammability, good conductivity, and wide chemical window. It can not only broaden the operating temperature range of the battery, but also has good stability to metallic lithium, and can also improve the safety of the battery at high power density, eliminating the potential safety hazards of the battery; through compounding with various functional additives, the structure of the solid phase interface film (SEI film) of the negative electrode of the lithium ion battery is improved, the overall stability of the battery is improved, the overall life of the battery is improved, the compatibility of the electrolyte and the negative electrode is improved, and the battery cycle is improved to increase the service life; the particle size of nano lithium carbonate is less than 80nm, the purity is high, the distribution is uniform, and the crystal form is good, which can effectively improve the various performances of the battery and increase the battery capacity. The present invention improves the contribution rate of lithium ions to conductivity and the migration rate of lithium ions in the electrolyte and SEI film. The conductivity of the electrolyte reaches 9.8-11.5mS / cm, which greatly improves the power of the lithium battery. DETAILED DESCRIPTION

[0016] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is described in detail below in conjunction with specific implementation methods.

[0017] Example 1 Preparation of high-rate stable non-aqueous electrolyte I At room temperature and pressure, with a water content of 1 ppm and an inert gas environment, LiSO 3 CF 3 11 parts, 55 parts of room temperature ionic liquid electrolyte (wherein [(CH 3 ) 3 NC 6 H 13 ] N(CF 3 SO 2 ) 2 50 parts of ionic liquid, 1 part of ethylene carbonate, 1.75 parts of ethyl methyl carbonate, 1.25 parts of 4-trifluoromethylethylene carbonate, 1 part of ethyl difluoroacetate), 6 parts of composite additives (including 1.92 parts of vinyl sulfite, (C 6 H 3 F)O 2 B(C 6 H 3 F 2 ) 1.8 parts, triisopropylphenyl phosphate 0.9 parts, cyclohexylbenzene 1.2 parts, nano lithium carbonate 0.48 parts), add to a conical flask with a ground mouth, mix well, and stir until LiSO 3 CF 3Completely dissolved to obtain a high-rate stable non-aqueous electrolyte I. The nano lithium carbonate is prepared by the following method: ethyl acetoacetate is added to a lithium hydroxide aqueous solution with a molar concentration of 0.5 mol / L, the mass ratio of ethyl acetoacetate to lithium ions is 0.9:100, and the lithium ion precursor is obtained by stirring at room temperature, and then carbon dioxide gas is introduced into the lithium ion precursor for contact reaction, the molar ratio of carbonate ions to lithium ions in the reaction system is 0.8:1, the contact temperature is 55-85°C, the contact time is 18-30h, and the pH is controlled to be 8.9-9.1. After the contact reaction is completed, the reaction product is allowed to stand at room temperature for 5-12h, and then the precipitate is separated by filtration, and the precipitate is washed with pure water, dried and ground to obtain nano lithium carbonate.

[0018] Example 2 Preparation of high rate stable non-aqueous electrolyte II At room temperature and pressure, with a moisture content of 1 ppm and an inert gas, LiAsF 6 19 parts, 75 parts of room temperature ionic liquid electrolyte (wherein [(CH 3 ) 3 NC 6 H 13 ] CF 3 SO 2 50 parts of ionic liquid, 7.5 parts of ethylene carbonate, 11.25 parts of ethyl methyl carbonate, 3.75 parts of 4-trifluoromethylethylene carbonate, 2.5 parts of ethyl difluoroacetate), 21 parts of composite additives (including 6.3 parts of vinyl sulfite, (C 6 F 4 ) 2 B(C 6 F 5 ) 4.62 parts, triisopropylphenyl phosphate 3.36 parts, cyclohexylbenzene 4.2 parts, nano lithium carbonate 2.25 parts), add to a conical flask with a ground mouth, mix well, and stir until LiAsF 6 The nano lithium carbonate is prepared by the following method: ethyl acetoacetate is added to a lithium hydroxide aqueous solution with a molar concentration of 4 mol / L, wherein the mass ratio of ethyl acetoacetate to lithium ions is 1.7:100, and the mixture is stirred evenly at room temperature to obtain a lithium ion precursor, and then carbon dioxide gas is introduced into the lithium ion precursor for contact reaction, wherein the molar ratio of carbonate ions to lithium ions in the reaction system is 1.5:1, the contact temperature is 55-85°C, the contact time is 18-30h, and the pH is controlled to be 8.9-9.1. After the contact reaction is completed, the reaction product is allowed to stand at room temperature for 5-12h, and then the precipitate is separated by filtration, and the precipitate is washed with pure water, dried and ground to obtain nano lithium carbonate.

[0019] Example 3 Preparation of high rate stable non-aqueous electrolyte III At room temperature and pressure, with a water content of 1 ppm and an inert gas, LiPF 6 19 parts, 60 parts of room temperature ionic liquid electrolyte (wherein [(CH 3 ) 3 NC 6 H 13 ] C(CF 3 SO 2 ) 3 50 parts of ionic liquid, 2.5 parts of ethylene carbonate, 4 parts of ethyl methyl carbonate, 2 parts of 4-trifluoromethylethylene carbonate, 1.5 parts of ethyl difluoroacetate), 15 parts of composite additives (including 4.8 parts of vinyl sulfite, (C 6 H 3 F)O 2 B(C 6 H 3 F 2 ) 3.6 parts, triisopropylphenyl phosphate 2.25 parts, cyclohexylbenzene 2.7 parts, nano lithium carbonate 1.65 parts), add to a conical flask with a ground mouth, mix well, and stir until LiPF 6 The nano lithium carbonate is prepared by the following method: ethyl acetoacetate is added to a lithium hydroxide aqueous solution with a molar concentration of 2 mol / L, wherein the mass ratio of ethyl acetoacetate to lithium ions is 1.3:100, and the mixture is stirred evenly at room temperature to obtain a lithium ion precursor, and then carbon dioxide gas is introduced into the lithium ion precursor for contact reaction, wherein the molar ratio of carbonate ions to lithium ions in the reaction system is 1.1:1, the contact temperature is 55-85°C, the contact time is 18-30h, and the pH is controlled to be 8.9-9.1. After the contact reaction is completed, the reaction product is allowed to stand at room temperature for 5-12h, and then the precipitate is separated by filtration, and the precipitate is washed with pure water, dried and ground to obtain nano lithium carbonate.

[0020] Example 4 Comparative Example The equipment and operation are the same as those in Example 3, except that the room temperature ionic liquid electrolyte is replaced by PC solvent to obtain non-aqueous electrolyte IV.

[0021] Example 5 Comparative Example The equipment and operation are the same as those in Example 3, except that the amount of nano lithium carbonate is changed to 0, to obtain non-aqueous electrolyte V.

[0022] Performance Test: The non-aqueous electrolyte prepared in each embodiment was tested as follows: Moisture, conductivity and acidity testing of non-aqueous electrolytes: The water content in the electrolyte was determined by the Coulometric Karl Fischer method, the acidity in the electrolyte was tested by acid-base titration, and the conductivity of the electrolyte was tested by a DJS-307 conductivity meter. The results are shown in Table 1.

[0023] Table 1 Comparison of test results of various non-aqueous electrolyte IV Rate discharge characteristics test of lithium battery:

[0024] The non-aqueous electrolytes were filled into 063048 batteries with a designed capacity of 850 mAh to prepare lithium batteries IV for discharge characteristic testing. The test results are shown in Table 2.

[0025] Rate discharge characteristic detection method, namely: 1. Charge to 4.2V at 1C constant voltage, with a cut-off current of 20mA; 2. Let it stand for 10 minutes and use a secondary battery performance test cabinet to test the battery capacity; 3. Discharge to 3.0V at 5C current; 4. Let it stand for 10 minutes and use a secondary battery performance test cabinet to test the battery capacity; 5. Discharge to 3.0V at 10C current; 6. Let it stand for 10 minutes and use a secondary battery performance test cabinet to test the battery capacity.

[0026] Battery cycle discharge test method: Cycle battery rate discharge characteristic test method steps 1 to 6.

[0027] Table 2 Comparison of test results of various batteries

[0028] The wastewater electrolyte prepared by the present invention is used in 063048 lithium batteries, replacing traditional solvents, broadening the battery operating temperature range and electrolyte conductivity, and the conductivity reaches 9.8-11.5mS / cm, thereby greatly improving the power of the lithium battery and performing excellently in multiple charge and discharge performance. By adopting composite additives and nano-scale lithium carbonate, various charge and discharge performances of the battery are improved. The introduction of vinyl sulfite in the present invention broadens the electrochemical properties of the electrolyte, especially the interface stability and high-voltage cycle electrical stability in the high voltage range, and the introduction of fluoroalkyl boride additives improves the electrolyte conductivity and reduces the internal resistance, and improves the migration rate of lithium ions in the electrolyte and SEI film; cyclohexylbenzene has a high boiling point and high stability, and can play an overcharge protection role when the lithium battery is overcharged at high voltage.

[0029] Finally, it should be noted that the above description is only a preferred embodiment of the present invention. Under the guidance of the present invention, those skilled in the art can make a variety of similar expressions without violating the purpose and claims of the present invention, and such changes all fall within the protection scope of the present invention.

Claims

1. A high rate stable non-aqueous electrolyte, characterized in that The method is composed of the following raw materials in parts by weight: 11-19 parts of lithium salt, 55-75 parts of room temperature ionic liquid electrolyte, and 6-21 parts of composite additives; The room temperature ionic liquid electrolyte is composed of a quaternary ammonium salt cation liquid and a co-solvent in a mass ratio of 1:(0.1-0.5); The composite additive is composed of the following raw materials in mass fraction: Vinyl vinyl sulfite 7-35%, fluoroalkyl boride 5-28%, triisopropylphenyl phosphate 11-20%, cyclohexylbenzene 8-26%, nano lithium carbonate 1-14%.

2. The high-rate stable non-aqueous electrolyte according to claim 1, characterized in that: The mass proportions of the raw materials are: 13 parts of lithium salt, 60 parts of room temperature ionic liquid electrolyte, and 15 parts of composite additives; the room temperature ionic liquid electrolyte is composed of a quaternary ammonium salt cation liquid and a solvent in a mass ratio of 1:0.

2.

3. The high-rate stable non-aqueous electrolyte according to claim 1 or 2, characterized in that The composite additive comprises: 32% of vinyl sulfite, 24% of fluoroalkyl boride, 15% of triisopropylphenyl phosphate, 18% of cyclohexylbenzene, and 11% of nano lithium carbonate.

4. The high-rate stable non-aqueous electrolyte according to claim 3, characterized in that: The cation of the quaternary ammonium salt cationic liquid is [(CH3)3NC6H 13 ] + , the anion is [N(CF3SO2)2] - , [BF4] - , [CF3SO2] - 、[C(CF3SO2)3] - One or more of the following.

5. The high-rate stable non-aqueous electrolyte according to claim 1 or 4, characterized in that: The components of the co-solvent and their corresponding percentage contents are: 10-30% ethylene carbonate, 20-45% ethyl methyl carbonate, 8-25% 4-trifluoromethylethylene carbonate, and 12-20% ethyl difluoroacetate.

6. The high-rate stable non-aqueous electrolyte according to claim 5, characterized in that The nano lithium carbonate is prepared by the following method: adding a dispersant to a lithium hydroxide aqueous solution with a molar concentration of 0.5-4 mol / L, wherein the mass ratio of the dispersant to lithium ions is (0.9-1.7):100, stirring evenly at room temperature to obtain a lithium ion precursor, and then introducing carbon dioxide gas into the lithium ion precursor for contact reaction, wherein the molar ratio of carbonate ions to lithium ions in the reaction system is (0.8-1.5):1, the contact temperature is 55-85°C, the contact time is 18-30h, and the pH is controlled to be 8.9-9.

1. After the contact reaction is completed, the reaction product is allowed to stand at room temperature for 5-12h, and then the precipitate is separated by filtration, and the precipitate is washed with pure water, dried and ground to obtain the nano lithium carbonate.

7. The high-rate stable non-aqueous electrolyte according to claim 6, characterized in that: The dispersant is one or a mixture of two or more of ethyl acetoacetate, p-toluenesulfonate, triethylamine and tribromoaniline.

8. The high-rate stable non-aqueous electrolyte according to any one of claims 1, 4 or 7, characterized in that: The lithium salt is any one of LiPF6, LiAsF6, LiSO3CF3, LiBF4 or a mixture of two or more thereof.

9. The high-rate stable non-aqueous electrolyte according to claim 8, characterized in that: The fluoroalkyl boride is any one of (C6H3F)O2B(C6H3F2), (C6F4)O2B(C6F5), or a mixture of two or more thereof.

10. A lithium battery comprising an anode, a cathode and a current collector, characterized in that: The lithium battery further comprises the high-rate stable non-aqueous electrolyte according to any one of claims 1 to 9.